{"id":106807,"date":"2017-10-18T06:30:45","date_gmt":"2017-10-17T22:30:45","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=106807"},"modified":"2017-10-15T20:42:39","modified_gmt":"2017-10-15T12:42:39","slug":"adv-energy-mater%ef%bc%9a%e5%8f%af%e4%ba%a7%e4%b8%9a%e5%8c%96%e3%80%81%e7%a9%ba%e6%b0%94%e7%a8%b3%e5%ae%9a%e7%9a%84o3%e5%9e%8b%e5%b1%82%e7%8a%b6%e6%b0%a7%e5%8c%96%e7%89%a9%e6%ad%a3%e6%9e%81%e6%88%90","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=106807","title":{"rendered":"Adv. Energy. Mater\uff1a\u53ef\u4ea7\u4e1a\u5316\u3001\u7a7a\u6c14\u7a33\u5b9a\u7684O3\u578b\u5c42\u72b6\u6c27\u5316\u7269\u6b63\u6781\u6210\u5c31\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u94a0\u7535"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u94a0\u79bb\u5b50\u7535\u6c60\u7531\u4e8e\u8d44\u6e90\u4e30\u5bcc\u3001\u8d85\u9ad8\u7684\u5b89\u5168\u6027\u7b49\u7279\u70b9\u4ee5\u53ca\u4e0e\u9502\u7535\u7c7b\u4f3c\u7684\u5316\u5b66\u7279\u6027\uff0c\u88ab\u8ba4\u4e3a\u662f\u6700\u5177\u6f5c\u529b\u7684\u66ff\u4ee3\u9502\u79bb\u5b50\u7535\u6c60\u7684\u80fd\u91cf\u5b58\u50a8\u7cfb\u7edf\u4e4b\u4e00\u3002\u76ee\u524d\u5df2\u6709\u8bb8\u591a\u5b66\u672f\u7814\u7a76\u63a2\u7d22\u9ad8\u6027\u80fd\u7684\u94a0\u79bb\u5b50\u7535\u6c60\u6b63\u6781\u6750\u6599\uff0c\u7136\u800c\u5728\u5b9e\u9645\u5e94\u7528\u4e2d\u8fd9\u4e9b\u6b63\u6781\u6750\u6599\u521d\u59cb\u5e93\u4f26\u6548\u7387\u4f4e\u3001\u53ef\u5faa\u73af\u94a0\u542b\u91cf\u4e0d\u8db3\u3001\u5de5\u4e1a\u53ef\u884c\u6027\u5dee\u7b49\u7f3a\u9677\u963b\u788d\u4e86\u94a0\u79bb\u5b50\u7535\u6c60\u5546\u4e1a\u5316\u5e94\u7528\u7684\u53d1\u5c55\u3002\u56e0\u6b64\uff0c\u4e3a\u5b9e\u73b0\u94a0\u79bb\u5b50\u7684\u5b9e\u9645\u5546\u4e1a\u5316\u5e94\u7528\uff0c\u4e9f\u9700\u53d1\u5c55\u89c4\u907f\u4e0a\u8ff0\u7f3a\u9677\u7684\u9ad8\u6027\u80fd\u94a0\u79bb\u5b50\u6b63\u6781\u6750\u6599\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u6fb3\u5927\u5229\u4e9a\u4f0d\u4f26\u8d21\u5927\u5b66\u7684\u7aa6\u4e16\u5b66\u6559\u6388\u3001\u9a86\u6587\u5f6c\u535a\u58eb\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u4ee5\u53ca\u6842\u6797\u7535\u5b50\u79d1\u6280\u5927\u5b66\u9093\u5efa\u79cb\u6559\u6388<\/strong>\u5728<strong>Adv. Energy. Mater<\/strong>\u4e0a\u53d1\u8868\u6700\u65b0\u7814\u7a76\u6210\u679c \u201c<strong>High Energy Density Sodium-Ion Battery with Industrially Feasible and Air-Stable O3-Type Layered Oxide Cathode<\/strong>\u201d\u3002\u5728\u8be5\u6587\u4e2d\uff0c\u7814\u7a76\u8005\u901a\u8fc7\u6210\u719f\u53ef\u5de5\u4e1a\u5316\u7684\u5171\u6c89\u79ef\u6280\u672f\u4e0e\u540e\u7eed\u7684\u9ad8\u6e29\u70e7\u7ed3\u8fc7\u7a0b\u5927\u89c4\u6a21\u5236\u5907\u5f97\u5230O<sub>3<\/sub>\u578bNa[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u5c42\u72b6\u6b63\u6781\u6750\u6599\uff0c\u8be5\u65b0\u578b\u6b63\u6781\u6750\u6599\u53ef\u5728\u7a7a\u6c14\u4e2d\u4fdd\u6301\u7a33\u5b9a\u3002\u6b64\u6b63\u6781\u6750\u6599\u4e2d\u7531\u8bb8\u591a\u4e00\u7ea7\u7eb3\u7c73\u6676\u6784\u6210\u7684\u5fae\u7c73\u4e8c\u7ea7\u7c92\u5b50\u5177\u6709\u8f83\u77ed\u7684\u6269\u6563\u8ddd\u79bb\uff0c\u53ef\u6709\u6548\u5730\u4fc3\u8fdb\u94a0\u79bb\u5b50\u7684\u4f20\u8f93\u3002\u8be5\u6b63\u6781\u6750\u6599\u57280.1 