{"id":108140,"date":"2017-10-24T06:30:01","date_gmt":"2017-10-23T22:30:01","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=108140"},"modified":"2017-10-25T21:39:50","modified_gmt":"2017-10-25T13:39:50","slug":"nano-letters%ef%bc%9a%e7%bc%ba%e9%99%b7%e8%af%b1%e5%af%bcmos2%e7%ba%b3%e7%b1%b3%e5%b8%a6%e5%a4%96%e5%bb%b6%e7%94%9f%e9%95%bf%e5%8f%8a%e5%85%b6%e9%ab%98%e6%95%88%e5%85%89%e5%82%ac%e5%8c%96%e5%88%b6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=108140","title":{"rendered":"Nano Letters\uff1a\u7f3a\u9677\u8bf1\u5bfcMoS2\u7eb3\u7c73\u5e26\u5916\u5ef6\u751f\u957f\u53ca\u5176\u9ad8\u6548\u5149\u50ac\u5316\u5236\u6c22"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u968f\u7740\u7ecf\u6d4e\u7684\u8fc5\u731b\u53d1\u5c55\uff0c\u6211\u56fd\u5bf9\u80fd\u6e90\u7684\u9700\u6c42\u65e5\u76ca\u589e\u52a0\u3002\u76ee\u524d\uff0c\u4eba\u7c7b\u4ecd\u4e3b\u8981\u4f9d\u8d56\u4e8e\u5316\u77f3\u71c3\u6599\u63d0\u4f9b\u80fd\u6e90\uff0c\u8fc7\u5ea6\u4f7f\u7528\u5316\u77f3\u71c3\u6599\u5df2\u9020\u6210\u4e25\u91cd\u7684\u80fd\u6e90\u548c\u73af\u5883\u95ee\u9898\uff0c\u5bfb\u6c42\u6e05\u6d01\u7684\u53ef\u518d\u751f\u80fd\u6e90\u8feb\u5728\u7709\u776b\u3002\u6c22\u6c14\u4f5c\u4e3a\u4e00\u79cd\u9ad8\u6548\u6e05\u6d01\u7684\u4e8c\u6b21\u80fd\u6e90\u8f7d\u4f53\uff0c\u88ab\u8a89\u4e3a\u672a\u6765\u7684\u77f3\u6cb9\u3002\u5f00\u53d1\u548c\u5229\u7528\u65e0\u6c61\u67d3\u7684\u6c22\u80fd\u6e90\u662f\u66ff\u4ee3\u5316\u77f3\u71c3\u6599\u7684\u4e00\u79cd\u6700\u4f73\u9014\u5f84\uff0c\u56e0\u6b64\u53d7\u5230\u4e86\u5404\u56fd\u7684\u9ad8\u5ea6\u5173\u6ce8\u3002\u6c34\u5206\u89e3\u5236\u6c22\u662f\u4ee5\u81ea\u7136\u754c\u53d6\u4e4b\u4e0d\u5c3d\u7684\u6c34\u4e3a\u539f\u6599\uff0c\u901a\u8fc7\u7535\u50ac\u5316\u5206\u89e3\u6c34\u7684\u65b9\u5f0f\u751f\u6210\u6c22\u6c14\uff0c\u56e0\u6b64\u662f\u4e00\u79cd\u5b89\u5168\u3001\u7eff\u8272\u3001\u6709\u6548\u7684\u5236\u6c22\u65b9\u6cd5\u3002\u4f46\u662f\u76ee\u524d\u5168\u7403\u4ec5\u670920%\u5de6\u53f3\u7684\u6c22\u6c14\u6765\u81ea\u4e8e\u6c34\u5206\u89e3\uff0c\u5176\u4e3b\u8981\u539f\u56e0\u662f\u6c34\u5206\u89e3\u8fc7\u5ea6\u4f9d\u8d56\u7a00\u6709\u91d1\u5c5e\u505a\u50ac\u5316\u5242\uff0c\u6bd4\u5982\u94c2\u3001\u94f1\u548c\u94d1\u3002\u800c\u8fd9\u4e9b\u7a00\u6709\u91d1\u5c5e\u50a8\u91cf\u5c11\u3001\u4ef7\u683c\u6602\u8d35\uff0c\u65e0\u6cd5\u6ee1\u8db3\u5de5\u4e1a\u751f\u4ea7\u9700\u8981