{"id":101308,"date":"2017-10-13T06:30:16","date_gmt":"2017-10-12T22:30:16","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=101308"},"modified":"2017-09-30T22:19:00","modified_gmt":"2017-09-30T14:19:00","slug":"%e9%81%93%e8%b7%af%e3%80%81%e5%b8%82%e6%94%bf%e3%80%81%e6%a1%a5%e6%a2%81%e3%80%81%e6%a0%b8%e7%94%b5%e7%ad%89%e8%af%b8%e5%a4%9a%e9%87%8d%e8%a6%81%e9%a2%86%e5%9f%9f%e5%bb%ba%e7%ad%91%e7%94%a8%e6%9d%90","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=101308","title":{"rendered":"\u9053\u8def\u3001\u5e02\u653f\u3001\u6865\u6881\u3001\u6838\u7535\u7b49\u8bf8\u591a\u91cd\u8981\u9886\u57df\u5efa\u7b51\u7528\u6750\uff1a\u6d3b\u6027\u7c89\u672b\u6df7\u51dd\u571f\uff08RPC\uff09"},"content":{"rendered":"<p><strong>\u6df7\u51dd\u571f\u662f\u5f53\u4eca\u571f\u6728\u5efa\u7b51\u5de5\u7a0b\u5e7f\u6cdb\u4f7f\u7528\u7684\u5efa\u7b51\u6750\u6599\uff0c\u968f\u7740\u79d1\u5b66\u6280\u672f\u7684\u8fdb\u6b65\u548c\u57ce\u5e02\u5316\u89c4\u6a21\u7684\u4e0d\u65ad\u6269\u5927\uff0c\u73b0\u4ee3\u5efa\u7b51\u65e5\u76ca\u5411\u9ad8\u5c42\u3001\u5927\u8de8\u548c\u5730\u4e0b\u53d1\u5c55\uff0c\u5bf9\u5efa\u7b51\u7ed3\u6784\u7684\u5b89\u5168\u6027\u3001\u9002\u7528\u6027\u548c\u8010\u4e45\u6027\u63d0\u51fa\u8d8a\u6765\u8d8a\u9ad8\u7684\u8981\u6c42\uff0c\u9ad8\u5f3a\u3001\u9ad8\u6027\u80fd\u6df7\u51dd\u571f\u7684\u51fa\u73b0\u548c\u53d1\u5c55\u9002\u5e94\u4e86\u8fd9\u4e00\u8981\u6c42\u3002\u9ad8\u5f3a\u548c\u9ad8\u6027\u80fd\u6df7\u51dd\u571f\u7531\u4e8e\u5177\u6709\u5f3a\u5ea6\u9ad8\u3001\u627f\u8f7d\u529b\u5927\u3001\u8d44\u6e90\u548c\u80fd\u6e90\u6d88\u8017\u5c11\u3001\u8010\u4e45\u6027\u597d\u7b49\u4f18\u70b9\uff0c\u6ee1\u8db3\u4e86\u571f\u6728\u5efa\u7b51\u5de5\u7a0b\u8f7b\u8d28\u3001\u9ad8\u5c42\u3001\u5927\u8de8\u3001\u91cd\u8f7d\u5316\u53ca\u8010\u4e45\u6027\u7b49\u65b9\u9762\u7684\u8981\u6c42\uff0c\u4ece\u800c\u5f97\u5230\u8fc5\u901f\u63a8\u5e7f\u548c\u5e94\u7528\u3002<\/strong><\/p>\n<p><strong>\u6d3b\u6027\u7c89\u672b\u6df7\u51dd\u571f\uff08reactive powder concrete\uff0cRPC\uff09<\/strong>\u662f\u6cd5\u56fdBOUYGUES\u516c\u53f8\u4e8e20\u4e16\u7eaa90\u5e74\u4ee3\u7387\u5148\u7814\u53d1\u7684\u65b0\u4e00\u4ee3\u9ad8\u5f3a\u548c\u9ad8\u6027\u80fd\u6df7\u51dd\u571f\uff0c\u5177\u6709\u8d85\u9ad8\u5f3a\u5ea6\u3001\u9ad8\u97e7\u6027\u548c\u826f\u597d\u7684\u8010\u4e45\u6027\u7b49\uff0c1994\u5e74\u5728Richard\u7b49\u53d1\u8868\u7684\u8bba\u6587\u4e2d\u516c\u5f00\u63d0\u51fa\u3002RPC\u4e3b\u8981\u7531\u6c34\u6ce5\u3001\u77f3\u82f1\u7802\u3001\u77f3\u82f1\u7c89\u3001\u7845\u7070\u3001\u8d85\u5851\u5316\u5242\u548c\u94a2\u7ea4\u7ef4\u7ec4\u6210\uff0c\u5728\u4e00\u5b9a\u5236\u5907\u5de5\u827a\u4e0b\u5176\u6297\u538b\u5f3a\u5ea6\u53ef\u8fbe200~800Mpa\uff08\u6309\u5f3a\u5ea6\u5206\u4e3aRPC200\u548cRPC800\u4e24\u7ea7\uff09\uff0c\u6297\u6298\u5f3a\u5ea6\u4e3a20~40MPa\uff0c\u65ad\u88c2\u80fd\u8fbe4\u00d710<sup>4<\/sup>J\/m<sup>2<\/sup>\u3002\u4f5c\u4e3a\u4e00\u79cd\u65b0\u578b\u7684\u9ad8\u6027\u80fd\u6df7\u51dd\u571f\uff0cRPC\u81ea\u95ee\u4e16\u4ee5\u6765\u4fbf\u53d7\u5230\u4e86\u56fd\u5185\u5916\u5b66\u8005\u7684\u5e7f\u6cdb\u91cd\u89c6\u4e0e\u5173\u6ce8\uff0c\u5e76\u5728\u9053\u8def\u3001\u5e02\u653f\u3001\u6865\u6881\u3001\u6838\u7535\u548c\u519b\u4e8b\u5de5\u7a0b\u7b49\u8bf8\u591a\u9886\u57df\u5f97\u5230\u4e86\u53d1\u5c55\u548c\u5e94\u7528\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101309 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/1-58.jpg\" alt=\"\" width=\"500\" height=\"326\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/1-58.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/1-58-300x196.