{"id":111932,"date":"2017-11-15T06:30:26","date_gmt":"2017-11-14T22:30:26","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=111932"},"modified":"2017-11-14T17:45:13","modified_gmt":"2017-11-14T09:45:13","slug":"corrors-sci-%ef%bc%9a%e8%a1%a8%e5%b1%82%e7%bb%93%e6%9e%84%e6%a2%af%e5%ba%a6%e5%8c%96%e5%af%b97150%e9%93%9d%e5%90%88%e9%87%91%e5%b1%80%e9%83%a8%e8%85%90%e8%9a%80%e6%98%af%e4%b8%80%e6%8a%8a%e5%8f%8c","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=111932","title":{"rendered":"Corrors. Sci.\uff1a\u8868\u5c42\u7ed3\u6784\u68af\u5ea6\u5316\u5bf97150\u94dd\u5408\u91d1\u5c40\u90e8\u8150\u8680\u662f\u4e00\u628a\u53cc\u5203\u5251"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><br \/>\n \u91d1\u5c5e\u6750\u6599\u6676\u7c92\u5c3a\u5bf8\u7eb3\u7c73\u5316\u53ef\u5206\u4e3a\u4e24\u5927\u7c7b\uff1a\u5757\u4f53\u7eb3\u7c73\u5316\u548c\u8868\u5c42\u7eb3\u7c73\u5316\u3002\u5757\u4f53\u7eb3\u7c73\u5316\u540e\uff0c\u6784\u4ef6\u6574\u4f53\u5f3a\u5ea6\u663e\u8457\u589e\u5927\uff0c\u540c\u65f6\u4e5f\u4f34\u968f\u7740\u97e7\u6027\u7684\u5267\u70c8\u4e0b\u964d\u3002\u8fd9\u4e00\u4e16\u754c\u6027\u96be\u9898\u76ee\u524d\u8fd8\u6682\u65f6\u65e0\u89e3\u3002\u8868\u5c42\u7eb3\u7c73\u5316\u867d\u7136\u5bf9\u6784\u4ef6\u6574\u4f53\u5f3a\u5ea6\u7684\u6539\u5584\u6709\u9650\uff0c\u4f46\u5bf9\u8868\u9762\u76f8\u5173\u6027\u8d28\u5982\u8150\u8680\u3001\u75b2\u52b3\u548c\u65ad\u88c2\u97e7\u6027\u7b49\u4f5c\u7528\u5de8\u5927\u3002\u76ee\u524d\u6765\u770b\uff0c\u8868\u5c42\u7eb3\u7c73\u5316\u662f\u66f4\u6709\u5e94\u7528\u524d\u666f\u7684\u4e00\u7c7b\u6280\u672f\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><br \/>\n \u8fd1\u65e5\uff0c<strong>\u666e\u6e21\u5927\u5b66Qingyou Han<\/strong>\u6559\u6388<strong>\uff08\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u5728<strong>Corrors. Sci<\/strong>\u4e0a\u53d1\u8868\u4e86\u9898\u4e3a\u201c<strong>Localized corrosion behaviour of AA7150 after ultrasonic shot peening: corrosion depth vs. impact energy<\/strong>\u201d\u7684\u6587\u7ae0\u3002\u8be5\u6587\u7814\u7a76\u4e86\u8d85\u58f0\u55b7\u4e38\u8868\u9762\u5267\u70c8\u5851\u6027\u53d8\u5f62\u540eAA7150\u94dd\u5408\u91d1\u7684\u5c40\u90e8\u8150\u8680\u52a8\u529b\u5b66\u7279\u5f81\u3002\u8d85\u58f0\u55b7\u4e38\u5904\u7406\u540e\uff0c\u94dd\u5408\u91d1\u8868\u5c42\u6676\u7c92\u5c3a\u5bf8\u7eb3\u7c73\u5316\u3001\u68af\u5ea6\u5316\uff0c\u65f6\u6548\u6790\u51fa\u7684\u7eb3\u7c73\u5f3a\u5316\u76f8\u91cd\u65b0\u56de\u6eb6\u8868\u5c42\u94dd\u57fa\u4f53\uff0c\u7ec4\u7ec7\u5747\u4e00\u5316\u6548\u679c\u663e\u8457\u3002\u8868\u5c42\u5316\u5b66\u6210\u5206\u4e5f\u51fa\u73b0\u53d8\u5316\uff0c\u83b7\u53d6\u4e86\u4e00\u79cd\u8868\u5c42\u7ed3\u6784\u68af\u5ea6\u5316\u76847150\u94dd\u5408\u91d1\u3002<\/p>\n<p>\u901a\u8fc7\u8c03\u63a7\u55b7\u4e38\u65f6\u95f4\u3001\u8d85\u58f0\u632f\u5e45\u3001\u55b7\u4e38\u8ddd\u79bb\u548c\u55b7\u4e38\u7c92\u5f84\uff0c\u83b7\u53d6\u4e86\u4e0d\u540c\u51b2\u51fb\u80fd\u91cf\u7684AA7150\u6837\u54c1\u3002\u5728\u6807\u51c6\u6676\u95f4\u8150\u8680\u6eb6\u6db2\u4e2d\u6d78\u6ce124h\u540e\uff0c\u9ad8\u80fd\u91cf\u55b7\u4e38\u5904\u7406\u6837\uff08\u5851\u6027\u53d8\u5f62\u539a\u5ea6 &gt; 20 \u00b5m\uff09\u7684\u5c40\u90e8\u8150\u8680\u5b8c\u5168\u88ab\u6291\u5236\u3002\u4f46\u4f4e\u80fd\u91cf\u55b7\u4e38\u5904\u7406\u6837\uff08\u5851\u6027\u53d8\u5f62\u539a\u5ea6 &lt; 20 \u00b5m\uff09\u7684\u70b9\u8680\u5751\u5448\u201c\u9488\u72b6\u201d\uff0c\u8150\u8680\u6df1\u5ea6\u53cd\u800c\u6bd4\u7a7a\u767d\u6837\u66f4\u5927\u3002\u6d78\u6ce172h\u540e\uff0c\u9ad8\u80fd\u91cf\u55b7\u4e38\u5904\u7406\u6837\u4e5f\u51fa\u73b0\u7a7f\u900f\u529b\u66f4\u5f3a\u7684\u201c\u9488\u72b6\u201d\u70b9\u8680\u5751\u3002\u8fd9\u662f\u7531\u4e8e\u8868\u5c42\u7ed3\u6784\u68af\u5ea6\u5316\u662f\u4e00\u628a\u53cc\u5203\u5251\uff0c\u5b83\u80fd\u591f\u663e\u8457\u6291\u5236\u5408\u91d1\u5c40\u90e8\u8150\u8680\u7684\u8bf1\u53d1\u4f46\u53c8\u4f1a\u52a0\u901f\u5c40\u90e8\u8150\u8680\u7684\u6269\u5c55\u8fc7\u7a0b\u3002\u672c\u6587\u6784\u5efa\u4e86\u8868\u5c42\u7ec4\u7ec7\u3001\u6210\u5206\u4e0e\u5c40\u90e8\u8150\u8680\u4e4b\u95f4\u7684\u5173\u7cfb\u3002<\/p>\n<p><strong>Graphic Abstract<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111933\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/0-3.jpg\" alt=\"\" width=\"600\" height=\"309\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/0-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/0-3-300x155.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00 \u00a07150\u677f\u6750\u7684\u91d1\u76f8<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111934\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/1-57.jpg\" alt=\"\" width=\"600\" height=\"752\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/1-57.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/1-57-239x300.jpg 239w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe\u4e8c \u00a0\u8d85\u58f0\u55b7\u4e38\u88c5\u7f6e\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111935\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/2-44.jpg\" alt=\"\" width=\"600\" height=\"475\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/2-44.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/2-44-300x238.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u8868\u4e00 \u00a0\u56db\u7ec4\u8d85\u58f0\u55b7\u4e38\u5904\u7406\u53c2\u6570<\/strong><\/p>\n<table style=\"height: 129px; width: 595px;\">\n<tbody>\n<tr style=\"height: 25px;\">\n<td style=\"width: 165px; height: 25px; text-align: center;\">3mm-8.2mm-80%-t<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">7.5s<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">30s<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">2min<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">4min<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">8min<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">16min<\/td>\n<\/tr>\n<tr style=\"height: 25px;\">\n<td style=\"width: 165px; height: 25px; text-align: center;\">4mm-10mm-A-8min<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">30%<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">40%<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">60%<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">80%<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">100%<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">\u00a0<\/td>\n<\/tr>\n<tr style=\"height: 25px;\">\n<td style=\"width: 165px; height: 25px; text-align: center;\">3mm-d-80%-8min<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">18mm<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">15mm<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">12mm<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">9mm<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">6mm<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">\u00a0<\/td>\n<\/tr>\n<tr style=\"height: 