{"id":114038,"date":"2017-12-27T06:30:48","date_gmt":"2017-12-26T22:30:48","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=114038"},"modified":"2017-12-25T19:20:58","modified_gmt":"2017-12-25T11:20:58","slug":"%e5%ad%a6%e6%9c%af%e5%b9%b2%e8%b4%a7-%e5%a4%9a%e5%ad%94%e6%9d%90%e6%96%99%e4%b8%ad%e7%94%b5%e8%8d%b7%e5%8f%8a%e7%89%a9%e8%b4%a8%e4%bc%a0%e8%be%93","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=114038","title":{"rendered":"\u5b66\u672f\u5e72\u8d27 | \u591a\u5b54\u6750\u6599\u4e2d\u7535\u8377\u53ca\u7269\u8d28\u4f20\u8f93"},"content":{"rendered":"<p><strong>\u4e00<\/strong><strong>.<\/strong><strong>\u591a\u5b54\u6750\u6599\u5b9a\u4e49\u53ca\u5e94\u7528\u7b80\u4ecb<\/strong><\/p>\n<p>\u591a\u5b54\u6750\u6599\u662f\u4e00\u79cd\u7531\u76f8\u4e92\u8d2f\u901a\u6216\u5c01\u95ed\u7684\u5b54\u6d1e\u6784\u6210\u7f51\u7edc\u7ed3\u6784\u7684\u6750\u6599\uff0c\u5b54\u6d1e\u7684\u8fb9\u754c\u6216\u8868\u9762\u7531\u652f\u67f1\u6216\u5e73\u677f\u6784\u6210\u3002\u5178\u578b\u7684\u5b54\u7ed3\u6784\u6709\uff1a\u4e00\u79cd\u662f\u7531\u5927\u91cf\u591a\u8fb9\u5f62\u5b54\u5728\u5e73\u9762\u4e0a\u805a\u96c6\u5f62\u6210\u7684\u4e8c\u7ef4\u7ed3\u6784\uff1b\u7531\u4e8e\u5176\u5f62\u72b6\u7c7b\u4f3c\u4e8e\u8702\u623f\u7684\u516d\u8fb9\u5f62\u7ed3\u6784\u800c\u88ab\u79f0\u4e3a\u201c\u8702\u7a9d\u201d\u6750\u6599\uff1b\u66f4\u4e3a\u666e\u904d\u7684\u662f\u7531\u5927\u91cf\u591a\u9762\u4f53\u5f62\u72b6\u7684\u5b54\u6d1e\u5728\u7a7a\u95f4\u805a\u96c6\u5f62\u6210\u7684\u4e09\u7ef4\u7ed3\u6784\uff0c\u901a\u5e38\u79f0\u4e4b\u4e3a\u201c\u6ce1\u6cab\u201d\u6750\u6599\u3002\u5982\u679c\u6784\u6210\u5b54\u6d1e\u7684\u56fa\u4f53\u53ea\u5b58\u5728\u4e8e\u5b54\u6d1e\u7684\u8fb9\u754c\uff08\u5373\u5b54\u6d1e\u4e4b\u95f4\u662f\u76f8\u901a\u7684\uff09\uff0c\u5219\u79f0\u4e3a\u5f00\u5b54\uff1b\u5982\u679c\u5b54\u6d1e\u8868\u9762\u4e5f\u662f\u5b9e\u5fc3\u7684\uff0c\u5373\u6bcf\u4e2a\u5b54\u6d1e\u4e0e\u5468\u56f4\u5b54\u6d1e\u5b8c\u5168\u9694\u5f00\uff0c\u5219\u79f0\u4e3a\u95ed\u5b54\uff1b\u800c\u6709\u4e9b\u5b54\u6d1e\u5219\u662f\u534a\u5f00\u5b54\u534a\u95ed\u5b54\u7684\u3002<\/p>\n<p>\u591a\u5b54\u6750\u6599\u662f\u5f53\u524d\u6750\u6599\u79d1\u5b66\u4e2d\u53d1\u5c55\u8f83\u4e3a\u8fc5\u901f\u7684\u4e00\u79cd\u6750\u6599\uff0c\u7279\u522b\u662f\u5b54\u5f84\u5728\u7eb3\u7c73\u91cf\u7ea7\u7684\u591a\u5b54\u6750\u6599\uff0c\u5177\u6709\u8bb8\u591a\u72ec\u7279\u7684\u6027\u8d28\u548c\u8f83\u5f3a\u7684\u5e94\u7528\u6027\uff0c\u5f15\u8d77\u4e86\u6b27\u7f8e\u79d1\u5b66\u754c\u4ee5\u53ca\u5de5\u5546\u754c\u7684\u91cd\u89c6\u3002\u57281994\u5e74\u7684MRS\u4f1a\u8bae\u4e0a\uff0c\u4e0d\u5c11\u4f01\u4e1a\u62a5\u5bfc\u4e86\u5b83\u4eec\u5