\u3002\u8fd1\u5e74\u6765\uff0c\u5bfb\u627e\u4ef7\u683c\u4f4e\u5ec9\u3001\u81ea\u7136\u754c\u50a8\u91cf\u9ad8\u7684\u6790\u6c22\u50ac\u5316\u5242\u6210\u4e3a\u4e86\u80fd\u6e90\u3001\u6750\u6599\u3001\u51dd\u805a\u6001\u7269\u7406\u3001\u5316\u5b66\u7b49\u8bf8\u591a\u9886\u57df\u7684\u7814\u7a76\u70ed\u70b9\u3002<\/p>\n<p>\u5149\u50ac\u5316\u5236\u6c22\u662f\u4e00\u79cd\u5f00\u8def\u7684\u5149\u7535\u5316\u5b66\u53cd\u5e94\uff0c\u4e3b\u8981\u901a\u8fc7\u5149\u9a71\u52a8\u534a\u5bfc\u4f53\u6750\u6599\u751f\u6210\u7535\u5b50\/\u7a7a\u7a74\u5bf9\uff0c\u7535\u5b50\u4f20\u8f93\u5230\u6790\u6c22\u50ac\u5316\u5242\u7136\u540e\u4e0e\u6c34\u53cd\u5e94\u751f\u6210\u6c22\u6c14\u3002\u4ee5\u7535\u5b50\u4f5c\u4e3a\u5a92\u4ecb\uff0c\u8fd9\u79cd\u7b56\u7565\u5b9e\u73b0\u4e86\u5149\u80fd\u5230\u5316\u5b66\u80fd\u7684\u76f4\u63a5\u8f6c\u6362\uff0c\u662f\u4e00\u79cd\u80fd\u591f\u4ece\u6839\u672c\u4e0a\u66ff\u4ee3\u5316\u77f3\u71c3\u6599\u7684\u4eba\u5de5\u5149\u5408\u6280\u672f\uff0c\u56e0\u6b64\u79f0\u4e3a\u53ef\u6301\u7eed\u201c\u5149\u5b50\u201d\u7ecf\u6d4e\u6548\u5e94\u3002\u8fc7\u53bb\u4e8c\u5341\u5e74\uff0c\u7814\u7a76\u7684\u7126\u70b9\u4e3b\u8981\u96c6\u4e2d\u5728\u5982\u4f55\u6539\u6027\u534a\u5bfc\u4f53\u6750\u6599\uff0c\u7f29\u5c0f\u5e26\u9699\uff0c\u589e\u52a0\u5149\u6355\u83b7\u80fd\u529b\uff0c\u63d0\u9ad8\u5149\u751f\u7535\u5b50\u6548\u7387\u4e0a\uff0c\u800c\u5bf9\u4e8e\u6790\u6c22\u50ac\u5316\u5242\u7684\u7814\u7a76\uff0c\u4e3b\u8981\u4ee5\u8d1f\u8f7d\u94c2\u4e3a\u4e3b\u3002\u76f4\u5230\u8d8a\u6765\u8d8a\u591a\u7684\u5ec9\u4ef7\u7684\u3001\u9ad8\u6d3b\u6027\u7684\u6790\u6c22\u50ac\u5316\u5242\u88ab\u62a5\u9053\u540e\uff0c\u4eba\u4eec\u624d\u5f00\u59cb\u8003\u8651\u4ece\u6790\u6c22\u50ac\u5316\u5242\u5165\u624b\uff0c\u964d\u4f4e\u5149\u50ac\u5316\u5236\u6c22\u7684\u6210\u672c\u3002\u65e9\u572820\u4e16\u7eaa70\u5e74\u4ee3\uff0c\u5c31\u6709\u5173\u4e8eMoS<sub>2<\/sub>\u50ac\u5316\u6790\u6c22\u53cd\u5e94\u7684\u62a5\u9053\u3002\u7136\u800c\u5757\u4f53\u7684MoS<sub>2<\/sub>\u7531\u4e8e\u5bfc\u7535\u6027\u5dee\u3001\u6d3b\u6027\u4f4d\u70b9\u5c11\u5bfc\u81f4\u50ac\u5316\u6027\u80fd\u5dee\uff0c\u56e0\u6b64\u4e4b\u540e\u7684\u5f88\u957f\u4e00\u6bb5\u65f6\u95f4\uff0c\u5173\u4e8eMoS<sub>2<\/sub> \u7684\u6790\u6c22\u53cd\u5e94\u50ac\u5316\u5242\u90fd\u65e0\u4eba\u95ee\u6d25\u3002\u76f4\u52302005\u5e74\uff0cHinnemann\u7b49\u53d1\u73b