{"id":102309,"date":"2017-09-19T06:30:18","date_gmt":"2017-09-18T22:30:18","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=102309"},"modified":"2017-09-17T10:05:08","modified_gmt":"2017-09-17T02:05:08","slug":"%e5%ad%a6%e6%9c%af%e5%b9%b2%e8%b4%a7%e2%94%82%e8%88%aa%e7%a9%ba%e7%94%a8%e9%92%9b%e5%90%88%e9%87%91%e7%a0%94%e7%a9%b6%e8%bf%9b%e5%b1%95","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=102309","title":{"rendered":"\u5b66\u672f\u5e72\u8d27\u2502\u822a\u7a7a\u7528\u949b\u5408\u91d1\u7814\u7a76\u8fdb\u5c55"},"content":{"rendered":"<p><strong>\u5f15\u8a00\uff1a<\/strong>\u949b\u5408\u91d1\u7531\u4e8e\u5176\u6bd4\u5f3a\u5ea6\u9ad8\u3001\u8010\u8150\u8680\u6027\u597d\u7b49\u4f18\u70b9\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u822a\u7a7a\u822a\u5929\u9886\u57df\u3002\u672c\u6587\u4ecb\u7ecd\u4e86\u8fd1\u5e74\u6765\u4e3b\u8981\u949b\u5408\u91d1\u7684\u7814\u7a76\u8fdb\u5c55\uff0c\u5305\u62ec\u9ad8\u5f3a\u9ad8\u97e7\u578b\u949b\u5408\u91d1\uff08Ti-1023\u3001Ti-15-3\u3001\u03b221S\u548cBT-22\uff09\u3001\u9ad8\u6e29\u949b\u5408\u91d1\uff08IMI834\u3001Ti-1100\u3001BT36\u548cTi-60\uff09\u3001\u635f\u4f24\u5bb9\u9650\u949b\u5408\u91d1\uff08TC21\u548cTC4-DT\uff09\u548c\u963b\u71c3\u949b\u5408\u91d1\uff08Alloy C\u3001BTT-l\u548cBTT-3\uff094\u4e2a\u65b9\u9762\uff0c\u5e76\u5c55\u671b\u4e86\u822a\u7a7a\u822a\u5929\u7528\u949b\u5408\u91d1\u7684\u53d1\u5c55\u65b9\u5411\u3002<\/p>\n<p>\u949b\u662f\u5e7f\u6cdb\u5e94\u7528\u4e8e\u822a\u7a7a\u822a\u5929\u9886\u57df\u7684\u4e00\u79cd\u91cd\u8981\u7ed3\u6784\u91d1\u5c5e\uff0c\u5176\u5177\u6709\u6bd4\u5f3a\u5ea6\u9ad8\u3001\u8010\u8150\u8680\u6027\u80fd\u597d\u4ee5\u53ca\u4f7f\u7528\u6e29\u5ea6\u8303\u56f4\u5bbd\uff08-269-600\u2103\uff09\u7684\u663e\u8457\u4f18\u70b9\uff0c\u949b\u6750\u7684\u6bd4\u5f3a\u5ea6\u4f4d\u5c45-253\uff5e600\u2103\u5185\u5e38\u7528\u91d1\u5c5e\u6750\u6599\u4e4b\u9996\uff0c\u56e0\u6b64\u5f88\u5feb\u88ab\u7528\u4e8e\u822a\u7a7a\u5de5\u4e1a\u3002\u822a\u7a7a\u59cb\u7ec8\u662f50\u5e74\u6765\u4e16\u754c\u949b\u5e02\u573a\u4e2d\u6700\u5927\u7684\u7528\u6237\uff0c\u56fe1\u7ed9\u51fa\u4e86A350\u7528\u949b\u7684\u4e3b\u8981\u90e8\u4f4d\u548c\u90e8\u4ef6\u3002\u76ee\u524d\uff0c\u5148\u8fdb\u98de\u673a\u4e0a\u7684\u949b\u6750\u91cd\u91cf\u5df2\u8fbe\u98de\u673a\u7ed3\u6784\u603b\u91cd\u768430%\uff5e35%\uff0c\u949b\u6750\u5df2\u6210\u4e3a\u73b0\u4ee3\u98de\u673a\u4e0d\u53ef\u7f3a\u5c11\u7684\u7ed3\u6784\u6750\u6599\u3002\u8fd1\u5e74\u6765\uff0c\u7531\u4e8e\u822a\u7a7a\u5de5\u4e1a\u5bf9\u9ad8\u5f3a\u5ea6\u3001\u9ad8\u5f39\u6027\u6a21\u91cf\u3001\u8010\u9ad8\u6e29\u3001\u4f4e\u5bc6\u5ea6\u7684\u65b0\u578b\u7ed3\u6784\u6750\u6599\u9700\u8981\u65e5\u76ca\u8feb\u5207\uff0c\u5927\u5927\u4fc3\u8fdb\u4e86\u949b\u5236\u9020\u4e1a\u7684\u8fc5\u901f\u53d1\u5c55\u3002\u56e0\u6b64\uff0c\u672c\u6587\u9996\u5148\u4ecb\u7ecd\u4e86\u949b\u5408\u91d1\u7684\u5178\u578b\u7ec4\u7ec7\u7c7b\u578b\u53ca\u76f8\u5e94\u7684\u6027\u80fd\uff0c\u7136\u540e\u4ece\u8fd1\u5e74\u6240\u5f00\u53d1\u7684\u65b0\u578b\u949b\u5408\u91d1\u7b80\u8ff0\u5176\u7814\u7a76\u8fdb\u5c55\uff0c\u4e3b\u8981\u5206\u4e3a\u4ee5\u4e0b\u56db\u7c7b\uff1a(1)\u9ad8\u5f3a\u9ad8\u97e7\u578b\u949b\u5408\u91d1\uff1b(2)\u9ad8\u6e29\u949b\u5408\u91d1\uff1b(3) \u635f\u4f24\u5bb9\u9650\u949b\u5408\u91d1\uff1b(4)\u963b\u71c3\u949b\u5408\u91d1\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-102315\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/QQ\u56fe\u724720170916170303.jpg\" alt=\"\" width=\"500\" height=\"325\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/QQ\u56fe\u724720170916170303.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/QQ\u56fe\u724720170916170303-300x195.