26px;\">\n<td style=\"width: 165px; height: 26px; text-align: center;\">D-10mm-80%-8min<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">1mm<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">3mm<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">5mm<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">\u00a0<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">\u00a0<\/td>\n<td style=\"width: 75px; height: 25px; text-align: center;\">\u00a0<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong>\u56fe\u4e09 \u00a0\u8d85\u58f0\u632f\u5e45\u5bf97150\u94dd\u5408\u91d1\u8868\u5c42\u53d8\u5f62\u539a\u5ea6\u548c\u5c40\u90e8\u8150\u8680\u6df1\u5ea6\u7684\u5f71\u54cd\uff08\u55b7\u4e38\u65f6\u95f4\u3001\u55b7\u4e38\u8ddd\u79bb\u548c\u55b7\u4e38\u7c92\u5f84\u7684\u5f71\u54cd\u8be6\u89c1\u539f\u6587\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111936\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/3-40.jpg\" alt=\"\" width=\"600\" height=\"669\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/3-40.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/3-40-269x300.jpg 269w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(<strong>a<\/strong>) \u8d85\u58f0\u632f\u5e45\u8d8a\u5927\uff0c\u80fd\u91cf\u8d8a\u9ad8\uff0c\u55b7\u4e38\u4f5c\u7528\u6df1\u5ea6\u8d8a\u5927<br \/>\n (<strong>b<\/strong>) \u55b7\u4e38\u5904\u7406\u533a\u57df\u4e0e\u7a7a\u767d\u533a\u57df\u7684\u8150\u8680\u6df1\u5ea6\u5bf9\u6bd4<br \/>\n (<strong>c<\/strong>) \u5c40\u90e8\u8150\u8680\u5f62\u8c8c\u4e0e\u6df1\u5ea6<br \/>\n (<strong>d<\/strong>) \u5c40\u90e8\u8150\u8680\u6df1\u5ea6\u7684\u7edf\u8ba1\u7ed3\u679c<\/p>\n<p><strong>\u56fe\u56db \u00a0\u6837\u54c1\u7684OCP<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111937\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/4-36.jpg\" alt=\"\" width=\"600\" height=\"442\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/4-36.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/4-36-300x221.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(<strong>a<\/strong>) \u55b7\u4e38\u65f6\u95f4\u7684\u5f71\u54cd<br \/>\n (<strong>b<\/strong>) \u8d85\u58f0\u632f\u5e45\u7684\u5f71\u54cd<br \/>\n (<strong>c<\/strong>) \u55b7\u4e38\u8ddd\u79bb\u7684\u5f71\u54cd<br \/>\n (<strong>d<\/strong>) \u55b7\u4e38\u7c92\u5f84\u7684\u5f71\u54cd<\/p>\n<p><strong>\u56fe\u4e94 \u00a0\u5143\u7d20\u8868\u9762\u504f\u6790\u53ca\u5176\u5bf9OCP\u5f71\u54cd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111938\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/5-25.jpg\" alt=\"\" width=\"600\" height=\"393\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/5-25.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/5-25-300x197.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (<strong>a<\/strong>) \u9ad8\u80fd\u91cf\u5904\u7406\u6837\u54c1\u7684\u5143\u7d20\u8868\u5c42\u504f\u6790<br \/>\n (<strong>b<\/strong>) \u4f4e\u80fd\u91cf\u5904\u7406\u6837\u54c1\u7684OCP-\u7ec4\u6210\u5173\u7cfb<br \/>\n (<strong>c<\/strong>) \u9ad8\u80fd\u91cf\u5904\u7406\u6837\u54c1\u7684OCP-\u7ec4\u6210\u5173\u7cfb<\/p>\n<p><strong>\u56fe\u516d \u00a0\u6837\u54c1\u7684XRD\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111939\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/6-16.jpg\" alt=\"\" width=\"600\" height=\"457\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/6-16.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/6-16-300x229.