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p>\u6df7\u51dd\u571f\u662f\u5f53\u4ee3\u5e7f\u6cdb\u4f7f\u7528\u7684\u5efa\u7b51\u6750\u6599\uff0c\u4e5f\u662f\u73b0\u4ee3\u6700\u5927\u5b97\u7684\u4eba\u9020\u6750\u6599\uff0c\u5df2\u6210\u4e3a\u571f\u6728\u5de5\u7a0b\u7528\u6750\u7684\u4e3b\u4f53\u3002\u636e\u4e0d\u5b8c\u5168\u7edf\u8ba1\uff0c2012\u5e74\u4e16\u754c\u6c34\u6ce5\u4ea7\u91cf\u5df2\u8d85\u8fc738.2\u4ebft\uff0c\u6298\u5408\u6210\u6df7\u51dd\u571f\u5219\u5927\u4e8e150\u4ebfm<sup>3<\/sup>\uff0c\u6211\u56fd\u7684\u6c34\u6ce5\u4ea7\u91cf\u8fbe21.84\u4ebft\uff0c\u5546\u54c1\u6df7\u51dd\u571f\u4ea7\u91cf8.88\u4ebfm<sup>3<\/sup>\uff0c\u7ea6\u4e3a\u4e16\u754c\u603b\u4ea7\u91cf\u76841\/2\uff0c\u5c45\u4e16\u754c\u9996\u4f4d\u3002<\/p>\n<p>\u4e0e\u5176\u4ed6\u5efa\u7b51\u6750\u6599\u76f8\u6bd4\uff0c\u6df7\u51dd\u571f\u5177\u6709\u6297\u538b\u5f3a\u5ea6\u9ad8\u3001\u5f39\u6027\u6a21\u91cf\u5927\u3001\u8010\u4e45\u6027\u597d\u7b49\u7279\u70b9\uff0c\u540c\u65f6\uff0c\u751f\u4ea7\u539f\u6599\u5e7f\u6cdb\u3001\u6210\u672c\u4f4e\u3001\u751f\u4ea7\u5de5\u827a\u7b80\u4fbf\u4f7f\u5b83\u5728\u571f\u6728\u5de5\u7a0b\u9886\u57df\u5f97\u5230\u4e86\u5e7f\u6cdb\u5e94\u7528\u3002\u7136\u800c\uff0c\u4e00\u822c\u7684\u6df7\u51dd\u571f\u6750\u6599\u5b58\u5728\u53d8\u5f62\u6027\u80fd\u8f83\u5dee\u3001\u8106\u6027\u5927\u3001\u81ea\u91cd\u5927\u3001\u6297\u62c9\u5f3a\u5ea6\u4f4e\u7b49\u7f3a\u70b9\uff0c\u5728\u4e00\u5b9a\u8303\u56f4\u5185\u53c8\u9650\u5236\u4e86\u5b83\u7684\u4f7f\u7528\u3002\u56e0\u6b64\uff0c\u6539\u5584\u6df7\u51dd\u571f\u6750\u6599\u7684\u6027\u80fd\u4fbf\u6210\u4e3a\u5b66\u672f\u754c\u548c\u5de5\u7a0b\u754c\u575a\u6301\u4e0d\u61c8\u7684\u7814\u7a76\u8bfe\u9898\uff0c\u4eba\u4eec\u671f\u671b\u6df7\u51dd\u571f\u6750\u6599\u5177\u6709\u66f4\u9ad8\u7684\u5f3a\u5ea6\u3001\u66f4\u5927\u7684\u5f39\u6027\u6a21\u91cf\u548c\u66f4\u597d\u7684\u53d8\u5f62\u80fd\u529b\uff0c\u5176\u4e2d\uff0c\u63d0\u9ad8\u6df7\u51dd\u571f\u5f3a\u5ea6\u66f4\u662f\u8bf8\u591a\u56fd\u5185\u5916\u7814\u7a76\u8005\u767e\u4f59\u5e74\u6765\u52aa\u529b\u7684\u65b9\u5411\u3002<\/p>\n<p>\u6df7\u51dd\u571f\u7684\u5f3a\u5ea6\u548c\u6c34\u7070\u6bd4\u6709\u5173\uff0c\u6c34\u7070\u6bd4\u8d8a\u5c0f\uff0c\u6df7\u51dd\u571f\u7684\u5f3a\u5ea6\u8d8a\u9ad8\uff0c\u4f46\u4ec5\u9760\u51cf\u5c0f\u6c34\u7070\u6bd4\u63d0\u9ad8\u6df7\u51dd\u571f\u5f3a\u5ea6\u4e5f\u662f\u4e0d\u73b0\u5b9e\u7684\uff0c\u56e0\u4e3a\u8fc7\u5c0f\u6c34\u7070\u6bd4\u7684\u6df7\u51dd\u571f\u5de5\u4f5c\u6027\u3001\u6d41\u52a8\u6027\u975e\u5e38\u5dee\uff0c\u5b9e\u9645\u4e0a\u6210\u4e86\u5e72\u786c\u6027\u6df7\u51dd\u571f\uff0c\u540c\u65f6\u4e5f\u4f7f\u6df7\u51dd\u571f\u53d8\u5f97\u4e0d\u5bc6\u5b9e\uff0c\u5f3a\u5ea6\u53cd\u800c\u964d\u4f4e\u3002<\/p>\n<p>\u51cf\u6c34\u5242\u7684\u53d1\u660e\u4e0e\u5e94\u7528\uff0c\u4ee5\u53ca\u7845\u7070\u3001\u7c89\u7164\u7070\u3001\u6cb8\u77f3\u7c89\u7b49\u4f18\u8d28\u77ff\u7269\u63ba\u6599\u7684\u4f7f\u7528\uff0c\u662f\u6df7\u51dd\u571f\u6280\u672f\u7684\u91cd\u5927\u53d1\u5c55\u3002\u63ba\u5165\u51cf\u6c34\u5242\u53ef\u4ee5\u5927\u5e45\u964d\u4f4e\u6c34\u7070\u6bd4\u5e76\u4fdd\u8bc1\u6df7\u5408\u6599\u7684\u6d41\u52a8\u6027\uff0c\u4f7f\u6df7\u5408\u6599\u7684\u62cc\u5236\u3001\u8fd0\u8f93\u3001\u6d47\u7b51\u548c\u6210\u578b\u7b49\u5de5\u827a\u53d8\u5f97\u5bb9\u6613\uff0c\u63d0\u9ad8\u5f3a\u5ea6\u7684\u540c\u65f6\u6539\u5584\u4e86\u6df7\u51dd\u571f\u7684\u6027\u80fd\uff1b\u7845\u7070\u7b49\u6d3b\u6027\u63ba\u6599\u5219\u53ef\u4ee5\u51cf\u5c11\u6c34\u6ce5\u4e2d\u7684\u78b1\u9aa8\u6599\u53cd\u5e94\uff0c\u540c\u65f6\u6539\u5584\u6df7\u51dd\u571f\u7684\u5b54\u7ed3\u6784\u5e76\u964d\u4f4e\u5b54\u9699\u7387\uff0c\u4ece\u800c\u63d0\u9ad8\u6df7\u51dd\u571f\u7684\u5f3a\u5ea6\u3002<\/p>\n<p>20\u4e16\u7eaa60\u5e74\u4ee3\uff0c\u65e5\u672c\u9996\u5148\u6210\u529f\u7814\u5236\u51fa\u9ad8\u6548\u51cf\u6c34\u5242\uff0c\u4ece\u6b64\u5f00\u8f9f\u4e86\u6df7\u51dd\u571f\u6280\u672f\u7684\u65b0\u65f6\u4ee3\u3002\u9ad8\u6548\u51cf\u6c34\u5242\u4f7f\u6df7\u51dd\u571f\u7684\u9ad8\u5f3a\u548c\u9ad8\u6d41\u6001\u53d8\u5f97\u76f8\u5f53\u5bb9\u6613\uff0c\u4f7f\u9ad8\u5f3a\u6df7\u51dd\u571f\uff08high