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe1\u00a0 A350\u7528\u949b\u4e3b\u8981\u90e8\u4f4d\u548c\u90e8\u4ef6<\/p>\n<p><span style=\"color: #0000ff;\"><strong>\u4e00\u3001\u949b\u5408\u91d1\u7684\u5178\u578b\u7ec4\u7ec7\u7c7b\u578b\u53ca\u76f8\u5e94\u7684\u6027\u80fd<\/strong><\/span><\/p>\n<p>\u949b\u548c\u949b\u5408\u91d1\u94f8\u4ef6\u7684\u663e\u5fae\u7ec4\u7ec7\u901a\u5e38\u90fd\u662f\u4ece\u9ad8\u6e29\u03b2\u533a\u51b7\u5374\u4e0b\u6765\u5f62\u6210\u7684\u8f6c\u53d8\u7684\u03b2\u7ec4\u7ec7\uff0c\u7ec4\u7ec7\u4fdd\u6301\u7740\u539f\u59cb\u7684\u03b2\u6676\u754c\uff0c\u6676\u754c\u5185\u7531\u9488\u72b6\u6216\u7247\u72b6\u4ee5\u53ca\u7f51\u7bee\u72b6\u7684\u03b1\u76f8\u7ec4\u6210\uff0c\u7ecf\u8fc7\u53d8\u5f62\u52a0\u5de5\u548c\u70ed\u5904\u7406\u53ef\u83b7\u5f97\u4e0d\u540c\u7684\u7ec4\u7ec7\u7ed3\u6784\u3002\u56fe2\u6240\u793a\u4e3a\u5178\u578b\u7684\u949b\u5408\u91d1\u7ec4\u7ec7\u5f62\u8c8c\u3002\u901a\u5e38\u949b\u5408\u91d1\u7ec4\u7ec7\u6309\u5f62\u6001\u7279\u5f81\u53ef\u4ee5\u5206\u4e3a\uff1a\u9b4f\u6c0f\u7ec4\u7ec7\u3001\u53cc\u6001\u7ec4\u7ec7\u3001\u7f51\u7bee\u7ec4\u7ec7\u548c\u7b49\u8f74\u7ec4\u7ec7\u3002\u4e0a\u8ff0\u7ec4\u7ec7\u5f62\u6210\u4e3b\u8981\u53d6\u51b3\u4e8e\u70ed\u53d8\u5f62\u548c\u70ed\u5904\u7406\u5de5\u827a\u3002<\/p>\n<p>(1) <strong>\u9b4f\u6c0f\u7ec4\u7ec7<\/strong>\uff1a\u5176\u7279\u70b9\u662f\u539f\u59cb\u03b2\u6676\u7c92\u7c97\u5927\u6e05\u6670\u5b8c\u6574\uff0c\u6676\u754c\u4e0a\u6709\u975e\u5e38\u660e\u663e\u7684\u8fde\u7eed\u03b1\u76f8\uff0c\u6676\u5185\u4e3a\u7c97\u5927\u7247\u72b6\u6709\u89c4\u5219\u5e73\u884c\u6392\u5217\u7684\u03b1\u76f8\u675f\u57df\uff0c\u7247\u95f4\u4e3a\u03b2\u76f8(\u56fe2a)\u3002\u5f53\u5408\u91d1\u53d8\u5f62\u7684\u5f00\u59cb\u6e29\u5ea6\u548c\u7ec8\u4e86\u6e29\u5ea6\u90fd\u5728\u03b2\u76f8\u533a\u4e14\u53d8\u5f62\u91cf\u4e0d\u5927\u65f6\uff0c\u6216\u5c06\u5408\u91d1\u52a0\u70ed\u5230\u03b2\u76f8\u533a\u8f83\u6162\u51b7\u5374\u65f6\uff0c\u90fd\u5c06\u5f62\u6210\u8fd9\u79cd\u7ec4\u7ec7\u3002<\/p>\n<p>(2) <strong>\u53cc\u6001\u7ec4\u7ec7<\/strong>\uff1a\u5176\u7279\u70b9\u662f\u5728\u8f6c\u53d8\u03b2\u7ec4\u7ec7\u57fa\u4f53\u4e0a\u5206\u5e03\u6709\u4e00\u5b9a\u6570\u91cf\u7684\u4e0d\u8fde\u7eed\u7684\u521d\u751f\u7b49\u8f74\u03b1\u76f8\u6676\u7c92\uff0c\u4f46\u603b\u542b\u91cf\u5c0f\u4e8e50%\uff0c\u56e0\u800c\u7ec4\u7ec7\u4e2d\u6709\u7b49\u8f74\u521d\u751f\u03b1\u4e0e\u03b2\u8f6c\u53d8\u7ec4\u7ec7\u4e2d\u7684\u7247\u72b6\u03b1\u4e24\u79cd\u5f62\u6001(\u56fe2b)\u3002\u5f53\u5408\u91d1\u5728\u03b1+\u03b2\u4e24\u76f8\u533a\u7684\u4e0a\u90e8\u6e29\u5ea6\u52a0\u70ed\u548c\u53d8\u5f62\u65f6\u53ef\u5f62\u6210\u8fd9\u79cd\u7ec4\u7ec7\u3002\u8fd9\u7c7b\u7ec4\u7ec7\u5177\u6709\u8f83\u597d\u7684\u7efc\u5408\u529b\u5b66\u6027\u80fd\u3002<\/p>\n<p>(3) <strong>\u7f51\u7bee\u7ec4\u7ec7<\/strong>\uff1a\u5176\u7279\u5f81\u662f\u539f\u59cb\u03b2\u6676\u7c92\u6676\u754c\u4e0d\u540c\u7a0b\u5ea6\u5730\u88ab\u7834\u574f\uff0c\u6676\u5185\u03b1\u7247\u53d8\u77ed\uff0c\u03b1\u76f8\u53d6\u5411\u6df7\u6742\uff0c\u4ea4\u9519\u6392\u5217\uff0c\u5f62\u6210\u7f16\u7ec7\u7f51\u7bee\u72b6\u7ed3\u6784(\u56fe2c)\u3002\u5f53\u5408\u91d1\u5728\u03b2\u8f6c\u53d8\u70b9\u9644\u8fd1\u7ecf\u8fc7\u8f83\u5927\u53d8\u5f62\uff0c\u800c\u5728\u03b1+\u03b2\u4e24\u76f8\u533a\u53d8\u5f62\u91cf\u4e0d\u591f\u5927\u65f6\u5f62\u6210\u8fd9\u79cd\u7ec4\u7ec7\u3002\u5176\u7279\u70b9\u662f\uff1a\u5851\u6027\u3001\u51b2\u51fb\u97e7\u6027\u597d\uff0c\u4e14\u5177\u6709\u8f83\u597d\u7684\u9ad8\u6e29\u6301\u4e45\u548c\u6297\u8815\u53d8\u6027\u80fd\u3002<\/p>\n<p>(4) <strong>\u7b49\u8f74\u7ec4\u7ec7<\/strong>\uff1a\u5176\u7279\u70b9\u662f\u542b\u6709\u8f83\u591a\u7684(\u8d8550%)\u521d\u751f\u03b1\u6676\u7c92\uff0c\u5b58\u5728\u7740\u4e00\u5b9a\u6570\u91cf\u7684\u03b2\u8f6c\u53d8\u7ec4\u7ec7\uff0c\u5206\u5e03\u5728\u03b1\u76f8\u8fb9\u754c\u5904\uff0c\u5747\u5448\u7b49\u8f74\u6216\u591a\u8fb9\u5f62(\u56fe2d)\u3002\u7247\u72b6\u03b1\u7ecf\u53d8\u5f62\u540e\u52a0\u70ed\u53ef\u5f62\u6210\u7b49\u8f74\u03b1\uff0c\u7b49\u8f74\u5316\u7a0b\u5ea6\u7684\u5927\u5c0f\uff0c\u53d7\u53d8\u5f62\u7a0b\u5ea6\u3001\u52a0\u70ed\u6e29\u5ea6\u548c\u4fdd\u6e29\u65f6\u95f4\u7684\u5f71\u54cd\u3002\u603b\u7684\u8d8b\u52bf\u662f\u968f\u7740\u53d8\u5f62\u7a0b\u5ea6\u7684\u589e\u5927\uff0c\u52a0\u70ed\u6e29\u5ea6\u5347\u9ad8\uff0c\u4fdd\u6e29\u65f6\u95f4\u5ef6\u957f\uff0c\u7b49\u8f74\u5316\u7a0b\u5ea6\u52a0\u5927\u3002\u8fd9\u79cd\u7ec4\u7ec7\u7684\u7279\u70b9\u662f\u7efc\u5408\u6027\u80fd\u597d\uff0c\u7279\u522b\u662f\u5851\u6027\u548c\u51b2\u51fb\u97e7\u6027\u8f83\u9ad8\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-102314\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/QQ\u56fe\u724720170913111356.jpg\" alt=\"\" width=\"700\" height=\"539\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/QQ\u56fe\u724720170913111356.jpg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/09\/QQ\u56fe\u724720170913111356-300x231.jpg 