728\u591a\u5b54\u6750\u6599\u5b9e\u9645\u5e94\u7528\u65b9\u9762\u7684\u65b0\u8fdb\u5c55\u3002\u7f8e\u56fd\u80fd\u6e90\u90e8\u4e3a\u7528\u4e8e\u9009\u62e9\u900f\u8fc7\u819c\u5206\u79bb\u6280\u672f\u7684\u591a\u5b54\u6750\u6599\u7684\u8fdb\u4e00\u6b65\u7814\u7a76\u63d0\u4f9b\u4e86\u5de8\u989d\u8d44\u52a9\u5ddd\u3002\u591a\u5b54\u6750\u6599\u7684\u7814\u7a76\u8303\u56f4\u5f88\u5e7f\uff0c\u76ee\u524d\u7814\u7a76\u5f97\u8f83\u591a\u7684\u6709\u5404\u79cd\u65e0\u673a\u6c14\u51dd\u80f6\u3001\u6709\u673a\u6c14\u51dd\u80f6\u95ed\u3001\u591a\u5b54\u534a\u5bfc\u4f53\u6750\u6599\u3001\u591a\u5b54\u91d1\u5c5e\u6750\u6599\u7b49\u3002\u8fd9\u4e9b\u6750\u6599\u7684\u5171\u540c\u7279\u70b9\u662f\u5bc6\u5ea6\u5c0f\uff0c\u5b54\u6d1e\u7387\u9ad8\uff0c\u6bd4\u8868\u9762\u79ef\u5927\uff0c\u5bf9\u6c14\u4f53\u6709\u9009\u62e9\u6027\u900f\u8fc7\u4f5c\u7528\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-114039\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image001-1-1.jpg\" alt=\"\" width=\"500\" height=\"375\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image001-1-1.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image001-1-1-300x225.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe\u4e00 \u591a\u5b54\u6750\u6599\u793a\u4f8b<\/p>\n<p><strong>\u4e8c<\/strong><strong>.<\/strong><strong>\u591a\u5b54\u6750\u6599\u5206\u7c7b\u7279\u6027\u4e2d\u7684\u7535\u8377\u53ca\u7269\u8d28\u4f20\u8f93<\/strong><\/p>\n<p><span style=\"color: #ff0000;\"><strong>1.<\/strong><strong>\u673a\u68b0\u6027\u80fd<\/strong><\/span><\/p>\n<p>\u591a\u5b54\u6750\u6599\u5236\u5907\u7684\u96f6\u4ef6\uff0c\u80fd\u5728\u964d\u4f4e\u5bc6\u5ea6\u7684\u540c\u65f6\uff0c\u63d0\u9ad8\u5f3a\u5ea6\u548c\u521a\u5ea6\u7b49\u673a\u68b0\u6027\u80fd\u3002\u636e\u6d4b\u7b97\uff0c\u4f7f\u7528\u591a\u5b54\u6750\u6599\u5236\u9020\u7684\u98de\u673a\uff0c\u5728\u540c\u7b49\u673a\u68b0\u6027\u80fd\u6761\u4ef6\u4e0b\uff0c\u51c0\u8d28\u91cf\u5c06\u51cf\u8f7b\u4e00\u534a\u3002\u53e6\u5916\uff0c\u591a\u5b54\u6750\u6599\u5177\u6709\u8f83\u9ad8\u7684\u51b2\u51fb\u97e7\u6027\uff0c\u5e94\u7528\u4e8e\u6c7d\u8f66\u5de5\u4e1a\uff0c\u5c06\u6709\u6548\u964d\u4f4e\u4ea4\u901a\u4e8b\u6545\u7ed9\u4e58\u5ba2\u5e26\u6765\u7684\u4f24\u5bb3\u3002<\/p>\n<p>\u5e94\u8be5\u5c06\u591a\u5b54\u7ed3\u6784\u5bf9\u673a\u68b0\u6027\u80fd\u7684\u5f71\u54cd\u5206\u6210\u76f4\u63a5\u7684\u4e0e\u95f4\u63a5\u7684\u4e24\u79cd\u5f71\u54cd\u3002\u4f8b\u5982\u52a0\u5feb\uff08\u6216\u51cf\u7f13\uff09\u6269\u6563\u8fc7\u7a0b\uff0c\u5bf9\u76f8\u53d8\u7684\u4f5c\u7528\u8fd9\u7c7b\u5b54\u9699\u7684\u95f4\u63a5\u5f71\u54cd\u5728\u4e8e\u4f1a\u5f62\u6210\u67d0\u4e9b\u7ed3\u6784\u3002\u6c14\u5b54\u7684