C\u65f6\u53ef\u9006\u5bb9\u91cf\u9ad8\u8fbe172 mA h g<sup>-1<\/sup>\uff0c20 C\u65f61000\u6b21\u5faa\u73af\u540e\u5bb9\u91cf\u4fdd\u6301\u7387\u53ef\u9ad8\u8fbe70.4 %\u3002\u9664\u6b64\u4e4b\u5916\uff0c\u8be5\u6b63\u6781\u6750\u6599\u4e0e\u786c\u78b3\u8d1f\u6781\u6709\u8f83\u597d\u7684\u517c\u5bb9\u6027\uff0c\u4e24\u8005\u6784\u7b51\u7684\u5168\u7535\u6c60\u7684\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9ad8\uff080.1 C\u65f6\uff0c215 Wh kg<sup>-1<\/sup>\uff09\u4e14\u500d\u7387\u7279\u6027\u597d\u3002\u8be5\u6b63\u6781\u6750\u6599\u4e0e\u8d1f\u6781\u517c\u5bb9\u6027\u597d\u3001\u7535\u5316\u5b66\u6027\u80fd\u4f18\u5f02\u3001\u5236\u5907\u5de5\u827a\u53ef\u4ea7\u4e1a\u5316\uff0c\u5176\u5c06\u63a8\u8fdb\u94a0\u79bb\u5b50\u7535\u6c60\u5546\u4e1a\u5316\u7684\u53d1\u5c55\u811a\u6b65\uff0c\u5177\u6709\u8f83\u597d\u7684\u5e94\u7528\u524d\u666f\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe1 \u5171\u6c89\u79ef\u7cfb\u7edf\u88c5\u7f6e\u56fe\u4e0e\u6b63\u6781\u6750\u6599\u5f62\u8c8c\u53ca\u7ed3\u6784\u8868\u5f81\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-106814\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0001.jpg\" alt=\"\" width=\"600\" height=\"579\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0001.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0001-300x290.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff0910 L\u7684\u5171\u6c89\u79ef\u7cfb\u7edf\u7684\u5149\u5b66\u7167\u7247\uff1b<\/p>\n<p>\uff08b\uff09Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u6b63\u6781\u6750\u6599SEM\u56fe\u7247\uff1b<\/p>\n<p>\uff08c\uff09Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u7eb3\u7c73\u7247\u539f\u59cb\u72b6\u6001\u4e0b\u7684STEM\u56fe\u7247\uff1b<\/p>\n<p>\uff08d\uff09Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u7eb3\u7c73\u7247\u7535\u5b50\u884d\u5c04\u56fe\u6837\uff1b<\/p>\n<p>\uff08e-i\uff09Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u539f\u59cb\u6676\u4f53\u7684\u5143\u7d20\u5206\u5e03\u56fe\uff1b<\/p>\n<p>\uff08j\uff09XRD \uff08\u63d2\u56fe\u4e3a\u5206\u5b50\u7ed3\u6784\u6a21\u578b\uff09\uff1b<\/p>\n<p>\uff08k-n\uff09\u76f8\u5e94\u5143\u7d20\u7684EELS\u4fe1\u53f7\u56fe\uff1b<\/p>\n<p>\uff08o-q\uff09Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u7eb3\u7c73\u7247\u6a2a\u622a\u9762HAADF-STEM\u56fe\u3002<\/p>\n<p><strong>\u56fe2 Na\/\/Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u7535\u5316\u5b66\u6027\u80fd\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-106815\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0002.jpg\" alt=\"\" width=\"600\" height=\"967\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0002.