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe2 \u949b\u5408\u91d1\u57fa\u672c\u7ec4\u7ec7\uff1a(a) \u9b4f\u6c0f\u7ec4\u7ec7\uff0c(b) \u7f51\u7bee\u7ec4\u7ec7\uff0c(c) \u7b49\u8f74\u7ec4\u7ec7\uff0c(d) \u53cc\u6001\u7ec4\u7ec7<\/p>\n<p><span style=\"color: #0000ff;\"><strong>\u4e8c\u3001\u65b0\u578b\u949b\u5408\u91d1<\/strong><\/span><\/p>\n<p><strong>1<\/strong><strong>\u3001\u9ad8\u5f3a\u9ad8\u97e7<\/strong><strong>\u03b2<\/strong><strong>\u578b\u949b\u5408\u91d1<\/strong><strong>\u00a0\u00a0\u00a0\u00a0 <\/strong><\/p>\n<p>\u00a0\u00a0\u03b2\u578b\u949b\u5408\u91d1\u5177\u6709\u826f\u597d\u7684\u52a0\u5de5\u6027\u80fd\uff0c\u6613\u953b\u9020\u3001\u53ef\u8f67\u5236\u3001\u710a\u63a5\uff0c\u53ef\u901a\u8fc7\u56fa\u6eb6\u65f6\u6548\u5904\u7406\u83b7\u5f97\u8f83\u9ad8\u5f3a\u5ea6\u548c\u65ad\u88c2\u97e7\u6027\u3002\u76ee\u524d\uff0c\u5728\u98de\u673a\u4e0a\u83b7\u5f97\u5b9e\u9645\u5e94\u7528\u7684\u9ad8\u5f3a\u9ad8\u97e7\u03b2\u578b\u949b\u5408\u91d1\u4e3b\u8981\u6709\u4ee5\u4e0b\u51e0\u79cd\uff1a<\/p>\n<p>Ti-1023(Ti-10V-2Fe-3Al)\u949b\u5408\u91d1\u662f\u7531\u7f8e\u56fdTimet\u516c\u53f8\u4e8e1971\u5e74\u7814\u5236\u7684\u3002\u5b83\u662f\u4e00\u79cd\u4e3a\u9002\u5e94\u635f\u4f24\u5bb9\u9650\u6027\u8bbe\u8ba1\u539f\u5219\u800c\u4ea7\u751f\u7684\u9ad8\u7ed3\u6784\u6548\u76ca\u3001\u9ad8\u53ef\u9760\u6027\u548c\u4f4e\u5236\u9020\u6210\u672c\u7684\u953b\u9020\u949b\u5408\u91d1\uff0c\u8be5\u5408\u91d1\u7684Al\u5f53\u91cf\u4e3a4.0\uff0cMo\u5f53\u91cf\u4e3a11.1\uff0c(\u03b1+\u03b2)\/\u03b2\u76f8\u8f6c\u53d8\u6e29\u5ea6\u4e3a790\uff5e805\u2103\uff0c\u5177\u6709\u8f83\u5927\u7684\u6dec\u900f\u6027\u548c\u663e\u8457\u7684\u70ed\u5904\u7406\u5f3a\u5316\u6548\u679c\uff0c\u5177\u6709\u4f18\u5f02\u7684\u953b\u9020\u6027\u80fd\uff0c\u5728760\u2103\u53ef\u8fdb\u884c\u7b49\u6e29\u953b\u9020\uff0c\u63d0\u4f9b\u5404\u79cd\u8fd1\u51c0\u578b\u52a0\u5de5\u953b\u4ef6\u3002\u7ecf\u70ed\u5904\u7406\u540e\uff0c\u8be5\u5408\u91d1\u7684\u03c3<sub>b<\/sub>\u4e3a965\uff5e1310MPa\uff0cK<sub>IC<\/sub>\u4e3a99\uff5e33 MPa\u00b7m<sup>1\/2<\/sup>\u3002\u5df2\u7ecf\u7528\u4e8e\u6ce2\u97f3777\u5ba2\u673a\u8d77\u843d\u67b6\u4e3b\u6881\uff0c\u7a7a\u5ba2A380\u7684\u4e3b\u8d77\u843d\u67b6\u652f\u67f1\u3002<\/p>\n<p>Ti-l5-3 (Ti-15V-3Cr 3Al- 3Sn)\u9ad8\u5f3a\u03b2\u949b\u5408\u91d1\u662f20\u4e16\u7eaa70\u5e74\u4ee3\u7531\u7f8e\u56fd\u7a7a\u519b\u90e8\u95e8\u8d44\u52a9\u4e0b\u5f00\u53d1\u51fa\u6765\u7684\u4e00\u79cd\u8fd1\u03b2\u578b\u7684\u9ad8\u5f3a\u6297\u8150\u8680\u5408\u91d1\u3002\u8be5\u5408\u91d1\u7684Al\u5f53\u91cf\u4e3a5.0\uff0cMo\u5f53\u91cf\u4e3a15.7\uff0c(\u03b1+\u03b2)\/\u03b2\u76f8\u8f6c\u53d8\u6e29\u5ea6\u4e3a750\uff5e770\u2103\uff0c\u5177\u6709\u4f18\u826f\u7684\u51b7\u53d8\u5f62\u6027\u3001\u65f6\u6548\u786c\u5316\u6027\u80fd\u548c\u53ef\u710a\u63a5\u6027\u80fd\u7b49\u7279\u70b9\uff0c\u5176\u51b7\u52a0\u5de5\u6027\u80fd\u6bd4\u5de5\u4e1a\u7eaf\u949b\u8fd8\u597d\uff0c\u53ef\u5728\u56fa\u6eb6\u72b6\u6001\u4e0b\u8fdb\u884c\u5404\u79cd\u590d\u6742\u96f6\u4ef6\u7684\u51b7\u6210\u5f62\uff0c\u6709\u8f83\u5c0f\u7684\u88c2\u7eb9\u654f\u611f\u6027\uff0c\u65f6\u6548\u540e\u7684\u03c3<sub>b<\/sub>\u22651310MPa\uff0c\u8be5\u5408\u91d1\u7279\u522b\u9002\u5b9c\u5236\u9020\u706b\u7bad\u53d1\u52a8\u673a\u63a8\u8fdb\u5242\u8d2e\u7bb1\u548c\u5bfc\u7ba1\u7b49\u90e8\u4ef6\uff0c\u5e76\u4e14\u5df2\u5e94\u7528\u5230\u6ce2\u97f3777\u4e0a\u7684\u5e94\u7528\u63a7\u5236\u7cfb\u7edf\u7ba1\u9053\u548c\u706d\u706b\u7f50\u3002<\/p>\n<p>\u03b2-21S(Ti-15Mo-3Al-2.7Nb-0.2Si)\u5408\u91d1\u662f\u7f8e\u56fdTimet\u516c\u53f8\u4e8e1989\u5e74\u7814