strength concrete\uff0cHSC\uff09\u7684\u5e7f\u6cdb\u5e94\u7528\u6210\u4e3a\u53ef\u80fd\u3002\u572820\u4e16\u7eaa70\u5e74\u4ee3\u672b\u671f\uff0c\u65e5\u672c\u5df2\u7ecf\u80fd\u591f\u5236\u5907C80~C90\u7684HSC\uff0c90\u5e74\u4ee3\u521d\u671f\uff0c\u65e5\u672c\u96c6\u4e2d\u7814\u7a76\u4f7f\u7528C110HSC\u5efa\u902060~90\u5c42\u9ad8\u5c42\u5efa\u7b51\u7684\u53ef\u884c\u6027\u548c\u5173\u952e\u6280\u672f\uff1b\u5317\u7f8e\u4e8e1976\u5e74\u5f00\u59cb\u91c7\u7528\u9ad8\u6548\u51cf\u6c34\u5242\u5236\u5907HSC\uff0c\u5e76\u5f88\u5feb\u5728\u9ad8\u5c42\u5efa\u7b51\u4e2d\u5e7f\u6cdb\u5e94\u7528\uff1b\u6211\u56fd\u6e05\u534e\u5927\u5b66\u572820\u4e16\u7eaa70\u5e74\u4ee3\u672b\u671f\u81ea\u884c\u7814\u5236\u51fa\u9ad8\u6548\u51cf\u6c34\u5242\u5e76\u6295\u5165\u751f\u4ea7\uff0c\u4e3a\u6211\u56fdHSC\u7684\u53d1\u5c55\u63d0\u4f9b\u4e86\u57fa\u7840\uff0c\u4f46\u76f4\u523080\u5e74\u4ee3\u521d\u671f\uff0c\u6211\u56fd\u624d\u5f00\u59cb\u5bf9HSC\u8fdb\u884c\u5e7f\u6cdb\u7684\u7814\u7a76\u548c\u5e94\u7528\u3002<\/p>\n<p><strong>\u5728HSC\u5e94\u7528\u4e2d\uff0c\u968f\u7740\u65b0\u578b\u5916\u52a0\u5242\u548c\u80f6\u51dd\u6750\u6599\uff08\u5c24\u5176\u662f\u7845\u7070\uff09\u7684\u51fa\u73b0\uff0c\u4f7f\u65e2\u6709\u4f18\u826f\u5de5\u4f5c\u5ea6\uff0c\u53c8\u6709\u4f18\u5f02\u529b\u5b66\u6027\u80fd\u548c\u8010\u4e45\u6027\u7684\u6df7\u51dd\u571f\u751f\u4ea7\u6210\u4e3a\u73b0\u5b9e\uff0c\u8fd9\u79cd\u65b0\u578b\u6df7\u51dd\u571f\u79f0\u4e3a\u9ad8\u6027\u80fd\u6df7\u51dd\u571f\uff08high performance concrete\uff0cHPC\uff09\uff0c\u5e76\u5728\u5b9e\u9645\u5de5\u7a0b\u4e2d\u5f97\u5230\u4e86\u5e94\u7528\u3002<\/strong><\/p>\n<p>\u4f8b\u5982\uff0c\u7f8e\u56fd\u897f\u96c5\u56fe\u7b2c\u4e8c\u8054\u5408\u5e7f\u573a\u5927\u53a6\u662f\u4e16\u754c\u7b2c\u4e00\u5ea7\u91c7\u7528\u5e73\u5747\u6297\u538b\u5f3a\u5ea6\u8fbe120MPa\u7684HPC\u5efa\u9020\u7684\u5efa\u7b51\uff081989\u5e74\uff0c56\u5c42\uff0c\u9ad8226m\uff0cC120\uff09\u3002Scotia\u5927\u53a6\u662f\u52a0\u62ff\u5927\u7528HPC\u5efa\u9020\u7684\u7b2c\u4e00\u5e62\u6df7\u51dd\u571f\u5efa\u7b51\uff081988\u5e74\uff0cC70\uff09\uff0c\u4e5f\u662f\u8be5\u56fd\u6700\u9ad8\u7684\u6df7\u51dd\u571f\u5efa\u7b51\u30021991\u5e74\u6211\u56fd\u7684\u5e7f\u4e1c\u56fd\u8d38\u5927\u53a6\u9996\u6b21\u5e94\u7528C60\u7684HPC\uff0c\u6b64\u540e\uff0cHPC\u5728\u56fd\u5185\u9ad8\u5c42\u5efa\u7b51\u4e2d\u5f97\u5230\u4e86\u5e7f\u6cdb\u5e94\u7528\uff0c\u5982\u4e0a\u6d77\u91d1\u8302\u5927\u53a6\uff08C60\uff09\u3001\u6c88\u9633\u7687\u671d\u4e07\u946b\u56fd\u9645\u5927\u53a6\uff08C60\uff09\u548c\u5317\u4eac\u897f\u7ad9\uff08C60\uff09\u7b49\u5de5\u7a0b\u3002<\/p>\n<p>\u5728\u6865\u6881\u96a7\u9053\u5de5\u7a0b\u4e2d\uff0c\u65e5\u672c\u65e9\u572820\u4e16\u7eaa60\u5e74\u4ee3\u5c31\u91c7\u7528C60\uff5eC80\u6df7\u51dd\u571f\u5efa\u8bbe\u9ad8\u5f3a\u6df7\u51dd\u571f\u94c1\u8def\u6865\u3002\u6cd5\u56fd\u7684\u4f0a\u6c83\u7eb3\u6cb3\u6865\u91c7\u7528C70\u7684HPC\u548c\u4f53\u5916\u9884\u5e94\u529b\u7d22\u7684\u7ed3\u6784\u5f62\u5f0f\uff0c\u4f7f\u6df7\u51dd\u571f\u7528\u91cf\u51cf\u5c1130%\uff0c\u81ea\u91cd\u964d\u4f4e24%\u3002\u7f8e\u56fd\u7ebd\u7ea6\u81ea1996\u5e74\u5c31\u8981\u6c42\u5168\u5dde\u65b0\u5efa\u6865\u6881\u7684\u6865\u9762\u5fc5\u987b\u4f7f\u7528HPC\u3002\u6b27\u6d32\u82f1\u5409\u5229\u6d77\u5ce1\u96a7\u9053\u4f4d\u4e8e\u6d77\u5e73\u9762\u4e0b50\uff5e250m\uff0c\u603b\u957f50.5km\uff0c\u5176\u4e2d37km\u4f4d\u4e8e\u6d77\u5e73\u9762\u4e0b\uff0c\u6574\u4e2a\u96a7\u9053\u7531\u4e09\u6761\u5206\u96a7\u9053\u7ec4\u6210\uff0c\u8bbe\u8ba1\u5bff\u547d\u4e3a120\u5e74\uff0c\u539f\u8bbe\u8ba1\u5f3a\u5ea6\u4e3a45MPa\uff0c\u7531\u4e8e\u8010\u4e45\u6027\u65b9\u9762\u7684\u8981\u6c42\uff0c\u91c7\u7528\u4e86\u5e73\u5747\u6297\u538b\u5f3a\u5ea6\u7ea663MPa\u7684HSC\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101310 