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0002-186x300.jpg 186w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff090.1 mV s<sup>-1<\/sup>\u626b\u901f\u4e0b\u524d\u4e94\u6b21\u5faa\u73af\u7684\u5faa\u73af\u4f0f\u5b89\u66f2\u7ebf\u56fe\uff1b<\/p>\n<p>\uff08b\uff09Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u7535\u6781\u7b2c\u4e8c\u6b21\u5faa\u73af\u7684\u5145\u653e\u7535\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08c\uff0cd\uff090.5 C\u548c1 C\u500d\u7387\u4e0b\u5145\u653e\u7535\u66f2\u7ebf;<\/p>\n<p>\uff08e\uff090.1 C\u30010.5 C\u30011 C\u500d\u7387\u4e0b\u7684\u5faa\u73af\u6027\u80fd;<\/p>\n<p>\uff08f\uff091~50 C\u500d\u7387\u4e0b\u7684\u500d\u7387\u7279\u6027\u56fe\uff1b<\/p>\n<p>\uff08g\uff095 C\u300120 C\u300150 C\u500d\u7387\u4e0b\u7684\u5faa\u73af\u6027\u80fd\u3002<\/p>\n<p><strong>\u56fe3 Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u4e2dNa<sup>+<\/sup>\u7535\u5316\u5b66\u52a8\u529b\u5b66\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-106816\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0003.jpg\" alt=\"\" width=\"600\" height=\"443\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0003.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0003-300x222.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u6b63\u6781\u6750\u6599\u7684\u9996\u6b21\u5faa\u73af\u6052\u7535\u6d41\u95f4\u6b47\u6ef4\u5b9a\uff08GITT\uff09\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08b\uff09\u6ef4\u5b9a\u65f6\uff0c\u7535\u6c60\u7535\u538b\u4e0e\u03c4<sup>1\/2<\/sup>\u7684\u7ebf\u6027\u5173\u7cfb\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08c\uff09\u6839\u636eGITT\u8ba1\u7b97Na<sup>+<\/sup>\u6269\u6563\u7387\u4e0e\u5145\u653e\u7535\u72b6\u6001\u7684\u5173\u7cfb\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08d\uff09\u6839\u636eEIS\u8ba1\u7b97\u4e0d\u540c\u7535\u538b\u4e0b\u7684Na<sup>+<\/sup>\u6269\u6563\u7387\u3002<\/p>\n<p><strong>\u56fe4 HAADF-STEM-EELS\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-106817\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0004.jpg\" alt=\"\" width=\"600\" height=\"618\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0004.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0004-291x300.jpg 291w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff091 C\u500d\u7387\u4e0b400\u6b21\u5faa\u73af\u6d3b\u6027\u6750\u6599\u7684HAADF-STEM-EELS\u56fe\u7247\uff1b<\/p>\n<p>\uff08b-d\uff09a\u56fe\u4e2d\u76f8\u5e94\u533a\u57df\u7684EELS\u4fe1\u53f7\u66f2\u7ebf\u56fe \uff1b<\/p>\n<p>\uff08e-g\uff09a\u56fe\u4e2de\u3001f\u3001g\u4f4d\u7f6e\u5904\u7684HAADF-STEM\u56fe\uff1b<\/p>\n<p>\uff08e1-g1\uff09a\u56fe\u4e2de\u3001f\u3001g\u4f4d\u7f6e\u5904\u7684FFT\u56fe\u4e0e\u63a8\u6d4b\u7684\u7ed3\u6784\u56fe\uff08\u63d2\u56fe\uff09\u3002<\/p>\n<p><strong>\u56fe5 \u5168\u7535\u6c60\u7535\u5316\u5b66\u6027\u80fd\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-106818\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0005.jpg\" alt=\"\" width=\"600\" height=\"442\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0005.