\u5236\u7684\u4e00\u79cd\u6297\u6c27\u5316\u3001\u8d85\u9ad8\u5f3a\u949b\u5408\u91d1\u3002\u8be5\u5408\u91d1\u7684Al\u5f53\u91cf\u4e3a4.0\uff0cMo\u5f53\u91cf\u4e3a15.8\uff0c(\u03b1+\u03b2)\/\u03b2\u76f8\u8f6c\u53d8\u6e29\u5ea6\u4e3a793\uff5e810\u2103\uff0c\u5177\u6709\u826f\u597d\u7684\u6297\u6c27\u5316\u6027\u80fd\uff0c\u53ef\u5728540\u2103\u4e0b\u957f\u671f\u5de5\u4f5c\uff1b\u51b7\u3001\u70ed\u52a0\u5de5\u6027\u80fd\u4f18\u826f\u3002\u70ed\u5904\u7406\u540e\uff0c\u03c3<sub>b<\/sub>=1150\uff5e1350MPa\uff0c\u03b4<sub>5<\/sub>=6%\uff5e8%\u3002\u8be5\u5408\u91d1\u9002\u7528\u4e8e\u53d1\u52a8\u673a\u886c\u5957\u548c\u55b7\u7ba1\u7b49\uff0c\u5df2\u7ecf\u88ab\u7f8e\u56fd\u56fd\u5bb6\u5b87\u822a\u5c40(NASA)\u7528\u4f5c\u78b3\u5316\u7845\uff0f\u949b\u590d\u5408\u6750\u6599\u7684\u57fa\u4f53\u6750\u6599\u3002<\/p>\n<p>BT22(Ti-5Al-5Mo-5V-1Fe-1Cr)\u5408\u91d1\u662f\u4fc4\u7f57\u65af\u4e8e20\u4e16\u7eaa70\u5e74\u4ee3\u7814\u5236\u6210\u529f\u7684\u4e00\u79cd\u9ad8\u5f3a\u5ea6\u8fd1\u03b2\u578b\u949b\u5408\u91d1\u3002\u8be5\u5408\u91d1\u7684Al\u5f53\u91cf\u4e3a6.0\uff0cMo\u5f53\u91cf\u4e3a11.8\uff0c(\u03b1+\u03b2)\/\u03b2\u76f8\u8f6c\u53d8\u6e29\u5ea6\u4e3a860\uff5e990\u2103\uff0c\u5177\u6709\u826f\u597d\u7684\u52a0\u5de5\u6027\u80fd\u548c\u710a\u63a5\u6027\u80fd\uff0c\u4e3b\u8981\u7528\u4e8e\u751f\u4ea7\u6a21\u953b\u4ef6\uff0c\u5176\u6dec\u900f\u6df1\u5ea6\u8fbe200mm\uff0c\u5176\u03c3<sub>b<\/sub>\u22651105MPa\u3002\u8be5\u5408\u91d1\u65e2\u53ef\u7528\u4e8e\u5236\u9020\u5728350\uff5e400\u2103\u4e0b\u957f\u671f\u5de5\u4f5c\u7684\u673a\u8eab\u3001\u673a\u7ffc\u53d7\u529b\u4ef6\u53ca\u64cd\u4f5c\u7cfb\u7edf\u7b49\u7684\u7d27\u56fa\u4ef6\uff0c\u4e5f\u53ef\u5236\u9020\u5de5\u4f5c\u6e29\u5ea6\u4f4e\u4e8e350\u2103\u7684\u53d1\u52a8\u673a\u7684\u98ce\u6247\u76d8\u548c\u53f6\u7247\u7b49\u3002\u4e14\u5df2\u7ecf\u7528\u4e8e1L-86\u548c1L-96-300\u7684\u673a\u8eab\u3001\u673a\u7ffc\u3001\u8d77\u843d\u67b6\u548c\u5176\u4ed6\u9ad8\u627f\u8f7d\u90e8\u4ef6\u3002<\/p>\n<p><strong>2<\/strong><strong>\u3001\u9ad8\u6e29\u949b\u5408\u91d1<\/strong><\/p>\n<p>\u9ad8\u6e29\u949b\u5408\u91d1\u662f\u73b0\u4ee3\u822a\u7a7a\u53d1\u52a8\u673a\u7684\u5173\u952e\u6750\u6599\u4e4b\u4e00\uff0c\u9ad8\u6027\u80fd\u822a\u7a7a\u53d1\u52a8\u673a\u7684\u53d1\u5c55\u9700\u6c42\u7275\u5f15\u7740\u9ad8\u6e29\u949b\u5408\u91d1\u7684\u53d1\u5c55\u3002\u9ad8\u6e29\u949b\u5408\u91d1\u4e3b\u8981\u7528\u4f5c\u98de\u673a\u53d1\u52a8\u673a\u7684\u538b\u6c14\u673a\u76d8\u548c\u53f6\u7247\u3001\u673a\u5323\uff0c\u4ee5\u51cf\u8f7b\u53d1\u52a8\u673a\u8d28\u91cf\uff0c\u63d0\u9ad8\u63a8\u91cd\u6bd4\u3002\u53d1\u52a8\u673a\u5bf9\u9ad8\u6e29\u949b\u5408\u91d1\u7684\u8981\u6c42\u975e\u5e38\u82db\u523b\uff0c\u5b83\u8981\u6c42\u6750\u6599\u5177\u6709\u5ba4\u6e29\u6027\u80fd\u3001\u9ad8\u6e29\u5f3a\u5ea6\u3001\u8815\u53d8\u6027\u80fd\u3001\u70ed\u7a33\u5b9a\u6027\u3001\u75b2\u52b3\u6027\u80fd\u548c\u65ad\u88c2\u97e7\u6027\u7684\u826f\u597d\u5339\u914d\u3002<\/p>\n<p>20\u4e16\u7eaa50\u5e74\u4ee3\u6700\u65e9\u7528\u4e8e\u822a\u7a7a\u53d1\u52a8\u673a\u7684Ti-6Al-4V\u5408\u91d1\u670d\u5f79\u6e29\u5ea6\u4e00\u822c\u4e0d\u8d85\u8fc7350\u2103\uff1b\u968f\u540e\u76f8\u7ee7\u7814\u5236\u51fa\u4f7f\u7528\u6e29\u5ea6\u4e3a400\u2103\u5de6\u53f3\u7684IMI550\u3001BT3-l\u7b49\u5408\u91d1\uff1b60\u5e74\u4ee3\uff0c\u5404\u56fd\u5148\u540e\u6210\u529f\u7814\u5236\u4e86\u4f7f\u7528\u6e29\u5ea6\u5728450\u2103~500\u2103\u7684IMI679\u3001IMI685\u3001Ti6246\u3001Ti6242\u7b49\u5408\u91d1\uff1b\u76ee\u524d\uff0c\u4e16\u754c\u8303\u56f4\u5185\u7814\u5236\u51fa\u7684\u6700\u9ad8\u4f7f\u7528\u6e29\u5ea6\u4e3a600\u2103\u7684\u9ad8\u6e29\u949b\u5408\u91d1\u6709\u82f1\u56fd\u7684IM1834\u3001\u7f8e\u56fd\u7684Ti-1100\u3001\u4fc4\u7f57\u65af\u7684BT36\u53ca\u4e2d\u56fd\u7684Ti-60\u3002\u4e0b\u9762\u4e3b\u8981\u4ecb\u7ecd\u51e0\u79cd\u6709\u4ee3\u8868\u6027\u7684\u9ad8\u6e29\u949b\u5408\u91d1\uff1a<\/p>\n<p>IMI834(Ti-5.8Al-4Sn-3.5Zr-0.7Nb-0.5Mo-0.35Si)\u5408\u91d1\u662f\u82f1\u56fd\u4e8e1984\u5e74\u7814\u5236\u7684\u4e00\u79cd\u8fd1\u03b1\u578b\u949b\u5408\u91d1\u3002\u8be