\u76f4\u63a5\u5f71\u54cd\u5219\u8868\u73b0\u4e3a\u6c14\u5b54\u7ec4\u7ec7\u7684\u7279\u6027\u4e0e\u673a\u68b0\u6027\u80fd\u4e4b\u95f4\u7684\u5173\u7cfb\u3002\u901a\u8fc7\u4f7f\u7528\u5355\u76f8\u7684\u6750\u6599\u53ef\u4ee5\u533a\u5206\u5f00\u6c14\u5b54\u7684\u76f4\u63a5\u5f71\u54cd\u4e0e\u95f4\u63a5\u5f71\u54cd\u3002<\/p>\n<p>\u300a\u591a\u5b54\u6750\u6599\u7684\u673a\u68b0\u6027\u80fd\u300b\u6587\u732e\u4e2d\u63d0\u5230\uff0c\u5bf9\u5404\u79cd\u724c\u53f7\u7684\u5de5\u4e1a\u94c1\u7c89\u8fdb\u884c\u8bd5\u9a8c\u540e\u7684\u7ed3\u679c\u8868\u660e\uff0c\u968f\u7740\u4f34\u751f\u6742\u8d28\u6d53\u5ea6\u7684\u51cf\u5c11\uff0cKIC\u76f8\u5173\u5ea6\u7684\u6700\u5c0f\u503c\u4e0e\u6700\u5927\u503c\u662f\u5411\u7740\u66f4\u4f4e\u5b54\u9699\u7387\u7684\u65b9\u5411\u53d8\u52a8\u7684\uff0c\u4f46\u4e0d\u80fd\u6210\u529f\u533a\u5206\u4e0a\u8ff0\u56e0\u7d20\u7684\u5f71\u54cd\u3002\u5bf9\u6240\u6709\u7684\u5b54\u9699\u7387\u503c\u6765\u8bf4\uff0c\u94c1\u8bd5\u6837\u7684\u65ad\u53e3\u5747\u662f\u6676\u5185\u7684\uff0c\u800c\u5728\u7834\u574f\u8868\u9762\u4e0a\u7684\u6700\u5927\u7834\u65ad\u7387\u4e0e\u6700\u5c0f\u7684\u6297\u88c2\u6027\u76f8\u5bf9\u5e94\u3002\u6240\u83b7\u5f97\u7684\u7ed3\u679c\u66fe\u4e88\u4ee5\u89e3\u8bfb\u3002\u6839\u636e\u6c14\u5b54\u5747\u5177\u6709\u5706\u7403\u5f62\u72b6\u548c\u5747\u5300\u5206\u5e03\u7684\u5047\u8bbe\u51fa\u53d1\uff0c\u88c2\u7eb9\u5728\u6c14\u5b54\u95f4\u7a7f\u8fc7\u65f6\u4f1a\u8c61\u5f39\u6027\u7ea4\u7ef4\u4e00\u6837\u53d1\u751f\u7eaf\u5316\u4e0e\u5f2f\u66f2\u3002\u5b9e\u9a8c\u8868\u660e\u6709\u53ef\u80fd\u7531\u4e8e\u6c14\u5b54\u800c\u963b\u6b62\u4e86\u88c2\u7eb9\u5728\u94c1\u4e2d\u7684\u6269\u5c55\u3002\u540c\u65f6\u8bc1\u660e\uff0c\u9664\u4e86\u4e00\u822c\u7684\u5b54\u9699\u7387\u5916\u8fd8\u5fc5\u987b\u8003\u8651\u5176\u4ed6\u7684\u591a\u5b54\u7ed3\u6784\u7684\u7279\u6027\uff0c\u5728\u6b64\u60c5\u51b5\u4e0b\u5bf9\u4e8e\u540c\u6837\u7684\u7403\u5f62\u5b54\u9699\u3002<\/p>\n<p><span style=\"color: #ff0000;\"><strong>2.\u5438\u9644\u6027\u80fd<\/strong><\/span><\/p>\n<p>\u4e0d\u540c\u6c14\u4f53\u6216\u6db2\u4f53\u7684\u5206\u5b50\u76f4\u5f84\u53ca\u70ed\u8fd0\u52a8\u81ea\u7531\u5ea6\u5404\u4e0d\u76f8\u540c\uff0c\u56e0\u6b64\uff0c\u53ef\u5229\u7528\u540c\u7c7b\u591a\u5b54\u6750\u6599\u5bf9\u4e0d\u540c\u6c14\u4f53\u6216\u6db2\u4f53\u5438\u9644\u80fd\u529b\u7684\u5dee\u5f02\u7279\u6027\uff0c\u5236\u5907\u51fa\u7528\u4e8e\u51c0\u5316\u6c14\u4f53\u6216\u6db2\u4f53\u4e14\u53ef\u91cd\u590d\u4f7f\u7528\u7684\u9ad8\u6548\u591a\u5b54\u5438\u9644\u51c0\u5316\u6750\u6599\u3002\u4e0d\u540c\u7684\u5b54\u6750\u6599\u5bf9\u6c2e\u6c14\u5438\u9644\u7684\u80fd\u529b\u4e0d\u540c\uff0c\u5728\u65e5\u5e38