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/2-35.jpg\" alt=\"\" width=\"600\" height=\"469\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/2-35.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/2-35-300x235.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><img decoding=\"async\" class=\"img_loading\" src=\"data:image\/gif;base64,iVBORw0KGgoAAAANSUhEUgAAAAEAAAABCAYAAAAfFcSJAAAADUlEQVQImWNgYGBgAAAABQABh6FO1AAAAABJRU5ErkJggg==\" data-s=\"300,640\" data-type=\"jpeg\" data-src=\"http:\/\/mmbiz.qpic.cn\/mmbiz_jpg\/WvZZ689QqoOWEmicia48KRtNVZtJ56ZyJOicAcMmDXhcWXLmkn6TvQv0xTLQyMSbv9oKYccxNzDSGcCfJaCJibbKDQ\/0?wx_fmt=jpeg\" data-ratio=\"0.7830188679245284\" data-w=\"636\" \/>\u5728\u6211\u56fd\uff0c\u4eac\u6d25\u57ce\u9645\u94c1\u8def\u662f\u9996\u6b21\u5728\u8bbe\u8ba1\u4e2d\u63d0\u51fa\u8981\u6c42\u91c7\u7528HPC\u7684\u8f68\u9053\u4ea4\u901a\u5de5\u7a0b\uff0c\u8be5\u5de5\u7a0b2005\u5e74\u5e95\u5f00\u5de5\u81f32008\u5e748\u6708\u5f00\u901a\u8fd0\u8425\uff0c\u5728\u91c7\u7528HPC\u7684\u6240\u6709\u7ed3\u6784\u7269\u4e2d\uff0c\u7ecf\u68c0\u6d4b\u6ca1\u6709\u53d1\u73b0\u6df7\u51dd\u571f\u5f00\u88c2\u3001\u8150\u8680\u3001\u6eb6\u6d1e\u7b49\u73b0\u8c61\uff0c\u6df7\u51dd\u571f\u8868\u73b0\u51fa\u8f83\u597d\u7684\u8010\u4e45\u6027\u3002<\/p>\n<p>\u6211\u56fd\u7684\u4e00\u4e9b\u56fd\u6709\u5927\u578b\u7164\u77ff\u5728\u77ff\u4e95\u65bd\u5de5\u548c\u96a7\u9053\u652f\u62a4\u4e2d\u4e5f\u63a8\u5e7f\u4f7f\u7528HSC\u548cHPC\uff0c\u5982\u6dee\u5357\u77ff\u4e1a\u96c6\u56e2\u4e01\u96c6\u77ff\u5728\u51bb\u7ed3\u6bb5\u4e95\u58c1\u7ed3\u6784\u8bbe\u8ba1\u4e2d\u9996\u6b21\u91c7\u7528\u4e86C60\uff5eC70HSC\u548cHPC\uff0c\u5e76\u5728\u8be5\u77ff\u7684\u4e09\u4e2a\u4e95\u7b52\u51bb\u7ed3\u6bb5\u4e95\u58c1\u5de5\u7a0b\u4e2d\u5f97\u5230\u6210\u529f\u5e94\u7528\u3002\u5728\u6fb3\u5927\u5229\u4e9a\u3001\u52a0\u62ff\u5927\u3001\u65e5\u672c\u548c\u7f8e\u56fd\uff0cHPC\u5df2\u7528\u4e8e\u56fa\u5b9a\u5f0f\u548c\u6f02\u6d6e\u5f0f\u94bb\u4e95\u5e73\u53f0\u3002<\/p>\n<p>HSC\u548cHPC\u7684\u5e7f\u6cdb\u5e94\u7528\uff0c\u4e5f\u66b4\u9732\u51fa\u4e00\u4e9b\u95ee\u9898\u3002\u4e00\u662fHSC\u7684\u9ad8\u8106\u6027\u4e25\u91cd\u5f71\u54cd\u7ed3\u6784\u7684\u6297\u9707\u6027\uff1b\u4e8c\u662fHSC\u6c34\u7070\u6bd4\u8f83\u4f4e\uff0c\u5bb9\u6613\u4ea7\u751f\u8f83\u5927\u7684\u6536\u7f29\u53d8\u5f62\uff0c\u5bfc\u81f4\u7ed3\u6784\u8fc7\u65e9\u51fa\u73b0\u88c2\u7f1d\uff0c\u5f71\u54cd\u7ed3\u6784\u7684\u6b63\u5e38\u4f7f\u7528\u3002\u4f8b\u5982\uff0c\u7f8e\u56fd\u7684\u6df7\u51dd\u571f\u6865\u9762\u677f\u572820\u4e16\u7eaa70\u5e74\u4ee3\u666e\u904d\u5f00\u88c2\uff0c\u4e3a\u5ef6\u957f\u6865\u7684\u4f7f\u7528\u5bff\u547d\u8f6c\u800c\u4f7f\u7528\u66f4\u9ad8\u5f3a\u5ea6\u7684\u6df7\u51dd\u571f\u8fdb\u884c\u7ffb\u4fee\u30021995\u5e74\u7f8e\u56fd\u516c\u8def\u6218\u7565\u7814\u7a76\u8ba1\u5212\u7684\u8c03\u67e5\u7ed3\u679c\u8868\u660e\uff0c\u7ea6\u670910\u4e07\u5ea7\u6865\u6881\u7684\u6865\u9762\u677f\u5728\u6d47\u7b51\u540e\u4e00\u4e2a\u6708\u5185\u4fbf\u51fa\u73b0\u95f4\u96941~3m\u7684\u88c2\u7f1d\u3002\u5206\u6790\u8ba4\u4e3a\uff0cHSC\u65e9\u671f\u7684\u5f39\u6027\u6a21\u91cf\u968f\u5f3a\u5ea6\u5347\u9ad8\u800c\u589e\u5927\uff0c\u540c\u65f6\u53d8\u5f62\u53d7\u7ea6\u675f\u4ea7\u751f\u7684\u5e94\u529b\u677e\u5f1b\u4f5c\u7528\uff08\u5f90\u53