0MoS<sub>2<\/sub>\u7684Mo\u8fb9\u754c\u7ed3\u6784\u4e0e\u56fa\u6c2e\u9176\u7684\u6790\u6c22\u53cd\u5e94\u6d3b\u6027\u4f4d\u70b9\u7684\u7ed3\u6784\u6781\u4e3a\u76f8\u4f3c\uff0c\u53ef\u80fd\u5177\u6709\u5f88\u9ad8\u7684\u6790\u6c22\u53cd\u5e94\u50ac\u5316\u6d3b\u6027\uff0c\u4e14\u8fd9\u79cd\u7c7b\u77f3\u58a8\u70ef\u4e8c\u7ef4\u6750\u6599\u5177\u6709\u8d85\u9ad8\u7684\u6bd4\u8868\u9762\u79ef\u548c\u4f4e\u5ec9\u7684\u4ef7\u683c\u7b49\u4f18\u70b9\uff0c\u62e5\u6709\u5de8\u5927\u7684\u5546\u4e1a\u4ef7\u503c\u3002\u4f46\u662f\u76f8\u5bf9\u4e8e\u91d1\u5c5e\u94c2\uff0cMoS<sub>2<\/sub>\u662f\u4e8c\u7ef4\u7ed3\u6784\u7684\u534a\u5bfc\u4f53\u6750\u6599\uff0c\u4e0e\u5149\u50ac\u5316\u5242\u7ed3\u5408\u65f6\uff0c\u5f02\u8d28\u7ed3\u754c\u9762\u533a\u57df\u8f83\u5c0f\u4e14\u7535\u8377\u4f20\u8f93\u8fdf\u7f13\uff0c\u5982\u4f55\u901a\u8fc7\u7eb3\u7c73\u7ed3\u6784\u7684\u8c03\u63a7\u63d0\u9ad8MoS<sub>2<\/sub>\u6790\u6c22\u6d3b\u6027\u662f\u63a8\u52a8\u8fd9\u79cd\u65e0\u94c2\u5f00\u8def\u5149\u50ac\u5316\u53cd\u5e94\u7684\u5173\u952e\u3002\u9488\u5bf9\u8fd9\u4e00\u5173\u952e\u79d1\u5b66\u95ee\u9898\uff0c\u5f20\u4f83\u6559\u6388\u901a\u8fc7MoS<sub>2<\/sub>\u5b9a\u5411\u9644\u7740\u751f\u957f\u673a\u5236\u6210\u529f\u5236\u5907\u4e86\u975e\u5bf9\u79f0\u4e0e\u5bf9\u79f0MoS2\u672b\u68a2\u710a\u63a5CdS\u7eb3\u7c73\u7ebf\uff08tipped\u00a0structure\u5206\u522b\u53d1\u8868\u4e8eAdv. Func.\u00a0Mater.\u00a026 (2016) 4527\uff0cNano.\u00a0Energy.\u00a034 (2017) 481\u4e0a\uff09\uff0c\u5728420nm\u6ce2\u957f\u4e0b\u83b7\u5f97\u4e8637.6%\u7684\u91cf\u5b50\u6548\u7387\u3002\u7136\u800c\uff0c\u94c2\u672b\u68a2\u710a\u63a5CdS\u7eb3\u7c73\u7ebf\u5728\u5149\u50ac\u5316\u5236\u6c22\u53cd\u5e94\u4e2d\u7684\u91cf\u5b50\u6548\u7387\u5df2\u7ecf\u63a5\u8fd1100%\uff0c\u56e0\u6b64\uff0c\u5c31\u7535\u8377\u4f20\u8f93\u6548\u7387\u800c\u8a00\uff0cMoS<sub>2<\/sub>\u8ddf\u94c2\u4e4b\u95f4\u4ecd\u5b58\u5728\u5f88\u5927\u7684\u5dee\u8ddd\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u5357\u4eac\u7406\u5de5\u5927\u5b66\u5f20\u4f83\u6559\u6388<\/strong>\u4f9d\u6258<strong>\u66fe\u6d77\u6ce2\u6559\u6388<\/strong>\u7684<strong>\u5de5\u4fe1\u90e8\u91cd\u70b9\u5b9e\u9a8c\u5ba4<\/strong>\uff0c\u4e0e<strong>\u7f8e\u56fd\u65af\u5766\u798f\u5927\u5b66\uff0c\u97e9\u56fd\u5ef6\u4e16\u5927\u5b66\uff0c\u97e9\u56fd\u6210\u5747\u9986\u5927\u5b66\uff0c\u97e9\u56fd\u79d1\u5b66\u7814