\u751f\u4ea7\u751f\u6d3b\u4e2d\u7684\u5e94\u7528\u4e5f\u4e0d\u4e00\u6837\u3002\u6362\u53e5\u8bdd\u8bf4\uff0c\u4e0d\u540c\u7684\u5e94\u7528\u8981\u6c42\u5b54\u6750\u6599\u6709\u4e0d\u540c\u7684\u7279\u6027\u3002\u5fae\u5b54\u6cb8\u77f3\u5206\u5b50\u7b5b\u3001\u4ecb\u5b54\u6750\u6599\u3001\u591a\u7ea7\u5b54\u6750\u6599\u548c\u591a\u5b54\u82b3\u9999\u9aa8\u67b6\uff08PAF\uff09\u6750\u6599\u6709\u5404\u81ea\u7684\u7279\u6027\uff0c\u4e5f\u662f\u56e0\u4e3a\u5176\u7ed3\u6784\u548c\u7279\u6027\u4e0d\u540c\u800c\u5e94\u7528\u5230\u65e5\u5e38\u751f\u6d3b\u7684\u5404\u4e2a\u9886\u57df\u4e2d\u7684\u3002\u6bd4\u5982\u5fae\u5b54\u6cb8\u77f3\u5206\u5b50\u7b5b\u4ee5\u5176\u89c4\u5219\u7684\u5b54\u9053\u7ed3\u6784\u548c\u5c3a\u5bf8\u3001\u8f83\u5f3a\u7684\u5438\u9644\u80fd\u529b\u548c\u8f83\u9ad8\u7684\u50ac\u5316\u6027\u80fd\uff0c\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u77f3\u6cb9\u50ac\u5316\u3001\u73af\u5883\u4fdd\u62a4\u3001\u7cbe\u7ec6\u5316\u5de5\u7b49\u9886\u57df\u3002\u4ecb\u5b54\u6750\u6599\u4ee5\u5176\u8f83\u7a84\u7684\u5b54\u5f84\u5206\u5e03\u3001\u8f83\u89c4\u5219\u7684\u5b54\u9053\u6392\u5217\u987a\u5e8f\u4ee5\u53ca\u8f83\u5927\u7684\u6bd4\u8868\u9762\u79ef\u4e3a\u57fa\u7840\uff0c\u5728\u5927\u5206\u5b50\u50ac\u5316\u53cd\u5e94\u4e2d\u662f\u826f\u597d\u7684\u50ac\u5316\u5242\u53ca\u50ac\u5316\u5242\u8f7d\u4f53\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-114040\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image002-1.png\" alt=\"\" width=\"513\" height=\"322\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image002-1.png 513w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image002-1-300x188.png 300w\" sizes=\"(max-width: 513px) 100vw, 513px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe\u4e8c \u591a\u5b54\u6cb9\u6599\u78b3\u5438\u9644\u6750\u6599\u5236\u5907\u548c\u5e94\u7528\u6280\u672f<\/p>\n<p>\u300a\u5e94\u7528\u5c42\u72b6\u7845\u9178\u76d0\u77ff\u7269\u5236\u5907\u591a\u5b54\u6750\u6599\u53ca\u5176\u5438\u9644\u6027\u80fd\u7814\u7a76\u300b\u6587\u7ae0\u4e2d\u7684\u5438\u9644\u673a\u7406\u8bf4\u660e\u4e86\u591a\u5b54\u6750\u6599\u5438\u9644\u6027\u80fd\u4e2d\u7684\u7535\u8377\u548c\u7269\u8d28\u4f20\u8f93\u3002\u7406\u8bba\u8ba8\u8bba\u4e86\u6c27\u5316\u7269\u77ff\u7269\u5bf9\u91cd\u91d1\u5c5e\u79bb\u5b50\u7684\u4e13\u6027\u5438\u9644\uff0c\u8ba4\u4e3a\u5bf9\u91cd\u91d1\u5c5e\u79bb\u5b50\u8d77\u4e13\u6027\u5438\u9644\u4f5c\u7528\u7684\u662f\u77ff\u7269\u7684\u53ef\u53d8\u7535\u8377\u8868\u9762\u3002\u94c1\u3001\u94dd\u7b49\u65e0\u5b9a\u5f62\u6c34\u5408\u6c27\u5316\u7269\u548c\u6c22\u6c27\u5316\u7269\u7684\u8868\u9762\u7531\u91d1\u5c5e\u79bb\u5b50\u548c\u8f7b\u57