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/aenm201701610-fig-0005-300x221.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u5145\u653e\u7535\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08b\uff09\u4ee5Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u4e3a\u6b63\u6781\u3001\u539f\u59cb\u786c\u78b3\u4e3a\u8d1f\u6781\u7684\u5168\u7535\u6c60\u57280.5 C\u65f6\u7684\u5faa\u73af\u6027\u80fd\uff1b<\/p>\n<p>\uff08c\uff09\u8be5\u5168\u7535\u6c60\u4e0e\u5176\u4ed6\u62a5\u9053\u4e2d\u7684\u94a0\u79bb\u5b50\u7535\u6c60\u5168\u7535\u6c60\u80fd\u91cf\u5bc6\u5ea6\u7684\u5bf9\u6bd4\u56fe\uff1b<\/p>\n<p>\uff08d\uff09\u94a0\u79bb\u5b50\u8f6f\u5305\u7535\u6c60\u70b9\u4eaeLED\u706f\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><br \/>\n \u5728\u8fd9\u9879\u5de5\u4f5c\u4e2d\uff0c\u7814\u7a76\u8005\u5229\u7528\u5171\u6c89\u79ef\u6280\u672f\u5927\u89c4\u6a21\u5236\u5907\u65b0\u578b\u7a7a\u6c14\u7a33\u5b9a\u7684O3\u578bNa[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u6b63\u6781\u6750\u6599\uff0c\u8be5\u6b63\u6781\u6750\u6599\u4e8c\u7ea7\u5fae\u578b\u9897\u7c92\u7531\u4e00\u7ea7\u7eb3\u7c73\u7247\u6676\u4f53\u805a\u96c6\u800c\u6210\uff0c\u7ef4\u6301\u4e86\u524d\u9a71\u4f53\u7684\u5fae\u7403\u7ed3\u6784\u3002\u7531\u4e8e\u6269\u6563\u8ddd\u79bb\u7f29\u77ed\u7684\u7279\u6027\uff0c\u8be5\u6b63\u6781\u6750\u6599\u80fd\u591f\u6709\u6548\u5730\u4fc3\u8fdb\u94a0\u79bb\u5b50\u7684\u4f20\u8f93\u5e76\u5229\u4e8e\u9ad8\u632f\u5b9e\u5bc6\u5ea6\u7684\u7269\u8d28\u4f20\u8f93\uff0c\u56e0\u800c\u4f53\u79ef\u80fd\u91cf\u5bc6\u5ea6\u8f83\u9ad8\u3002\u6b64\u6750\u6599\u7684\u534a\u7535\u6c60\u4e0e\u786c\u78b3\/\/ Na[Li<sub>0.05<\/sub>Mn<sub>0.50<\/sub>Ni<sub>0.30<\/sub>Cu<sub>0.10<\/sub>Mg<sub>0.05<\/sub>]O<sub>2<\/sub>\u5168\u7535\u6c60\u5177\u6709\u9ad8\u5bb9\u91cf\u3001\u9ad8\u500d\u7387\u7279\u6027\u3001\u7a33\u5b9a\u5faa\u73af\u6027\u80fd\u3002\u6b64\u65b0\u578b\u7684\u6b63\u6781\u6750\u6599\u7535\u5316\u5b66\u6027\u80fd\u4f18\u5f02\uff0c\u5176\u5236\u5907\u5de5\u827a\u53ef\u4ea7\u4e1a\u5316\uff0c\u5c06\u4fc3\u8fdb\u672a\u6765\u94a0\u79bb\u5b50\u7535\u6c60\u5728\u5927\u89c4\u6a21\u50a8\u80fd\u65b9\u9762\u7684\u53d1\u5c55\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5<\/strong>\uff1a<a href=\"http:\/\/onlinelibrary.wiley.com\/wol1\/doi\/10.1002\/aenm.201701610\/abstract\" target=\"_blank\" rel=\"noopener\">High Energy Density Sodium-Ion Battery with Industrially Feasible and Air-Stable O3-Type Layered Oxide Cathode<\/a>\u00a0 (Adv. Energy. Mater, 2017, DOI: 10.1002\/aenm.201701610)<\/p>\n<p><strong>\u56e2\u961f\u76f8\u5173\u8bba\u6587\u6c47\u603b<\/strong>\uff1a<br \/>\n <a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/aenm.201701428\/full\" target=\"_blank\" rel=\"noopener\">Advanced