\u7a76\u9662<\/strong>\u5c55\u5f00\u591a\u65b9\u7b49\u5408\u4f5c\uff0c\u901a\u8fc7\u7f3a\u9677\u8bf1\u5bfc\u7684\u5916\u5ef6\u751f\u957f\u6cd5\uff0c\u6210\u529f\u5408\u6210\u51fa\u4e86[001]\u53d6\u5411\u7684MoS<sub>2<\/sub>\u7eb3\u7c73\u5e26\/[0001]\u53d6\u5411\u7684CdS\u7eb3\u7c73\u7ebf\u7684\u5171\u8f74\u5f02\u8d28\u7ed3\u6784\u3002\u8fd9\u79cd\u5916\u5ef6\u7684\u5f02\u8d28\u7ed3\u6784\u5728420nm\u4e0b\uff0c\u8fbe\u5230\u4e8679.7%\u7684\u5149\u751f\u6c22\u6c14\u7684\u91cf\u5b50\u6548\u7387\uff0c\u5e76\u5728520nm\u6781\u9650\u5438\u6536\u8fb9\u754c\u4e0b\uff0c\u4ecd\u7136\u62e5\u67099.67%\u7684\u91cf\u5b50\u6548\u7387\u3002\u7ed3\u679c\u8868\u660e\uff0cCdS\u7eb3\u7c73\u7ebf\u8868\u754c\u9762\u7684\u7f3a\u9677\u79cd\u7c7b\u662f\u95f4\u9699\u91d1\u5c5eCd<sup>0<\/sup>\uff0c\u5e76\u96c6\u4e2d\u5728CdS\u7684(110)\u6676\u9762\u4e0a\u3002\u800cCdS(110)\u6676\u9762\u4e0a\u7684(101)\u7684\u6676\u683c\u95f4\u8ddd\u4e0eMoS<sub>2<\/sub>\uff08002\uff09\u6676\u9762\u7684\u6676\u683c\u95f4\u8ddd\u5339\u914d\u5ea6\u9ad8\u8fbe99.7%\uff0c\u901a\u8fc7\u95f4\u9699\u91d1\u5c5eCd\uff0c\u6210\u529f\u5f62\u6210\u4e86\u5171\u8f74\uff0c\u4e14\u4e0e\u8f74\u5411\u6210~30\u00b0\u5939\u89d2\u7684MoS<sub>2<\/sub>\u7eb3\u7c73\u5e26\/CdS\u7eb3\u7c73\u7ebf\u7684\u5916\u5ef6\u7ed3\u6784\u3002\u901a\u8fc7\u4f4e\u635f\u8017\u7684\u7535\u5b50\u80fd\u91cf\u635f\u5931\u8c31\uff0c\u8fdb\u4e00\u6b65\u8bc1\u5b9e\u4e86\u4e00\u4e2a\u4e0d\u540c\u4e8eCdS\u548cMoS<sub>2<\/sub>\u7eb3\u7c73\u5e26\u7684\u754c\u9762\u7ec4\u5206\uff0c\u968f\u540e\u7684\u5bc6\u5ea6\u6cdb\u51fd\u7406\u8bba\u6a21\u62df\u63ed\u793a\u4e86\u8fd9\u79cd\u7279\u6b8a\u7684\u754c\u9762\u5177\u6709\u91d1\u5c5e\u7279\u6027\uff0c\u56e0\u6b64\u4fc3\u8fdb\u4e86\u7535\u5b50\u5728\u754c\u9762\u7684\u4f4e\u635f\u8017\u4f20\u8f93\u3002\u8fd9\u4e00\u7ed3\u679c\u4e3a\u4ee5\u540e\u65b0\u578b\u65e0\u73c0\u6790\u6c22\u50ac\u5316\u5242\u5728\u5f00\u8def\u5149\u50ac\u5316\u5236\u6c22\u53cd\u5e94\u4e2d\u7684\u5e94\u7528\u6253\u5f00\u4e86\u4e00\u6247\u7a97\uff0c\u5e76\u4e3a\u5149\u50ac\u5316\u5242\u7684\u8bbe\u8ba1\u63d0\u4f9b\u4e86\u65b0\u7684\u601d\u8def\uff0c\u76f8\u5173\u7ed3\u679c\u53d1\u8868\u5728\u6700\u65b0\u4e00\u671f\u7684<strong>Nano Letters<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-108638\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/1-85.jpg\" alt=\"\" width=\"600\" height=\"522\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/1-85.