fa\u7ec4\u6210\uff0c\u5177\u6709\u4eb2\u6c34\u6027\u6027\u548c\u8def\u6613\u65af\u9178\u78b1\u884c\u4e3a\uff0c\u66b4\u9732\u5728\u8868\u9762\u4e0a\u7684\u8f7b\u57fa\u4f1a\u901a\u8fc7\u89e3\u79bb\u548c\u7f14\u5408\u800c\u5e26\u6709\u4e00\u5b9a\u91cf\u7684\u8868\u9762\u7535\u8377\uff0c\u7535\u8377\u91cf\u4f1a\u968f\u4ecb\u8d28\u7684\u503c\u800c\u53d8\u5316\u3002\u53ef\u53d8\u7535\u8377\u8868\u9762\u5bf9\u91cd\u91d1\u5c5e\u79bb\u5b50\u7684\u5438\u9644\u4f5c\u7528\u4e0e\u4ea4\u6362\u6027\u5438\u9644\u4e0d\u540c\uff0c\u5728\u53ef\u53d8\u7535\u8377\u8868\u9762\u91cd\u91d1\u5c5e\u79bb\u5b50\u80fd\u8fdb\u5165\u77ff\u7269\u7684\u91d1\u5c5e\u539f\u5b50\u914d\u4f4d\u58f3\u4e2d\u4e0e\u6c22\u6c27\u914d\u4f4d\u57fa\u56e2\u8fdb\u884c\u4ea4\u6362\uff0c\u901a\u8fc7\u5171\u4ef7\u952e\u6216\u914d\u4f4d\u952e\u7ed3\u5408\u5728\u56fa\u4f53\u8868\u9762\uff0c\u578b\u5c42\u72b6\u7845\u9178\u76d0\u77ff\u7269\u8fb9\u7f18\u88f8\u9732\u7684\u94dd\u9187\u3001\u94c1\u9187\u548c\u7845\u70f7\u9187\u4ee5\u53ca\u578b\u5c42\u72b6\u7845\u9178\u76d0\u77ff\u7269\u7684\u8f7b\u57fa\u94dd\u5c42\u57fa\u9762\u548c\u7845\u6c27\u70f7\u57fa\u9762\u4e0a\u7531\u65ad\u952e\u4ea7\u751f\u7684\u7845\u70f7\u9187\u5747\u5c5e\u6b64\u7c7b\u914d\u4f4d\u57fa\u56e2\u3002\u9664\u4e86\u4e13\u6027\u5438\u9644\u5916\u8fd8\u5b58\u5728\u4ea4\u6362\u6027\u5438\u9644\uff0c\u5c42\u72b6\u7845\u9178\u76d0\u7ed3\u6784\u4e2d\u5e7f\u6cdb\u5b58\u5728\u7740\u7c7b\u8d28\u540c\u8c61\u7f6e\u6362\u4f7f\u5176\u5e26\u6709\u4e00\u5b9a\u91cf\u7684\u8868\u9762\u51c0\u8d1f\u7535\u8377\uff0c\u5b83\u901a\u8fc7\u9759\u7535\u4f5c\u7528\u5438\u9644\u91cd\u91d1\u5c5e\u79bb\u5b50\uff0c\u5728\u4e00\u5b9a\u7a0b\u5ea6\u4e0a\uff0c\u5176\u5438\u9644\u5bb9\u91cf\u4e0e\u4ea4\u6362\u4f5c\u7528\u5177\u6709\u66f4\u5bc6\u5207\u7684\u5173\u7cfb\u3002\u7814\u7a76\u6240\u5f97\u591a\u5b54\u6c27\u5316\u94dd\u6750\u6599\u7531\u4e8e\u7ed3\u6784\u7834\u574f\uff0c\u6c27\u5316\u7845\u88ab\u6d3b\u5316\u78b1\u6d78\u4ece\u800c\u5f15\u8fdb\u5927\u91cf\u6c22\u6c27\u914d\u4f4d\u57fa\u56e2\uff0c\u65e2\u53ef\u4ee5\u4e0e\u91cd\u91d1\u5c5e\u79bb\u5b50\u4ea4\u6362\u5438\u9644\uff0c\u53c8\u53ef\u80fd\u5f15\u8d77\u4e00\u90e8\u5206\u91cd\u91d1\u5c5e\u79bb\u5b50\u5728\u8868\u9762\u548c\u5b54\u7ed3\u6784\u4e2d\u5f62\u6210\u6c89\u6dc0\uff0c\u4ece\u800c\u63d0\u9ad8\u5438\u9644\u91cf\u3002<\/p>\n<p><span style=\"color: #ff0000;\"><strong>3.