d8\uff09\u51cf\u5c0f\uff0c\u5bfc\u81f4\u5b83\u6bd4\u4e2d\u3001\u4f4e\u5f3a\u5ea6\u7684\u6df7\u51dd\u571f\u66f4\u5bb9\u6613\u5f00\u88c2\u3002\u5176\u6b21\uff0c\u7845\u7c89\u63ba\u91cf\u8d8a\u591a\u3001\u6c34\u80f6\u6bd4\u8d8a\u4f4e\u7684\u6df7\u51dd\u571f\uff0c\u65e9\u671f\u5f3a\u5ea6\u53d1\u5c55\u8d8a\u8fc5\u901f\uff0c\u5f00\u88c2\u548c\u5f3a\u5ea6\u5012\u7f29\u73b0\u8c61\u4e5f\u5c31\u8d8a\u663e\u8457\u3002\u6b64\u5916\uff0cHSC\u548cHPC\u5b58\u5728\u8010\u706b\u6027\u80fd\u5dee\u7684\u7f3a\u70b9\uff0c\u5f53\u906d\u53d7\u9ad8\u6e29\u6216\u706b\u707e\u65f6\uff0c\u6e29\u5ea6\u68af\u5ea6\u3001\u5185\u5916\u7ea6\u675f\u3001\u6c34\u6ce5\u6d46\u4f53\u540c\u9aa8\u6599\u70ed\u81a8\u80c0\u7684\u4e0d\u5339\u914d\u4ee5\u53ca\u6e29\u5ea6\u654f\u611f\u6027\u7b49\u4f1a\u5f15\u8d77\u6750\u6599\u70ed\u5f00\u88c2\uff0c\u5bfc\u81f4\u6df7\u51dd\u571f\u7684\u7206\u88c2\u6027\u7834\u574f\uff0c\u8fdb\u800c\u5f15\u53d1\u7ed3\u6784\u7684\u6574\u4f53\u5931\u6548\uff0c\u9020\u6210\u707e\u96be\u6027\u540e\u679c\u30021996\u5e74\u53d1\u751f\u5728\u82f1\u5409\u5229\u6d77\u5ce1\u96a7\u9053\u768410h\u706b\u707e\uff0c\u5bfc\u81f4\u6570\u5343\u7c73\u957f\u7684HPC\uff08\u6297\u538b\u5f3a\u5ea6\u8fbe\u5230100MPa\uff09\u7206\u88c2\uff0c\u9020\u6210\u96a7\u9053\u5185\u8868\u9762\u957f\u7ea640m\u3001\u539a\u7ea6450mm\u7684\u5265\u843d\u53d7\u635f\u30021999\u5e74\u8fde\u63a5\u6cd5\u56fd\u548c\u610f\u5927\u5229\u7684\u52c3\u6717\u5cf0\u96a7\u9053\u53d1\u751f\u706b\u707e\uff0c\u96a7\u9053\u4e2d\u7684\u6df7\u51dd\u571f\u886c\u780c\u88ab\u5168\u90e8\u70e7\u6bc1\uff0c\u4e8b\u6545\u53d1\u751f\u540e\uff0c\u8be5\u96a7\u9053\u88ab\u5173\u95ed\u7ef4\u4fee\u957f\u8fbe\u4e24\u5e74\u4e4b\u4e45\u3002\u7f8e\u56fd\u201c9\u00b711\u201d\u4e8b\u4ef6\u4e2d\u4e16\u8d38\u4e2d\u5fc3\u914d\u697c\u7684\u574d\u584c\u4e5f\u662f\u4e00\u4e2a\u8457\u540d\u7684\u4f8b\u5b50\uff0c\u94a2\u7b4b\u6df7\u51dd\u571f\u5927\u53a6\u5728800\u2103\u4ee5\u4e0a\u9ad8\u6e29\u4f5c\u7528\u4e0b\uff0c\u56e0\u7ed3\u6784\u4e27\u5931\u627f\u8f7d\u529b\u800c\u53d1\u751f\u574d\u584c\u3002\u6b64\u5916\uff0c\u6e29\u5ea6\u7684\u6301\u7eed\u4f5c\u7528\u8fd8\u4f1a\u5bfc\u81f4\u670d\u5f79\u671f\u5185\u6df7\u51dd\u571f\u7ed3\u6784\u7684\u8010\u4e45\u6027\u964d\u4f4e\uff0c\u4f7f\u7ed3\u6784\u8fc7\u65e9\u5730\u8fdb\u5165\u5927\u4fee\u9636\u6bb5\u6216\u8005\u63d0\u524d\u7ed3\u675f\u670d\u5f79\u5e74\u9650\u3002<\/p>\n<p>\u4e3a\u907f\u514d\u4e0a\u8ff0\u95ee\u9898\u7684\u53d1\u751f\uff0c\u5e38\u5728\u7845\u7070\u6df7\u51dd\u571f\u4e2d\u63ba\u5165\u94a2\u7ea4\u7ef4\u6765\u589e\u52a0\u6df7\u51dd\u571f\u7684\u97e7\u6027\u3001\u63a7\u5236\u5176\u5f00\u88c2\uff1b\u901a\u8fc7\u5728\u6df7\u51dd\u571f\u4e2d\u63ba\u52a0\u53ef\u7194\u7684\u6709\u673a\u7ea4\u7ef4\u3001\u5728\u6df7\u51dd\u571f\u5916\u5c42\u8bbe\u7f6e\u963b\u706b\u5c4f\u969c\u4ee5\u53ca\u5728\u6df7\u51dd\u571f\u5916\u5c42\u52a0\u8bbe\u94a2\u7b4b\u7f51\u6216\u8986\u76d6\u94a2\u677f\u3001\u94a2\u7b4b\u7f51\u7247\u7b49\u65b9\u6cd5\u6765\u9632\u6b62\u6df7\u51dd\u571f\u7684\u7206\u88c2\u98de\u6563\u3002\u4f46\u662f\uff0c\u63ba\u52a0\u94a2\u7ea4\u7ef4\u65f6\u7c97\u9aa8\u6599\u7684\u5b58\u5728\u4f1a\u4f7f\u94a2\u7ea4\u7ef4\u7684\u201c\u67b6\u6865\u201d\u4f5c\u7528\u53d7\u5230\u9650\u5236\uff0c\u800c\u4e14\u957f\u7684\u94a2\u7ea4\u7ef4\u5bf9\u62cc\u5408\u7269\u7684\u5de5\u4f5c\u5ea6\u5f71\u54cd\u53c8\u5341\u5206\u663e\u8457\u3002<\/p>\n<p><strong>1993\u5e74\uff0c\u6cd5\u56fdBOUYGUES\u516c\u53f8\u7684Richard\u548cCheyrezy\u4eff\u6548\u9ad8\u81f4\u5bc6\u6c34\u6ce5\u57fa\u5747\u5300\u4f53\u7cfb\uff08densified system containing homogeneously arranged ultrafine