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/1-85-300x261.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a-c\uff09CdS\u7eb3\u7c73\u7ebf\u7684(0002)\u6676\u9762<\/p>\n<p>\uff08d-f\uff09CdS\u7eb3\u7c73\u7ebf\u7684(110)\u6676\u9762<\/p>\n<p>\uff08g\uff0ch\uff09Cd\u00a03d\u00a0\u548c S 2p\u7684X\u5c04\u7ebf\u5149\u7535\u5b50\u8c31<\/p>\n<p>\uff08i\uff0c\u00a0j\uff09CdS\u7684(0002)\u548c(110)\u6676\u9762\u6a21\u578b\u4ee5\u53ca\u5bf9\u5e94\u7684\u5085\u91cc\u53f6\u8f6c\u5316\u70b9\u9635\u56fe\u8c31<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-108143\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72472-22.png\" alt=\"\" width=\"600\" height=\"253\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72472-22.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72472-22-300x127.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a-e\uff09\u5916\u5ef6\u9010\u6e10\u589e\u751f\u7684MoS<sub>2<\/sub>\u7eb3\u7c73\u5e26<\/p>\n<p>\uff08f\uff09\u9ad8\u89d2\u73af\u5f62\u6697\u573a\u50cf-\u626b\u63cf\u900f\u5c04\u7535\u5b50\u50cf\u4ee5\u53ca\u5143\u7d20\u5206\u5e03<\/p>\n<p>\uff08g\uff09\u5916\u5ef6\u754c\u9762\u7684\u9ad8\u6e05\u900f\u5c04\u50cf<\/p>\n<p>\uff08h\uff09\u5916\u5ef6\u7684\u6676\u4f53\u7ed3\u6784\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-108144\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72473-16.png\" alt=\"\" width=\"600\" height=\"685\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72473-16.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72473-16-263x300.png 263w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5916\u5ef6\u754c\u9762\u7684\u9ad8\u89d2\u73af\u5f62\u6697\u573a\u50cf\u4ee5\u53ca\u7403\u9762\u50cf\u5dee\u4fee\u6b63-\u626b\u63cf\u900f\u5c04\u7535\u5b50\u50cf<\/p>\n<p>\uff08b\uff09\u4f4e\u635f\u8017\u7535\u5b50\u4e22\u5931\u80fd\u8c31<\/p>\n<p>\uff08c\uff09\u5916\u5ef6\u754c\u9762\u7684\u5361\u65b9\u7cfb\u6570\u5206\u5e03\u56fe<\/p>\n<p>\uff08d\uff09\u5916\u5ef6\u754c\u9762\u7684\u626b\u63cf\u900f\u5c04\u7535\u5b50\u50cf\u7684\u5143\u7d20\u5206\u5e03\u56fe<\/p>\n<p>\uff08e\uff0cf\uff09\u5916\u5ef6\u754c\u9762\u7684\u6001\u5bc6\u5ea6\u4ee5\u53ca\u7535\u5b50\u5c40\u57df\u51fd\u6570\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-108146\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72474-18.png\" alt=\"\" width=\"600\" height=\"631\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72474-18.