\u6e17\u900f\u6027\u80fd<\/strong><\/span><\/p>\n<p>\u5728\u6750\u6599\u5236\u5907\u8fc7\u7a0b\u4e2d\uff0c\u901a\u8fc7\u63a7\u5236\u5b54\u9053\u5c3a\u5bf8\u3001\u65b9\u5411\u3001\u5b54\u578b\u53ca\u6392\u5217\u89c4\u5f8b\u7b49\u7ed3\u6784\u7279\u5f81\uff0c\u7ed3\u5408\u591a\u5b54\u6750\u6599\u8010\u70ed\u6027\u597d\uff0c\u7ed3\u6784\u7a33\u5b9a\u6027\u9ad8\u7b49\u56fa\u6709\u7279\u6027\uff0c\u53ef\u5236\u5907\u51fa\u591a\u5b54\u5206\u5b50\u7b5b\u3001\u9ad8\u6e29\u6c14\u4f53\u5206\u79bb\u819c\u7b49\u8fc7\u6ee4\u88c5\u7f6e\u3002<\/p>\n<p>\u6587\u732e\u62a5\u9053\uff0c\u5f53\u591a\u5b54\u6750\u6599\u7684\u5b54\u9699\u5ea6\u8303\u56f4\u4e3a57-95%\u65f6\uff0c\u7c98\u6027\u6e17\u900f\u7cfb\u6570\u4e0e\u60ef\u6027\u6e17\u900f\u7cfb\u6570\u5747\u968f\u5b54\u9699\u5ea6\u7684\u63d0\u9ad8\u663e\u8457\u589e\u5927\uff1b\u5f53\u591a\u5b54\u6750\u6599\u7684\u5c3a\u5bf8\u8303\u56f4\u4e3a10-40PPI\u65f6\uff0c\u7c98\u6027\u6e17\u900f\u7cfb\u6570\u4e0e\u60ef\u6027\u6e17\u900f\u7cfb\u6570\u53c8\u5747\u968f\u5b54\u5c3a\u5bf8\u7684\u589e\u5927\u800c\u663e\u8457\u63d0\u9ad8\u3002\u5b54\u5f84\u964d\u4f4e\u65f6\uff0c\u4f53\u79ef\u6bd4\u8868\u9762\u79ef\u589e\u5927\uff0c\u6d41\u4f53\u963b\u529b\u589e\u5927\uff0c\u7c98\u5ea6\u6e17\u900f\u7cfb\u6570\u51cf\u5c0f\uff1b\u5b54\u5f84\u964d\u4f4e\u65f6\uff0c\u76f8\u540c\u538b\u529b\u4e0b\u6d41\u4f53\u901a\u8fc7\u591a\u5b54\u6750\u6599\u7684\u6d41\u901f\u964d\u4f4e\uff0c\u6d41\u4f53\u60ef\u6027\u80fd\u91cf\u635f\u5931\u51cf\u5c0f\uff0c\u60ef\u6027\u6d17\u6f31\u53d8\u5c0f\u3002<\/p>\n<p><span style=\"color: #ff0000;\"><strong>4.\u5149\u7535\u6027\u80fd<\/strong><\/span><\/p>\n<p>\u591a\u5b54\u7845\u6750\u5728\u6fc0\u5149\u7167\u5c04\u4e0b\u53ef\u53d1\u51fa\u53ef\u89c1\u5149\uff0c\u6839\u636e\u8fd9\u4e00\u7279\u6027\uff0c\u88ab\u8ba4\u4e3a\u662f\u65b0\u578b\u5149\u7535\u5b50\u5143\u4ef6\u7684\u7406\u60f3\u6750\u6599\u3002\u540c\u65f6\uff0c\u591a\u5b54\u6750\u6599\u4e5f\u88ab\u8ba4\u4e3a\u662f\u672a\u6765\u6df7\u5408\u52a8\u529b\u6c7d\u8f66\u65b0\u578b\u71c3\u6599\u7535\u6c60\u4e2d\u7535\u6781\u6750\u6599\u7684\u9996\u9009\u3002\u8fd1\u5e74\u6765\u7814\u7a76\u8868\u660e\uff1a\u7535\u6781\u6d3b\u6027\u6750\u6599\u7684\u5b54\u5f84\u3001\u5b54\u7ed3\u6784\u3001\u5b54\u5206\u5e03\u4ee5\u53ca\u5b54\u58c1\u539a\u5ea6\u7b49\u80fd\u591f\u5728\u5f88\u5927\u7a0b\u5ea6\u4e0a\u5f71\u54cd\u7535\u89e3\u6db2\u7684\u6d78\u6da6\u3001\u79bb\u5b50\u7684\u4f20\u8f93\u4ee5\u53ca\u79bb\u5b50\u5728\u6d3b\u6027\u7684\u7269\u8d28\u6676\u4f53\u4e2d\u7684\u6269\u6563\uff0c\u4ece\u800c\u5f71\u54cd\u7535\u6781\u7684\u6574\u4f53\u6027\u80fd\uff0c\u591a\u5b54\u6750\u6599\u5728\u7535\u5316\u5b66\u80fd\u91cf\u8f6c\u6362\u548c\u5b58\u50a8\u4e2d\u7684\u5e94\u7528\u5df2\u7ecf\u6210\u4e3a\u65b0\u5174\u7684\u8bfe\u9898\uff0c\u5e76\u5f15\u8d77\u4e86\u5e7f\u6cdb\u7684\u5173\u6ce8\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-114041\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image004-2.jpg\" alt=\"\" width=\"500\" height=\"203\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image004-2.