5\u5408\u91d1\u7684Al\u5f53\u91cf\u4e3a8.7\uff0cMo\u5f53\u91cf\u4e3a0.7\uff0c(\u03b1+\u03b2)\/\u03b2\u76f8\u8f6c\u53d8\u6e29\u5ea6\u4e3a1045\u00b110\u2103\uff0c\u5177\u6709\u826f\u597d\u7684\u53d8\u5f62\u80fd\u529b\u3002\u7ecf\u70ed\u5904\u7406\u540e\uff0c\u8be5\u5408\u91d1\u7684\u03c3<sub>b<\/sub>\u2265930MPa\u3002\u5df2\u7ecf\u7528\u4e8e\u6ce2\u97f3777\u98de\u673a\u7684\u5927\u578b\u53d1\u52a8\u673aTrent700\u4e0a\u3002<\/p>\n<p>Ti-1100(Ti-6Al-2.75Sn-4Zr-0.4Mo-0.45Si)\u5408\u91d1\u662f\u7f8e\u56fd\u4e8e1988\u5e74\u7814\u5236\u7684\u9ad8\u70ed\u5f3a\u8fd1\u03b1\u578b\u949b\u5408\u91d1\u3002\u8be5\u5408\u91d1\u7684Al\u5f53\u91cf\u4e3a8.6\uff0cMo\u5f53\u91cf\u4e3a0.4\uff0c(\u03b1+\u03b2)\/\u03b2\u76f8\u8f6c\u53d8\u6e29\u5ea6\u4e3a1015\u2103\u3002\u8be5\u5408\u91d1\u5177\u6709\u826f\u597d\u7684\u9ad8\u6e29\u8815\u53d8\u6027\u80fd\u3001\u8f83\u4f4e\u7684\u97e7\u6027\u548c\u8f83\u5927\u7684\u75b2\u52b3\u88c2\u7eb9\u6269\u5c55\u901f\u7387\u3002\u5df2\u7ecf\u7528\u4e8e\u83b1\u5eb7\u660e\u516c\u53f8T55-712\u6539\u578b\u53d1\u52a8\u673a\u7684\u9ad8\u538b\u538b\u6c14\u673a\u8f6e\u76d8\u548c\u4f4e\u538b\u6da1\u8f6e\u53f6\u7247\u7b49\u96f6\u4ef6\u3002<\/p>\n<p>BT36(Ti-6.2A1-2Sn-3.6Zr-0.7Mo-0.1Y-5.0W-0.15Si)\u5408\u91d1\u662f\u4fc4\u7f57\u65af\u4e8e1992\u5e74\u7814\u5236\u7684\u4f7f\u7528\u6e29\u5ea6\u5728600\uff5e650\u2103\u7684\u949b\u5408\u91d1\u3002\u8be5\u5408\u91d1\u7684Al\u5f53\u91cf\u4e3a8.5\uff0cMo\u5f53\u91cf\u4e3a2.7\uff0c(\u03b1+\u03b2)\/\u03b2\u76f8\u8f6c\u53d8\u6e29\u5ea6\u4e3a1000\uff5e1025\u2103\uff0c\u5177\u6709\u826f\u597d\u7684\u9ad8\u6e29\u8815\u53d8\u6027\u80fd\u3002<\/p>\n<p>Ti60(Ti-5.8 Al-4.8 Sn-2.0Zr-1.0 Mo-0.35Si-0.85Nd)\u5408\u91d1\u662f20\u4e16\u7eaa90\u5e74\u4ee3\u672b\u7531\u4e2d\u56fd\u79d1\u5b66\u9662\u91d1\u5c5e\u7814\u7a76\u6240\u5728Ti55\u5408\u91d1\u57fa\u7840\u4e0a\u6539\u578b\u8bbe\u8ba1\u3001\u5b9d\u9e21\u6709\u8272\u91d1\u5c5e\u52a0\u5de5\u5382\u53c2\u4e0e\u7814\u5236\u7684\u4e00\u79cd600\u2103\u9ad8\u6e29\u949b\u5408\u91d1\u3002\u8be5\u5408\u91d1\u7684Al\u5f53\u91cf\u4e3a8.5\uff0cMo\u5f53\u91cf\u4e3a1.0\uff0c(\u03b1+\u03b2)\/\u03b2\u76f8\u8f6c\u53d8\u6e29\u5ea6\u4e3a1025\u2103\uff0c\u5177\u6709\u826f\u597d\u7684\u70ed\u7a33\u5b9a\u6027\u548c\u9ad8\u6e29\u6297\u6c27\u5316\u6027\u3002\u5df2\u7ecf\u8fdb\u884c\u4e86\u534a\u5de5\u4e1a\u6027\u4e2d\u8bd5\u8bd5\u9a8c(\u5305\u62ec\u538b\u6c14\u673a\u76d8\u6a21\u953b)\u548c\u5168\u9762\u6027\u80fd\u6d4b\u5b9a\u3002<\/p>\n<p><strong>3<\/strong><strong>\u3001\u635f\u4f24\u5bb9\u9650\u949b\u5408\u91d1<\/strong><strong>\u00a0\u00a0\u00a0\u00a0\u00a0 <\/strong><\/p>\n<p>\u76ee\u524d\u8f83\u4e3a\u5178\u578b\u7684\u635f\u4f24\u5bb9\u9650\u949b\u5408\u91d1\u6709\u4e24\u79cd\uff0c\u4e00\u79cd\u662f\u56fd\u5916\u7814\u5236\u7684\u9ad8\u5f3a\u9ad8\u97e7\u635f\u4f24\u5bb9\u9650\u949b\u5408\u91d1TC21\uff0c\u4e00\u79cd\u662f\u4e2d\u56fd\u7814\u5236\u7684\u4e2d\u5f3a\u9ad8\u97e7\u635f\u4f24\u5bb9\u9650\u949b\u5408\u91d1TC4-DT\u3002<\/p>\n<p>TC21(Ti-Al-Mo-Sn-Zr-Cr-Si-X) \u5408\u91d1\u662f\u897f\u5317\u6709\u8272\u91d1\u5c5e\u7814\u7a76\u9662\u4e8e2001 \u5e74\u7814\u5236\u7684\u4e00\u79cd\u9ad8\u5f3a\u3001\u9ad8\u97e7\u3001\u635f\u4f24\u5bb9\u9650\u578b\u4e24\u76f8\u949b\u5408\u91d1\uff0c\u662f\u6211\u56fd\u7814\u5236\u7684\u7b2c\u4e00\u4e2a\u5177\u6709\u81ea\u4e3b\u77e5\u8bc6\u4ea7\u6743\u7684\u9ad8\u5f3a\u635f\u4f24\u5bb9\u9650\u578b\u949b\u5408\u91d1\uff0c\u5317\u4eac\u822a\u7a7a\u6750\u6599\u7814\u7a76\u9662\u4e3a\u8be5\u5408\u91d1\u7684\u5e94\u7528\u7814\u7a76\u5355\u4f4d\u3002\u8be5\u5408\u91d1\u4e00\u822c\u4f7f\u7528\u72b6\u6001\u7684\u7ec4\u7ec7\u4e3a\u7f51\u7bee\u72b6\u6216\u4e09\u6001\u7ec4\u7ec7\uff0c\u5177\u6709\u4f18\u826f\u7684\u5f3a\u5ea6\u3001\u5851\u6027\u3001\u97e7\u6027\u548c\u4f4e\u7684\u88c2\u7eb9\u6269\u5c55\u901f\u7387\u5339\u914d\uff0c\u5176\u5178\u578b\u529b\u5b66\u6027\u80fd\u4e3a\u03c3<sub>b<\/sub>\uff1a1100MPa\uff0c\u03c3<sub>0.2<\/sub>\uff1a1000MPa\uff0c\u03b4\uff1a8%\uff0c\u03c8\uff1a15%\uff0cE\uff1a115 GPa\uff0cK<sub>IC<\/sub>\uff1a70 