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(<strong>a<\/strong>) \u7a7a\u767d\u6837\u3001\u4f4e\u80fd\u6837\u3001\u9ad8\u80fd\u6837\u4ee5\u53caAl\u7684\u7406\u8bba\u8ba1\u7b97XRD<br \/>\n (b) \u65f6\u6548\u6790\u51fa\u76f8\u7684\u56de\u6eb6<br \/>\n (<strong>c<\/strong>) (<strong>d<\/strong>) \u6676\u7c92\u5c3a\u5bf8\u548c\u5fae\u89c2\u5e94\u53d8\u6c42\u89e3<br \/>\n (<strong>e<\/strong>) (<strong>f<\/strong>) XRD\u884d\u5c04\u5cf0\u7684\u504f\u79fb<\/p>\n<p><strong>\u56fe\u4e03 \u00a0\u6837\u54c1\u7684SEM\u548c TEM<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111940\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/7-10.jpg\" alt=\"\" width=\"600\" height=\"600\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/7-10.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/7-10-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/7-10-300x300.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(<strong>a<\/strong>) \u7a7a\u767d\u6837SEM<br \/>\n (<strong>b<\/strong>) \u9ad8\u80fd\u91cf\u55b7\u4e38\u5904\u7406\u6837\u622a\u9762SEM\u00a0<br \/>\n (<strong>c<\/strong>) \u9ad8\u80fd\u91cf\u55b7\u4e38\u5904\u7406\u6837\u622a\u9762TEM (\u8ddd\u8868\u9762~10 \u00b5m)<br \/>\n (<strong>d<\/strong>) \u9ad8\u80fd\u91cf\u55b7\u4e38\u5904\u7406\u6837\u622a\u9762TEM (\u8ddd\u8868\u9762~5 \u00b5m)<\/p>\n<p><strong>\u56fe\u516b \u00a0\u6837\u54c1\u7684\u6781\u5316\u66f2\u7ebf\u548c\u70b9\u8680\u7535\u4f4d<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111941\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/8-9.jpg\" alt=\"\" width=\"600\" height=\"237\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/8-9.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/8-9-300x119.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(<strong>a<\/strong>) \u6837\u54c1\u7684\u6781\u5316\u66f2\u7ebf<br \/>\n (<strong>b<\/strong>) \u70b9\u8680\u7535\u4f4d\u4e0e\u55b7\u4e38\u65f6\u95f4\u7684\u5173\u7cfb<br \/>\n \u6ce8\uff1a\u8be5\u7ec4\u5c5e\u4e8e\u4f4e\u80fd\u91cf\u55b7\u4e38\u5904\u7406\u6837\u54c1<\/p>\n<p><strong>\u56fe\u4e5d \u00a0\u4e09\u6b21\u6d78\u6ce1\u540e\u7684\u8150\u8680\u622a\u9762\u4e0e\u6df1\u5ea6<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111942\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/9-7.jpg\" alt=\"\" width=\"600\" height=\"831\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/9-7.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/9-7-217x300.jpg 217w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(<strong>a<\/strong>) \u7a7a\u767d\u6837<br \/>\n (<strong>b<\/strong>) \u9ad8\u80fd\u91cf\u51b2\u51fb\u6837\u54c1<br \/>\n (<strong>c<\/strong>) \u8150\u8680\u6df1\u5ea6\u7edf\u8ba1<\/p>\n<p><strong>\u56fe10 \u00a0 \u5c40\u90e8\u8150\u8680\u52a8\u529b\u5b66\u7684\u6bd4\u8f83<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-111943\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/10-6.jpg\" alt=\"\" width=\"600\" height=\"272\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/10-6.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/10-6-300x136.