particles\uff0cDSP\uff09\uff0c\u5c06\u5176\u4e2d\u7684\u7c97\u9aa8\u6599\u5254\u9664\uff0c\u6362\u7528\u6700\u5927\u7c92\u5f84\u4e3a400~600\u03bcm\u7684\u77f3\u82f1\u7802\u4f5c\u4e3a\u9aa8\u6599\uff0c\u63ba\u5165\u9002\u91cf\u77ed\u7ea4\u7ef4\u548c\u7845\u7070\u7b49\u6d3b\u6027\u77ff\u7269\u63ba\u6599\uff0c\u901a\u8fc7\u6210\u578b\u65bd\u538b\u3001\u70ed\u517b\u62a4\u7b49\u5de5\u827a\uff0c\u5236\u5907\u51fa\u5f3a\u5ea6\u9ad8\u3001\u5176\u4ed6\u6027\u80fd\u4f18\u5f02\u7684\u6c34\u6ce5\u57fa\u590d\u5408\u6750\u6599\uff0c\u7531\u4e8e\u8fd9\u79cd\u6df7\u51dd\u571f\u589e\u52a0\u4e86\u7ec4\u5206\u7684\u7ec6\u5ea6\u548c\u53cd\u5e94\u6d3b\u6027\uff0c\u56e0\u6b64\u79f0\u4e3aRPC\u3002\u8be5\u6750\u6599\u7533\u62a5\u4e86\u4e13\u5229\uff0c\u5e76\u57281994\u5e74\u7f8e\u56fd\u6df7\u51dd\u571f\u5b66\u4f1a\u65e7\u91d1\u5c71\u6625\u5b63\u4f1a\u8bae\u4e0a\u9996\u6b21\u516c\u5f00\u30021998\u5e748\u6708\u5728\u52a0\u62ff\u5927\u9b41\u5317\u514b\u7701Sherbrooke\u5927\u5b66\u53ec\u5f00\u4e86\u7b2c\u4e00\u6b21\u6709\u5173RPC\u548cHPC\u7684\u56fd\u9645\u7814\u8ba8\u4f1a\uff0c\u4e0e\u4f1a\u4e13\u5bb6\u5c31RPC\u7684\u539f\u7406\u3001\u6027\u80fd\u548c\u5e94\u7528\u8fdb\u884c\u4e86\u5e7f\u6cdb\u6df1\u5165\u7684\u8ba8\u8bba\uff0c\u4e00\u81f4\u8ba4\u4e3a\uff1aRPC\u4f5c\u4e3a\u4e00\u79cd\u65b0\u578b\u6750\u6599\uff0c\u5177\u6709\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u3002<\/strong><\/p>\n<p>RPC\u6839\u636e\u5176\u6297\u538b\u5f3a\u5ea6\u5206\u4e3aRPC200\u548cRPC800\u4e24\u7ea7\u3002\u5176\u4e2d\uff0cRPC200\u7684\u5236\u5907\u6761\u4ef6\u63a5\u8fd1\u666e\u901a\u6df7\u51dd\u571f\uff08normal concrete\uff0cNC\uff09\uff0c\u5b83\u5728\u51dd\u56fa\u671f\u5185\u4e0d\u9700\u52a0\u538b\uff0c\u91c7\u7528\u70ed\u517b\u62a4\uff0c\u517b\u62a4\u6e29\u5ea6\u4e3a20~90\u2103\uff1bRPC800\u5728\u51dd\u56fa\u671f\u5185\u65bd\u52a010~50MPa\u7684\u538b\u529b\uff0c\u5e76\u5728250~400\u2103\u9ad8\u6e29\u4e0b\u517b\u62a4\u5236\u5f97\u3002\u51dd\u56fa\u671f\u5185RPC200\u7684\u6297\u538b\u5f3a\u5ea6\u53ef\u8fbe170~230MPa\uff0c\u662fHSC\u76843~12\u500d\uff0cRPC800\u7684\u6297\u538b\u5f3a\u5ea6\u5219\u9ad8\u8fbe500~800MPa\u3002\u91cd\u8981\u7684\u662f\uff0cRPC\u7684\u6297\u6298\u5f3a\u5ea6\u548c\u65ad\u88c2\u80fd\u5927\u5927\u63d0\u9ad8\uff0c\u6297\u6298\u5f3a\u5ea6\u8fbe50~60MPa\uff0c\u662fHSC\u768410\u500d\uff0c\u63ba\u5165\u5fae\u7ec6\u94a2\u7ea4\u7ef4\u80fd\u663e\u8457\u63d0\u9ad8RPC\u7684\u97e7\u6027\u548c\u65ad\u88c2\u80fd\uff0c\u5176\u65ad\u88c2\u80fd\u53ef\u8fbe3\u00d7104J\/m<sup>2<\/sup>\uff0c\u8db3\u53ef\u4e0e\u91d1\u5c5e\u5ab2\u7f8e\uff0c\u800c\u666e\u901a\u6df7\u51dd\u571f\u7684\u65ad\u88c2\u80fd\u4ec5\u4e3a120J\/m2\uff0c\u6709\u6548\u514b\u670d\u4e86HSC\u7684\u9ad8\u8106\u6027\u3002<\/p>\n<p><strong>\u88681<\/strong> \u7ed9\u51fa\u4e86RPC200\u548cRPC800\u7684\u5178\u578b\u914d\u6bd4\u3002<strong>\u88682 <\/strong>\u6bd4\u8f83\u4e86RPC\u548cHSC\u7684\u529b\u5b66\u6027\u80fd\u6307\u6807\uff0c<strong>\u88683<\/strong> \u7ed9\u51fa\u4e86\u4e00\u4e9b\u6750\u6599\u7684\u65ad\u88c2\u80fd\uff0c<strong>\u56fe1<\/strong> \u8868\u793a\u4e0d\u540c\u6750\u6599\u7684\u65ad\u88c2\u80fd\u3002<\/p>\n<p style=\"text-align: center;\"><strong>\u88681 RPC200\u548cRPC800\u7684\u5178\u578b\u914d\u6bd4\uff08\u4ee5\u91cd\u91cf\u8ba1\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101311 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/3-28.jpg\" alt=\"\" width=\"600\" height=\"306\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/3-28.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/3-28-300x153.