MPa\u00b7m<sup>1\/2<\/sup>\uff0cda\/dN\uff1a8\u00d710<sup>-5<\/sup> ~9\u00d710<sup>-5<\/sup> mm\/cycle\u3002\u4e0e\u5728\u7f8e\u56fdF-22\u98de\u673a\u5f97\u5230\u5e94\u7528\u7684Ti-6-22-22S(\u7f8e\u56fd)\u548c\u82cf-27\u7cfb\u5217\u98de\u673a\u5e7f\u6cdb\u5e94\u7528\u7684BT20(\u4fc4\u7f57\u65af)\u949b\u5408\u91d1\u76f8\u6bd4\uff0c\u5176\u7efc\u5408\u529b\u5b66\u6027\u80fd\u66f4\u52a0\u4f18\u5f02\uff0c\u7279\u522b\u662f\u5176\u5177\u6709\u975e\u5e38\u4f18\u5f02\u7684\u7535\u5b50\u675f\u710a\u63a5\u6027\u80fd\uff0c\u9002\u5408\u5236\u9020\u5927\u578b\u6574\u4f53\u6846\u3001\u53d1\u52a8\u673a\u9644\u8fd1\u6302\u67b6\u3001\u6881\u3001\u63a5\u5934\u3001\u8d77\u843d\u67b6\u90e8\u4ef6\u7b49\u91cd\u8981\u627f\u529b\u6784\u4ef6\u3002<\/p>\n<p>TC4-DT\u5408\u91d1\u662f\u5728\u7f8e\u56fd\u7684Ti-6Al-4VELI\u5408\u91d1\u57fa\u7840\u4e0a\u7531\u897f\u5317\u6709\u8272\u9662\u548c\u5317\u4eac\u822a\u7a7a\u6750\u6599\u7814\u7a76\u9662\u8054\u5408\u7814\u5236\u7684\u4e2d\u5f3a\u3001\u9ad8\u97e7\u3001\u635f\u4f24\u5bb9\u9650\u578b\u3001\u53ef\u710a\u949b\u5408\u91d1\uff0c\u5176\u6027\u80fd\u4e0eTi-6Al-4VELI\u76f8\u5f53\u3002\u4f46\u662fTC4-DT\u7684\u5408\u91d1\u6210\u5206\u8303\u56f4\u6bd4Ti-6AI-4VELI\u63a7\u5236\u66f4\u4e25\u683c\uff0c\u5177\u4f53\u4e3aAl\uff1a6.0-6. 35\uff0cV\uff1a3.6 -4.4\uff0cFe\u22640.25\uff0cC\u22640.05\uff0cO\u22640.13\uff0cN\u22640. 03\uff0cH\u22640.0125\uff0cTi\u4f59\u91cf\u3002\u8be5\u5408\u91d1\u5177\u6709\u4e2d\u7b49\u5f3a\u5ea6\u3001\u9ad8\u65ad\u88c2\u97e7\u5ea6\u548c\u9ad8\u635f\u4f24\u5bb9\u9650\u7b49\u7efc\u5408\u6027\u80fd\u5339\u914d\u7684\u7279\u70b9\uff0c\u5176\u5178\u578b\u529b\u5b66\u6027\u80fd\u4e3a\uff0c\u03c3<sub>b<\/sub>\uff1a895MPa\uff0c\u03c3<sub>0.2<\/sub>\uff1a795MPa\uff0c\u03b4\uff1a8%\uff0c\u03c8\uff1a15%\uff0cK<sub>IC<\/sub>\uff1a75MPa\u00b7m<sup>1\/2<\/sup>\uff0cda\/dN\uff1a9\u00d710<sup>-6<\/sup> mm\/cycle\u3002\u8be5\u5408\u91d1\u7279\u522b\u9002\u5408\u5236\u9020\u98de\u673a\u5927\u578b\u6574\u4f53\u6846\u3001\u6881\u3001\u63a5\u5934\u7b49\u5173\u952e\u627f\u529b\u6784\u4ef6\uff0c\u5df2\u7ecf\u5e94\u7528\u4e8e\u6ce2\u97f3777\u5ba2\u673a\u7684\u5b89\u5b9a\u9762\u8fde\u63a5\u63a5\u5934\u548cF\/A-22\u98de\u673a\u7684\u673a\u4f53\u3002<\/p>\n<p><strong>4<\/strong><strong>\u3001\u963b\u71c3\u949b\u5408\u91d1<\/strong><\/p>\n<p>\u4f5c\u4e3a\u822a\u7a7a\u53d1\u52a8\u673a\u6750\u6599\u4f7f\u7528\u65f6\uff0c\u666e\u901a\u949b\u5408\u91d1\u53ef\u80fd\u4f1a\u4ea7\u751f\u201c\u949b\u706b\u201d\uff0c\u4e3a\u4e86\u89e3\u51b3\u8fd9\u4e2a\u95ee\u9898\uff0c\u5404\u56fd\u5f00\u5c55\u4e86\u5bf9\u963b\u71c3\u949b\u5408\u91d1\u7684\u7814\u5236\u3002\u4e0b\u9762\u4e3b\u8981\u4ecb\u7ecd\u51e0\u79cd\u6709\u4ee3\u8868\u6027\u7684\u963b\u71c3\u949b\u5408\u91d1\uff1a<\/p>\n<p>Alloy C(Ti-35V-15Cr)\u5408\u91d1\u662f\u7f8e\u56fdP&amp;W\u516c\u53f8\u4e8e20\u4e16\u7eaa80\u5e74\u4ee3\u7814\u5236\u7684\u4e00\u79cd\u03b2\u578b\u949b\u5408\u91d1\u3002\u8be5\u5408\u91d1\u7684\u94bc\u5f53\u91cf\u4e3a47.5\uff0c\u662f\u76ee\u524d\u5de5\u4e1a\u7528\u03b2\u949b\u5408\u91d1\u94bc\u5f53\u91cf\u6700\u9ad8\u7684\u5408\u91d1\uff0c\u5177\u6709\u826f\u597d\u7684\u5ba4\u6e29\u548c\u9ad8\u6e29\u5851\u6027\u3001\u8815\u53d8\u548c\u75b2\u52b3\u6027\u80fd\uff0c\u53ef\u5236\u6210\u677f\u6750\u3001\u5e26\u6750\u3001\u68d2\u6750\u4ee5\u53ca\u953b\u4ef6\u7b49\u3002\u8be5\u5408\u91d1\u5df2\u7ecf\u5e94\u7528\u4e8eF119\u53d1\u52a8\u673a\uff08F\/A-22\u6218\u6597\u673a\u7684\u52a8\u529b\u88c5\u7f6e\uff09\u7684\u9ad8\u538b\u538b\u6c14\u673a\u673a\u5323\u3001\u5bfc\u5411\u53f6\u7247\u548c\u77e2\u91cf\u5c3e\u55b7\u7ba1\uff0c\u5e76\u4e8e1993\u5e741\u6708\u6210\u529f\u5730\u8fdb\u884c\u4e86\u98de\u884c\u5b9e\u9a8c\u3002<\/p>\n<p>BTT-1\u548cBTT-3\u4e3a\u4fc4\u7f57\u65af\u4ece\u6469\u64e6\u673a\u5236\u5165\u624b\u7814\u5236\u7684\u963b\u71c3\u949b\u5408\u91d1\uff0c\u5747\u4e3aTi-Cu-Al\u7cfb\u5408\u91d1\uff08\u6dfb\u52a0Mo\u3001V\u3001Zr\uff09\u3002<\/p>\n<p>BTT-l\u5177\u6709\u826f\u597d\u7684\u70ed\u52a0\u5de5\u6027\u80fd\uff0c\u53ef\u5236\u6210\u5f62\u72b6\u590d\u6742\u7684\u53d1\u52a8\u673a\u96f6\u4ef6\uff0c\u5982\u538b\u6c14\u673a\u673a\u5323\u548c\u53f6\u7247\uff0c\u5de5\u4f5c\u6e29\u5ea6\u53ef\u8fbe450\u2103\u3002<\/p>\n<p>BTT-3\u5408\u91d1\u7684\u5de5\u827a\u5851\u6027\u6bd4BTT-l\u5408\u91d1\u66f4\u597d\uff0c\u7279\u522b\u9002\u5408\u4e8e\u5236\u9020\u5404\u79cd\u677f\u6750\u548c\u7b94\u6750\u96f6\u4ef6\u3002BTT-3\u7684\u963b\u71c3\u80fd\u529b\u4e5f\u9ad8\u4e8eBTT-l\uff0c\u5728\u76f8\u540c\u7684\u8bd5\u9a8c\u6761\u4ef6\u4e0b\uff0cTi-6Al-4V\u7684\u6469\u64e6\u7740\u706b\u6e29\u5ea6\u4e3a100\u2103\uff0cBTT-l\u4e3a650\u2103\uff0cBTT-3\u5219\u5927\u4e8e800\u2103\u3002<\/p>\n<p><span