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/10\/\u56fe\u72474-18-285x300.png 285w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5f00\u8def\u5149\u50ac\u5316\u5236\u6c22\u4ea7\u7387<\/p>\n<p>\uff08b\uff09\u5355\u5149\u5b50\u8ba1\u6570\u4e0b\u7684\u5149\u751f\u7535\u5b50\u5bff\u547d<\/p>\n<p>\uff08c\uff09\u5149\u50ac\u5316\u5236\u6c22\u7684\u5faa\u73af\u6d4b\u8bd5<\/p>\n<p><strong><b>\u4e2a\u4eba\u7b80\u5386<\/b><\/strong><\/p>\n<p>\u5f20\u4f83\uff0c\u5357\u4eac\u7406\u5de5\u5927\u5b66\u6750\u6599\u5b66\u9662\u6559\u6388\u30022015\u5e74\u83b7\u5f97\u97e9\u56fd\u6210\u5747\u9986\u5927\u5b66\u7eb3\u7c73\u5de5\u5b66\u535a\u58eb\uff0c2015~2017\u5ef6\u4e16\u5927\u5b66BK1+\u7814\u7a76\u6559\u6388\u3002\u4e3b\u8981\u4ece\u4e8b\u5149\u7535\u534a\u5bfc\u4f53\u6750\u6599\u7684\u5fae\u89c2\u6784\u7b51\u3001\u5668\u4ef6\u7684\u5b8f\u89c2\u96c6\u6210\u53ca\u5176\u5728\u5149\u7535\u8f6c\u6362\u53ca\u5b58\u50a8\u7684\u5e94\u7528\u7814\u7a76\u3002\u5728\u6750\u6599\u7f3a\u9677\u6001\u6539\u6027\u3001\u5668\u4ef6\u8868\u754c\u9762\u7ed3\u6784\u8bbe\u8ba1\u3001\u7535\u8377\u4f20\u8f93\u548c\u8f6c\u79fb\u8c03\u63a7\u7b49\u65b9\u9762\u5171\u53d1\u8868SCI\/SCIE\u8bba\u658750\u4f59\u7bc7\uff0c\u4ed6\u5f151500\u4f59\u6b21 (h-index 22)\u3002\u8fd13\u5e74\u5c31\u5149\u7535\u8f6c\u6362\u53ca\u5b58\u50a8\u9886\u57df\u53d1\u8868\u8bba\u6587\u5982\u4e0b\u3002<\/p>\n<p>1.Double 2-dimensional H2-evoluting catalyst tipped photocatalyst nanowires: A new avenue for high-efficiency solar to H<sub>2<\/sub> generation. Nano Energy 34 (2017) 481<\/p>\n<p>2.Overcoming Charge Collection Limitation at Solid\/Liquid Interface by a Controllable Crystal Deficient Overlayer. Adv.\u00a0Energy.\u00a0Mater. 7 (2017) 1600923.<\/p>\n<p>3.An Order\/Disorder\/Water Junction System for Highly Efficient Co-Catalyst-Free Photocatalytic Hydrogen Generation. Energy. Environ. Sci. 9 (2016) 499.<\/p>\n<p>4.Delocalized Electron Accumulation at Nanorod Tips: Origin of Efficient H2 Generation. Adv.\u00a0Funct.\u00a0Mater.\u00a026 (2016) 4527<\/p>\n<p>5.Dual Oxygen and Tungsten Vacancies on a WO3 Photoanode for Enhanced Water Oxidation. Angew. Chem. Int. Ed. 55 (2016) 11819.