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image004-2-300x122.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe\u4e09 \u591a\u5b54\u7ed3\u6784\u548c\u7c89\u672b\u7ed3\u6784BiVO4\u5149\u9633\u6781\u6750\u6599\u5149\u7535\u50ac\u5316\u673a\u7406\u793a\u610f\u56fe<\/p>\n<p>\u4ee5\u8d85\u7ea7\u7535\u5bb9\u5668\u4e3a\u4f8b\uff0c\u5408\u7406\u7684\u5b54\u5f84\u5206\u5e03\u5bf9\u4e8e\u63d0\u9ad8\u78b3\u57fa\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u6574\u4f53\u6027\u80fd\u5982\u50a8\u80fd\u80fd\u529b\u7684\u5927\u5c0f\u3001\u901f\u7387\u7a33\u5b9a\u6027\u548c\u5faa\u73af\u7a33\u5b9a\u6027\u7b49\u975e\u5e38\u91cd\u8981\u3002\u2014\u822c\u6765\u8bf4\uff0c\u7406\u60f3\u8d85\u7ea7\u7535\u5bb9\u5668\u78b3\u6750\u6599\u5e94\u540c\u65f6\u5177\u6709\u591a\u79cd\u7c7b\u578b\u7684\u5b54\uff0c\u5373\u5fae\u5b54\u3001\u4ecb\u5b54\u548c\u5927\u5b54\u3002\u8fd9\u4e9b\u4e0d\u540c\u7c7b\u578b\u7684\u5b54\u5728\u7535\u5316\u5b66\u53cc\u7535\u5c42\u7535\u5bb9\u5668\u4e2d\u8d77\u4e0d\u540c\u7684\u4f5c\u7528\u3002\u5fae\u5b54\u4e3b\u8981\u7528\u4e8e\u7535\u8377\u50a8\u5b58\uff0c\u56e0\u6b64\u5fae\u5b54\u8d8a\u591a\uff0c\u50a8\u80fd\u80fd\u529b\u8d8a\u5f3a\uff0c\u80fd\u91cf\u5bc6\u5ea6\u8d8a\u5927\uff1b\u4ecb\u5b54\u4e3b\u8981\u8d1f\u8d23\u7535\u89e3\u8d28\u7684\u4f20\u8f93\uff0c\u5f71\u54cd\u53cc\u7535\u5c42\u7535\u5bb9\u5668\u7684\u901f\u7387\u7a33\u5b9a\u6027\u548c\u5faa\u73af\u7a33\u5b9a\u6027\uff1b\u800c\u5927\u5b54\u5219\u4f5c\u4e3a\u79bb\u5b50\u6c60\u4e3a\u4ecb\u5b54\u548c\u5fae\u5b54\u63d0\u4f9b\u8db3\u591f\u7684\u7535\u89e3\u8d28\u79bb\u5b50\uff0c\u4e5f\u5f71\u54cd\u5230\u901f\u7387\u7a33\u5b9a\u6027\u548c\u5faa\u73af\u7a33\u5b9a\u6027\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-114042\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image005-1-1.jpg\" alt=\"\" width=\"500\" height=\"382\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image005-1-1.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image005-1-1-300x229.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe\u56db \u591a\u5b54\u6750\u6599\u5728\u8d85\u7ea7\u7535\u5bb9\u5668\u4e2d\u7684\u5e94\u7528<\/p>\n<p>\u5bf9\u4e8e\u9502\u79bb\u5b50\u7535\u6c60\u8d1f\u6781\u6750\u6599\u7684\u79cd\u7c7b\u6765\u8bf4\uff0c\u5176\u79cd\u7c7b\u4e3b\u8981\u53ef\u4ee5\u5206\u4e3a\u78b3\u6750\u6599\u8d1f\u6781\u548c\u975e\u78b3\u6750\u6599\u8d1f\u6781\u3002\u78b3\u8d1f\u6781\u6750\u6599\u4e3b\u8981\u5305\u62ec\u77f3\u58a8\u8d1f\u6781\u6750\u6599\u3001\u8f6f\u78b3\u6750\u6599\u3001\u786c\u78b3\u6750\u6599\u4ee5\u53ca\u4e00\u4e9b\u78b3\u590d\u5408\u6750\u6599