style=\"color: #0000ff;\"><strong>\u4e09\u3001\u7ed3\u8bba\u4e0e\u5c55\u671b<\/strong><\/span><\/p>\n<p>\u6211\u56fd\u949b\u6750\u4ea7\u91cf\u4f4d\u5c45\u4e16\u754c\u7b2c\u56db\uff0c\u4f46\u822a\u7a7a\u822a\u5929\u7528\u9ad8\u7aef\u949b\u6750\u4ea7\u91cf\u53ea\u5360\u603b\u91cf\u768410\uff05\u5de6\u53f3\uff0c\u4e0e\u4e16\u754c\u768450\uff05\u6c34\u5e73\u4ecd\u5b58\u5728\u7740\u76f8\u5f53\u7684\u5dee\u8ddd\uff0c\u56e0\u6b64\u9700\u8981\u52a0\u5f3a\u7efc\u5408\u9ad8\u6027\u80fd\u949b\u5408\u91d1\u6750\u6599\u548c\u5e94\u7528\u7684\u521b\u65b0\u6027\u7814\u7a76\uff0c\u63d0\u9ad8\u822a\u7a7a\u822a\u5929\u949b\u5408\u91d1\u7684\u5e94\u7528\u6c34\u5e73\u548c\u7528\u91cf\u3002\u53d1\u5c55\u9ad8\u7efc\u5408\u6027\u80fd\u949b\u5408\u91d1\u6750\u6599\u4e0e\u4f4e\u6210\u672c\u5236\u9020\u6280\u672f\u662f\u6269\u5927\u949b\u5408\u91d1\u5e94\u7528\u7684\u4e24\u5927\u9a71\u52a8\u529b\u3002\u91c7\u7528\u5148\u8fdb\u7684\u5236\u9020\u6280\u672f\uff08\u5982\u6fc0\u5149\u8fd1\u51c0\u6210\u5f62\uff09\uff0c\u7528\u4ef7\u683c\u8f83\u4f4e\u7684\u5408\u91d1\u5143\u7d20\u53d6\u4ee3\u8d35\u7684\u91d1\u5c5e\u5143\u7d20\u964d\u4f4e\u949b\u5408\u91d1\u6210\u672c\uff0c\u5728\u63d0\u9ad8\u949b\u5408\u91d1\u6784\u4ef6\u7684\u6027\u80fd\u7684\u540c\u65f6\uff0c\u4fc3\u8fdb\u949b\u5408\u91d1\u5728\u822a\u7a7a\u822a\u5929\u9886\u57df\u7684\u5e94\u7528\u6c34\u5e73\u548c\u7528\u91cf\uff1b\u7cbe\u7b80\u949b\u5408\u91d1\u724c\u53f7\uff0c\u4f18\u5316\u949b\u5408\u91d1\u6027\u80fd\uff0c\u8981\u4e00\u6750\u591a\u7528\uff0c\u5f62\u6210\u9aa8\u5e72\u949b\u5408\u91d1\u4f53\u7cfb\uff0c\u662f\u672a\u6765\u949b\u5408\u91d1\u5728\u822a\u7a7a\u9886\u57df\u7684\u4e3b\u8981\u53d1\u5c55\u65b9\u5411\u3002<\/p>\n<p><strong>\u53c2\u8003\u6587\u732e<\/strong><\/p>\n<p><span style=\"line-height: 1.5;\">[1] \u6731\u77e5\u5bff. \u822a\u7a7a\u7ed3\u6784\u7528\u65b0\u578b\u9ad8\u6027\u80fd\u949b\u5408\u91d1\u6750\u6599\u6280\u672f\u7814\u7a76\u4e0e\u53d1\u5c55[J]. \u822a\u7a7a\u79d1\u5b66\u6280\u672f, 2012(01):5-9.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[2] \u4ed8\u8273\u8273, \u5b8b\u6708\u6e05, \u60e0\u677e\u9a81,\u7b49. \u822a\u7a7a\u7528\u949b\u5408\u91d1\u7684\u7814\u7a76\u4e0e\u5e94\u7528\u8fdb\u5c55[J]. \u7a00\u6709\u91d1\u5c5e, 2006, 30(6):850-856.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[3] \u8d75\u6c38\u5e86, \u845b\u9e4f. \u6211\u56fd\u81ea\u4e3b\u7814\u53d1\u949b\u5408\u91d1\u73b0\u72b6\u4e0e\u8fdb\u5c55[J]. \u822a\u7a7a\u6750\u6599\u5b66\u62a5, 2014, 34(04):51-61.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[4] \u6bdb\u5c0f\u5357, \u8d75\u6c38\u5e86, \u6768\u51a0\u519b. \u56fd\u5916\u822a\u7a7a\u53d1\u52a8\u673a\u7528\u949b\u5408\u91d1\u7684\u53d1\u5c55\u73b0\u72b6[J]. \u4e2d\u56fd\u6750\u6599\u8fdb\u5c55, 2007, 26(5):1-7.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[5] \u94b1\u4e5d\u7ea2. \u822a\u7a7a\u822a\u5929\u7528\u65b0\u578b\u949b\u5408\u91d1\u7684\u7814\u7a76\u53d1\u5c55\u53ca\u5e94\u7528[J]. \u7a00\u6709\u91d1\u5c5e, 2000, 24(3):218-223.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[6] \u6731\u77e5\u5bff, \u738b\u65b0\u5357, \u7ae5\u8def,\u7b49. \u822a\u7a7a\u7528\u635f\u4f24\u5bb9\u9650\u578b\u949b\u5408\u91d1\u7814\u7a76\u4e0e\u5e94\u7528[J]. \u4e2d\u56fd\u6750\u6599\u8fdb\u5c55, 2010, 29(5):14-17.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[7] \u66f9\u6625\u6653. \u822a\u7a7a\u7528\u949b\u5408\u91d1\u7684\u53d1\u5c55\u6982\u51b5[J]. \u822a\u7a7a\u79d1\u5b66\u6280\u672f, 2005(04):3-6.