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>1\u3001\u8d85\u58f0\u55b7\u4e38\u5904\u7406\u80fd\u91cf\u8d8a\u5927\uff0cOCP\u8d8a\u8d1f\uff0c\u5f52\u56e0\u4e8eZn\u7684\u8868\u5c42\u504f\u6790\u968f\u7740\u80fd\u91cf\u589e\u5927\u800c\u53d8\u5f97\u663e\u8457\u3002\u9ad8\u80fd\u91cf\u5904\u7406\u7684\u5408\u91d1\u8868\u5c42\u662f\u727a\u7272\u9633\u6781\u5c42\uff0c\u4fdd\u62a4\u4e86\u6b21\u8868\u5c42\u6216\u5408\u91d1\u57fa\u4f53\u3002<\/p>\n<p>2\u3001\u55b7\u4e38\u5904\u7406\u540e\uff0cAA7150\u7684\u70b9\u8680\u7535\u4f4d\u66f4\u6b63\uff0c\u5408\u91d1\u949d\u5316\u533a\u95f4\u589e\u5927\uff0c\u6781\u5927\u5730\u63d0\u5347\u4e86\u5408\u91d1\u8010\u5c40\u90e8\u8150\u8680\u8bf1\u53d1\u7684\u80fd\u529b\u3002\u8fd9\u5f52\u56e0\u4e8e\u8868\u5c42\u7ec4\u7ec7\u7684\u5747\u4e00\u5316\u3001\u6676\u7c92\u626d\u66f2\u7ec6\u5316\u4ee5\u53ca\u6b8b\u4f59\u538b\u5e94\u529b\u7684\u5f15\u5165\u3002<\/p>\n<p>3\u3001\u5408\u91d1\u7684\u5c40\u90e8\u8150\u8680\u4e00\u65e6\u8bf1\u53d1\uff0c\u68af\u5ea6\u5316\u7ed3\u6784\u5bfc\u81f4\u5f62\u6210\u5f00\u53e3\u8f83\u5c0f\u7684\u70b9\u8680\u5751\uff0c\u70b9\u8680\u5751\u5185\u5916\u7684\u7269\u8d28\u4ea4\u6362\u53d7\u963b\uff0c\u8680\u5751\u518d\u949d\u5316\u548c\u6d88\u4ea1\u80fd\u529b\u4e25\u91cd\u4e0b\u964d\uff0c\u56e0\u800c\u5f62\u6210\u4e86\u7a7f\u900f\u80fd\u529b\u66f4\u5f3a\u7684\u201c\u9488\u72b6\u201d\u70b9\u8680\u5751\u3002<\/p>\n<p>4\u3001\u4ece\u5c40\u90e8\u8150\u8680\u7684\u89d2\u5ea6\u770b\uff0c\u8868\u5c42\u7ed3\u6784\u68af\u5ea6\u5316\u53ef\u80fd\u662f\u4e00\u628a\u53cc\u5203\u5251\uff0c\u8981\u6839\u636e\u6750\u6599\u7684\u670d\u5f79\u73af\u5883\u9009\u62e9\u5408\u9002\u7684\u5de5\u827a\u53c2\u6570\uff0c\u5c3d\u91cf\u626c\u957f\u907f\u77ed\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong> <a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0010938X17312532\" target=\"_blank\" rel=\"noopener\">Localized corrosion behaviour of AA7150 after ultrasonic shot peening: corrosion depth vs. impact energy<\/a>(Corrors.Sci,2017,November 10,DOI:10.1016\/j.corsci.2017.11.008 )<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8liunian\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p><strong><b>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1aRDD-2011-CHERISH\uff0c\u4efb\u4e39\u4e39\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/b><\/strong><\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u91d1\u5c5e\u6750\u6599\u6676\u7c92\u5c3a\u5bf8\u7eb3\u7c73\u5316\u53ef\u5206\u4e3a\u4e24\u5927\u7c7b\uff1a\u5757\u4f53\u7eb3\u7c73\u5316\u548c\u8868\u5c42\u7eb3\u7c73\u5316\u3002\u5757\u4f53\u7eb3\u7c73\u5316\u540e\uff0c\u6784\u4ef6\u6574\u4f53\u5f3a\u5ea6\u663e\u8457\u589e\u5927\uff0c\u540c\u65f6\u4e5f\u4f34\u968f\u7740\u97e7\u6027\u7684\u5267\u70c8\u4e0b\u964d\u3002\u8fd9\u4e00\u4e16\u754c\u6027\u96be\u9898\u76ee\u524d\u8fd8\u6682\u65f6\u65e0&#8230;<\/p>\n","protected":false},"author":4237,"featured_media":111933,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[2554,16],"class_list":["post-111932","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-2554","tag-al"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/111932"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/4237"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=111932"}],"version-history":[{"count":11,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/111932\/revisions"}],"predecessor-version":[{"id":112008,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/111932\/revisions\/112008"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/111933"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=111932"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=111932"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=111932"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}