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"text-align: center;\"><img decoding=\"async\" class=\"img_loading\" src=\"data:image\/gif;base64,iVBORw0KGgoAAAANSUhEUgAAAAEAAAABCAYAAAAfFcSJAAAADUlEQVQImWNgYGBgAAAABQABh6FO1AAAAABJRU5ErkJggg==\" data-s=\"300,640\" data-type=\"jpeg\" data-src=\"http:\/\/mmbiz.qpic.cn\/mmbiz_jpg\/WvZZ689QqoOWEmicia48KRtNVZtJ56ZyJOHTx31pQumtMtm6gQOf3VdmJKicsjzic3ExAy0iaN9bqnjoIHskgg20ORQ\/0?wx_fmt=jpeg\" data-ratio=\"0.510752688172043\" data-w=\"744\" \/><strong>\u88682 RPC\u548cHSC\u7684\u529b\u5b66\u6027\u80fd\u6307\u6807<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101312 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/4-28.jpg\" alt=\"\" width=\"600\" height=\"125\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/4-28.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/4-28-300x63.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"text-align: center;\"><img decoding=\"async\" class=\"img_loading\" src=\"data:image\/gif;base64,iVBORw0KGgoAAAANSUhEUgAAAAEAAAABCAYAAAAfFcSJAAAADUlEQVQImWNgYGBgAAAABQABh6FO1AAAAABJRU5ErkJggg==\" data-s=\"300,640\" data-type=\"jpeg\" data-src=\"http:\/\/mmbiz.qpic.cn\/mmbiz_jpg\/WvZZ689QqoOWEmicia48KRtNVZtJ56ZyJOmGDprcib8Dt7icYLXCQ6M2mNKZ2xttOQrnpWh92TMvKTg0Cw7CRBiaGicg\/0?wx_fmt=jpeg\" data-ratio=\"0.20967741935483872\" data-w=\"744\" \/><strong>\u88683 \u4e0d\u540c\u6750\u6599\u7684\u65ad\u88c2\u80fd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101313 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/5-25.jpg\" alt=\"\" width=\"600\" height=\"58\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/5-25.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/5-25-300x29.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101314 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/6-14.jpg\" alt=\"\" width=\"500\" height=\"296\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/6-14.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/6-14-300x178.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: center;\"><img decoding=\"async\" class=\"img_loading\" src=\"data:image\/gif;base64,iVBORw0KGgoAAAANSUhEUgAAAAEAAAABCAYAAAAfFcSJAAAADUlEQVQImWNgYGBgAAAABQABh6FO1AAAAABJRU5ErkJggg==\" data-s=\"300,640\" data-type=\"jpeg\" data-src=\"http:\/\/mmbiz.qpic.cn\/mmbiz_jpg\/WvZZ689QqoOWEmicia48KRtNVZtJ56ZyJO568EY6lA78KVkAB9jSEGJesY4ehIS8o4fm5IykGRqcqLc3ZzQXZTiaA\/0?wx_fmt=jpeg\" data-ratio=\"0.0967741935483871\" data-w=\"744\" \/><strong>\u56fe1 \u4e0d\u540c\u6750\u6599\u7684\u65ad\u88c2\u80fd<\/strong><\/p>\n<p>RPC\u6c34\u80f6\u6bd4\u6781\u4f4e\uff0c\u826f\u597d\u7684\u5b54\u7ed3\u6784\u548c\u5b54\u9699\u7387\u4f7f\u5176\u5177\u6709\u6781\u4f4e\u7684\u6e17\u900f\u6027\u3001\u8f83\u9ad8\u7684\u6297\u73af\u5883\u4ecb\u8d28\u4fb5\u8680\u80fd\u529b\u548c\u826f\u597d\u7684\u8010\u78e8\u6027\u80fd\uff0c\u4ece\u800c\u4f7fRPC\u5177\u6709\u4f18\u5f02\u7684\u8010\u4e45\u6027\u3002<strong>\u88684<\/strong>\u662fRPC\u3001HPC\u4e0eNC\u7684\u8010\u4e45\u6027\u6bd4\u8f83\u3002<\/p>\n<p style=\"text-align: center;\"><strong>\u88684 RPC\u3001HPC\u548cNC\u7684\u8010\u4e45\u6027\u5bf9\u6bd4<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101315 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/7-9.jpg\" alt=\"\" width=\"600\" height=\"129\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/7-9.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/7-9-300x65.