Energy Materials, 2017, DOI: 10.1002\/aenm.201701428;<\/a><br \/>\n <a href=\"http:\/\/pubs.acs.org\/doi\/10.1021\/acsnano.6b07644\" target=\"_blank\" rel=\"noopener\">ACS Nano, 2017, 11, 1747-1754;<\/a><br \/>\n <a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/aenm.201700234\/full\" target=\"_blank\" rel=\"noopener\">Advanced Energy Materials, 2017, DOI: 10.1002\/aenm.201700234;<\/a><br \/>\n <a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.201502262\/abstract\" target=\"_blank\" rel=\"noopener\">Advanced Materials 2015, 27, 6862-6869;<\/a><br \/>\n <a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/smll.201600699\/abstract\" target=\"_blank\" rel=\"noopener\">Small 2016, 12, 3031-3038;<\/a><br \/>\n <a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/smll.201403535\/abstract\" target=\"_blank\" rel=\"noopener\">Small 2015, 11, 2817-2824;<\/a><br \/>\n <a href=\"http:\/\/pubs.rsc.org\/en\/content\/articlelanding\/2015\/cc\/c5cc01857a#!divAbstract\" target=\"_blank\" rel=\"noopener\">Chemical communications 2015, 51, 8269-8272;<\/a><br \/>\n <a href=\"http:\/\/pubs.rsc.org\/en\/content\/articlelanding\/2017\/ta\/c6ta10751f#!divAbstract\" target=\"_blank\" rel=\"noopener\">Journal of Materials Chemistry A 2017, 5, 5283-5289;\u00a0\u00a0<\/a><\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u65b0\u80fd\u6e90\u5c0f\u7ec4 \u66fe\u6c99 \u4f9b\u7a3f\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p><strong>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1aRDD-2011-CHERISH\uff0c\u4efb\u4e39\u4e39\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/strong><\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u94a0\u79bb\u5b50\u7535\u6c60\u7531\u4e8e\u8d44\u6e90\u4e30\u5bcc\u3001\u8d85\u9ad8\u7684\u5b89\u5168\u6027\u7b49\u7279\u70b9\u4ee5\u53ca\u4e0e\u9502\u7535\u7c7b\u4f3c\u7684\u5316\u5b66\u7279\u6027\uff0c\u88ab\u8ba4\u4e3a\u662f\u6700\u5177\u6f5c\u529b\u7684\u66ff\u4ee3\u9502\u79bb\u5b50\u7535\u6c60\u7684\u80fd\u91cf\u5b58\u50a8\u7cfb\u7edf\u4e4b\u4e00\u3002\u76ee\u524d\u5df2\u6709\u8bb8\u591a\u5b66\u672f\u7814\u7a76\u63a2\u7d22\u9ad8\u6027\u80fd&#8230;<\/p>\n","protected":false},"author":4633,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-106807","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/106807"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/4633"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=106807"}],"version-history":[{"count":9,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/106807\/revisions"}],"predecessor-version":[{"id":106978,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/106807\/revisions\/106978"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=106807"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=106807"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=106807"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}