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[8] \u674e\u660e\u6021. \u822a\u7a7a\u7528\u949b\u5408\u91d1\u7ed3\u6784\u6750\u6599[J]. \u4e16\u754c\u6709\u8272\u91d1\u5c5e, 2000(06):17-20.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[9] \u5f20\u5229\u519b, \u859b\u7965\u4e49, \u5e38\u8f89,\u7b49. \u6211\u56fd\u822a\u7a7a\u822a\u5929\u7528\u949b\u5408\u91d1\u6750\u6599[C]\/\/ \u7a7a\u95f4\u6750\u6599\u53ca\u5176\u5e94\u7528\u6280\u672f\u5b66\u672f\u4ea4\u6d41\u4f1a. 2011.<\/span><\/p>\n<p><span style=\"line-height: 1.5;\">[10] \u8d75\u6c38\u5e86, \u845b\u9e4f. \u6211\u56fd\u81ea\u4e3b\u7814\u53d1\u949b\u5408\u91d1\u73b0\u72b6\u4e0e\u8fdb\u5c55[J]. \u822a\u7a7a\u6750\u6599\u5b66\u62a5, 2014, 34(04):51-61.<\/span><\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u91d1\u5c5e\u6750\u6599\u5b66\u672f\u7ec4Sweet\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002\u6b22\u8fce\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u91d1\u5c5e\u6750\u6599\u5b66\u672f\u4ea4\u6d41\u7fa4\uff08458281221\uff09\uff01<\/p>\n<p>\u5b66\u672f\u5e72\u8d27\u81f4\u529b\u4e8e\u6210\u4e3a\u5e7f\u5927\u6750\u6599\u4eba\u8bfb\u8005\u9ad8\u6548\u83b7\u53d6\u77e5\u8bc6\u7684\u9014\u5f84\uff0c\u4e3a\u4e86\u66f4\u8d34\u5408\u5927\u4f17\u77e5\u8bc6\u9700\u6c42\uff0c\u73b0\u5411\u5927\u5bb6\u5f81\u96c6\u5e72\u8d27\u5199\u4f5c\u65b9\u5411\u3002\u5982\u679c\u4f60\u60f3\u4e86\u89e3\u54ea\u4e2a\u9886\u57df\u7684\u77e5\u8bc6\uff0c\u67d0\u4e2a\u8f6f\u4ef6\u7684\u5e94\u7528\u6216\u8005\u4efb\u4f55\u6709\u8da3\u7684\u60f3\u6cd5\u548c\u601d\u7ef4\u65b9\u5411\uff0c\u8bf7\u5728\u5fae\u4fe1\u4e0b\u65b9\u7559\u8a00\u677f\u7559\u8a00\uff0c\u6211\u4eec\u4f1a\u6536\u96c6\u5e76\u63a8\u51fa\u5927\u5bb6\u9700\u6c42\u7684\u5b66\u672f\u5e72\u8d27\uff0c\u6709\u5efa\u8bbe\u6027\u7684\u610f\u89c1\u6216\u8005\u60f3\u6cd5\u4e00\u7ecf\u91c7\u7eb3\uff0c\u6211\u4eec\u5c06\u63d0\u4f9b\u795e\u79d8\u5956\u52b1\u3002\u5feb\u5feb\u7559\u8a00\u5427\uff01\uff01<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u5411\u5404\u5927\u56e2\u961f\u8bda\u5fc3\u7ea6\u7a3f\uff0c\u8bfe\u9898\u7ec4\u6700\u65b0\u6210\u679c\u3001\u65b9\u5411\u603b\u7ed3\u3001\u56e2\u961f\u8bbf\u8c08\u3001\u5b9e\u9a8c\u6280\u80fd\u7b49\u7686\u53ef\u6295\u7a3f\uff0c\u8bf7\u8054\u7cfb\uff1a\u90ae\u7bb1tougao@cailiaoren.com \u6216 QQ\uff1a97482208\u3002<\/p>\n<p>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u627e<a href=\"http:\/\/mai.cailiaoren.com\/\" target=\"_blank\" rel=\"noopener\">\u6750\u6599\u4eba<\/a>\uff0c<strong>\u4e0a<\/strong><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\"><strong>\u6d4b\u8bd5\u8c37<\/strong><\/a><strong>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5f15\u8a00\uff1a\u949b\u5408\u91d1\u7531\u4e8e\u5176\u6bd4\u5f3a\u5ea6\u9ad8\u3001\u8010\u8150\u8680\u6027\u597d\u7b49\u4f18\u70b9\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u822a\u7a7a\u822a\u5929\u9886\u57df\u3002\u672c\u6587\u4ecb\u7ecd\u4e86\u8fd1\u5e74\u6765\u4e3b\u8981\u949b\u5408\u91d1\u7684\u7814\u7a76\u8fdb\u5c55\uff0c\u5305\u62ec\u9ad8\u5f3a\u9ad8\u97e7\u578b\u949b\u5408\u91d1\uff08Ti-1023\u3001Ti-15-3&#8230;<\/p>\n","protected":false},"author":2925,"featured_media":102312,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[689,63,1566],"class_list":["post-102309","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-ganhuo","tag-xueshu","tag-aircraft","tag-1566"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/102309"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2925"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=102309"}],"version-history":[{"count":6,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/102309\/revisions"}],"predecessor-version":[{"id":102470,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/102309\/revisions\/102470"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/102312"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=102309"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=102309"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=102309"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}