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u6d3b\u6027\u7c89\u672b\u6df7\u51dd\u571f(RPC)\u662f20\u4e16\u7eaa90\u5e74\u4ee3\u7814\u53d1\u7684\u4e00\u79cd\u5177\u6709\u8d85\u9ad8\u5f3a\u5ea6\u548c\u9ad8\u97e7\u6027\u7684\u65b0\u578b\u6c34\u6ce5\u57fa\u590d\u5408\u6750\u6599\u3002<strong>\u300a\u6d3b\u6027\u7c89\u672b\u6df7\u51dd\u571f\u7684\u5236\u5907\u4e0e\u7269\u7406\u529b\u5b66\u6027\u80fd\u300b<\/strong>\u7cfb\u7edf\u603b\u7ed3\u4f5c\u8005\u56e2\u961f10\u5e74\u6765\u5728RPC\u7814\u7a76\u65b9\u9762\u53d6\u5f97\u7684\u4e3b\u8981\u8fdb\u5c55\u3002\u5168\u4e66\u517110\u7ae0\uff0c\u5305\u62ecRPC\u7684\u5236\u5907\u539f\u7406\u53ca\u914d\u6bd4\u3001RPC\u7684\u9759\u529b\u5b66\u6027\u80fd\u3001\u94a2\u7ea4\u7ef4RPC\u7684\u9ecf\u7ed3\u673a\u7406\u3001RPC\u7684\u65ad\u88c2\u97e7\u6027\u53ca\u8868\u5f81\u65b9\u6cd5\u3001RPC\u7684\u5c3a\u5bf8\u6548\u5e94\u3001RPC\u7684\u52a8\u6001\u529b\u5b66\u6027\u80fd\u3001RPC\u7684\u70ed\u7269\u7406\u6027\u8d28\u3001RPC\u7684\u5185\u90e8\u6e29\u5ea6\u573a\u3001\u84b8\u6c7d\u538b\u5206\u5e03\u53ca\u7206\u88c2\u3001\u9ad8\u6e29\u4e0bRPC\u5185\u90e8\u6e29\u5ea6\u5e94\u529b\u7684\u6570\u503c\u8ba1\u7b97\u53ca\u7206\u88c2\u673a\u7406\u7b49\u65b9\u9762\u7684\u5185\u5bb9\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101317 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/8-9.jpg\" alt=\"\" width=\"400\" height=\"400\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/8-9.jpg 400w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/8-9-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/8-9-300x300.jpg 300w\" sizes=\"(max-width: 400px) 100vw, 400px\" \/><\/p>\n<p>\u6750\u6599\u4eba\u4e0e\u79d1\u5b66\u51fa\u7248\u793e\u63a8\u51fa\u8054\u5408\u8350\u4e66\u4e13\u9898\uff0c\u6301\u7eed\u5411\u8bfb\u8005\u63a8\u8350\u7ecf\u5178\u6750\u6599\u4e13\u8457\uff0c\u901a\u8fc7\u5bf9\u4e66\u7c4d\u7cbe\u9009\u5185\u5bb9\u7684\u5256\u6790\u629b\u7816\u5f15\u7389\uff0c\u626b\u63cf\u4e0b\u65b9\u4e8c\u7ef4\u7801\u8d2d\u4e70\u6b64\u4e66\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-101316 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/9-4.png\" alt=\"\" width=\"100\" height=\"100\" \/><\/p>\n<p>\u672c\u6587\u7531\u5fae\u4fe1\u516c\u4f17\u53f7\u79d1\u5b66\u51fa\u7248\u793e\uff08ID:sciencepress-cspm\uff09\u6388\u6743\u8f6c\u8f7d\uff0c\u7531\u6750\u6599\u4eba\u7f51\u5927\u57ce\u5c0f\u7231\u7f16\u8f91\u6574\u7406\uff0c\u6750\u6599\u4eba\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.htm\" target=\"_blank\" rel=\"noopener noreferrer\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p><strong>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u627e<a href=\"http:\/\/mai.cailiaoren.com\/\" target=\"_blank\" rel=\"noopener noreferrer\">\u6750\u6599\u4eba<\/a>\u3001\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener noreferrer\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u6df7\u51dd\u571f\u662f\u5f53\u4eca\u571f\u6728\u5efa\u7b51\u5de5\u7a0b\u5e7f\u6cdb\u4f7f\u7528\u7684\u5efa\u7b51\u6750\u6599\uff0c\u968f\u7740\u79d1\u5b66\u6280\u672f\u7684\u8fdb\u6b65\u548c\u57ce\u5e02\u5316\u89c4\u6a21\u7684\u4e0d\u65ad\u6269\u5927\uff0c\u73b0\u4ee3\u5efa\u7b51\u65e5\u76ca\u5411\u9ad8\u5c42\u3001\u5927\u8de8\u548c\u5730\u4e0b\u53d1\u5c55\uff0c\u5bf9\u5efa\u7b51\u7ed3\u6784\u7684\u5b89\u5168\u6027\u3001\u9002\u7528\u6027\u548c\u8010\u4e45\u6027\u63d0\u51fa&#8230;<\/p>\n","protected":false},"author":1369,"featured_media":101309,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-101308","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/101308"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/1369"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=101308"}],"version-history":[{"count":1,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/101308\/revisions"}],"predecessor-version":[{"id":101318,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/101308\/revisions\/101318"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/101309"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=101308"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=101308"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=101308"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}