<\/p>\n<p>6.Unassisted photoelectrochemical water splitting beyond 5.7% solar-to-hydrogen conversion efficiency by a wireless monolithic photoanode\/dye-sensitised solar cell tandem device. Nano Energy 13 (2015) 182.<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/pubs.acs.org\/doi\/10.1021\/acs.nanolett.7b02622\" target=\"_blank\" rel=\"noopener\">Defect-Induced Epitaxial Growth for Efficient Solar Hydrogen Production<\/a>\uff08Nano Letters,2017,DOI: 10.1021\/acs.nanolett.7b02622\uff09<\/p>\n<p>\u672c\u6587\u7531\u5357\u4eac\u7406\u5de5\u5927\u5b66\u5f20\u4f83\u8001\u5e08\u6295\u7a3f\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p><strong><b>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1aRDD-2011-CHERISH\uff0c\u4efb\u4e39\u4e39\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/b><\/strong><\/p>\n<p><strong><b>\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c<\/b><\/strong><strong><b>\u4e0a<\/b><\/strong><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\"><strong><b>\u6d4b\u8bd5\u8c37<\/b><\/strong><\/a><strong><b>\uff01<\/b><\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u8fd1\u5e74\u6765\uff0c\u968f\u7740\u7ecf\u6d4e\u7684\u8fc5\u731b\u53d1\u5c55\uff0c\u6211\u56fd\u5bf9\u80fd\u6e90\u7684\u9700\u6c42\u65e5\u76ca\u589e\u52a0\u3002\u76ee\u524d\uff0c\u4eba\u7c7b\u4ecd\u4e3b\u8981\u4f9d\u8d56\u4e8e\u5316\u77f3\u71c3\u6599\u63d0\u4f9b\u80fd\u6e90\uff0c\u8fc7\u5ea6\u4f7f\u7528\u5316\u77f3\u71c3\u6599\u5df2\u9020\u6210\u4e25\u91cd\u7684\u80fd\u6e90\u548c\u73af\u5883\u95ee\u9898\uff0c\u5bfb\u6c42\u6e05\u6d01\u7684\u53ef&#8230;<\/p>\n","protected":false},"author":349,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[113,33],"class_list":["post-108140","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-semiconductor","tag-nano"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/108140"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/349"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=108140"}],"version-history":[{"count":8,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/108140\/revisions"}],"predecessor-version":[{"id":108149,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/108140\/revisions\/108149"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=108140"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=108140"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=108140"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}