\uff0c\u8fd9\u7c7b\u8d1f\u6781\u6210\u672c\u8f83\u4f4e\uff0c\u800c\u4e14\u5faa\u73af\u7a33\u5b9a\u6027\u8f83\u597d\uff0c\u5df2\u7ecf\u5f88\u597d\u7684\u5e94\u7528\u4e8e\u5de5\u4e1a\u4e2d\uff0c\u4f46\u662f\u7406\u8bba\u6bd4\u5bb9\u91cf\u8f83\u5c0f\uff0c\u5bfc\u7535\u6027\u4e0d\u592a\u597d\u3002\u4e3a\u4e86\u63d0\u9ad8\u8d1f\u6781\u6750\u6599\u7684\u6bd4\u5bb9\u91cf\uff0c\u5f88\u591a\u7684\u7814\u7a76\u8f6c\u79fb\u5230\u4e86\u4e00\u4e9b\u91d1\u5c5e\u6c27\u5316\u7269\uff0c\u8fd8\u6709\u4e00\u4e9b\u9502\u5408\u91d1\u3002\u8fd9\u4e9b\u6750\u6599\u62e5\u6709\u6bd4\u77f3\u58a8\u66f4\u9ad8\u7684\u6bd4\u5bb9\u91cf\uff0c\u4f46\u5728\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\uff0c\u6750\u6599\u81ea\u8eab\u4f1a\u53d1\u751f\u4e25\u91cd\u7684\u4f53\u79ef\u81a8\u80c0\uff0c\u4f7f\u5f97\u6750\u6599\u7ed3\u6784\u53d1\u751f\u7834\u574f\uff0c\u7535\u6c60\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u975e\u5e38\u5dee\uff0c\u963b\u788d\u4e86\u5176\u5de5\u4e1a\u5316\u751f\u4ea7\u3002Yu\u7b49\u901a\u8fc7\u5c06\u591a\u5b54\u4e8c\u6c27\u5316\u949b\u5fae\u7403\u9576\u5d4c\u5230\u4e86\u77f3\u58a8\u70ef\u57fa\u591a\u5b54\u6750\u6599\u4e2d\u5236\u5907\u4e86\u4e00\u79cd\u65b0\u578b\u7684\u7535\u6781\u6750\u6599(MTO\/3D-GN)\u3002\u8fd9\u79cd\u6750\u6599\u5177\u6709\u4f18\u5f02\u7684\u7535\u5316\u5b66\u6027\u80fd\uff0c\u572820C\u7684\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u53ef\u9006\u6bd4\u5bb9\u91cf\u9ad8\u8fbe124mAh\/g\u3002\u8fd9\u79cd\u6750\u6599\u7684\u5faa\u73af\u6027\u80fd\u548c\u500d\u7387\u6027\u80fd\u4e5f\u90fd\u662f\u4f18\u4e8e\u5355\u7eaf\u7684\u4e8c\u6c27\u5316\u949b\u6750\u6599\u3002\u8fd9\u91cc\u7684\u53cd\u5e94\u673a\u7406\u53ef\u4ee5\u89e3\u91ca\u4e3a\uff1a\u4e09\u7ef4\u7684\u77f3\u58a8\u70ef\u57fa\u591a\u5b54\u6750\u6599(3D-GN)\u4e3a\u7535\u6781\u6750\u6599\u548c\u7535\u89e3\u6db2\u63d0\u4f9b\u4e86\u5927\u7684\u63a5\u89e6\u9762\u79ef\u3001\u52a0\u5feb\u4e86\u7535\u5b50\u548c\u9502\u79bb\u5b50\u7684\u4f20\u8f93\u901f\u5ea6\u4ee5\u53ca\u4e3a\u7535\u5316\u5b66\u53cd\u5e94\u8fc7\u7a0b\u4e2d\u4e8c\u6c27\u5316\u949b\u7684\u4f53\u79ef\u53d8\u5316\u63d0\u4f9b\u4e86\u53cc\u91cd\u4fdd\u62a4\uff0c\u6700\u4e3b\u8981\u7684\u662f\u7535\u5316\u5b66\u8fc7\u7a0b\u4e2d\u6574\u4e2a\u7535\u6781\u6750\u6599\u7684\u7684\u5bfc\u7535\u6027\u5f97\u5230\u4e86\u63d0\u9ad8\u3002Cao\u7b49\u901a\u8fc7\u5c06\u4e8c\u786b\u5316\u94bc\u6c89\u79ef\u5728\u591a\u5b54\u77f3\u58a8\u70ef\u9aa8\u67b6\u7684\u8868\u9762\u4e0a\u5236\u5907\u4e86\u4e00\u79cd\u4e0d\u9700\u8981\u7c98\u7ed3\u5242\u7684\u9502\u79bb\u5b50\u7535\u6c60\u7535\u6781\u6750\u6599\uff0c\u8fd9\u79cd\u6750\u6599\u62e5\u6709\u4f18\u5f02\u7684\u7535\u5316\u5b66\u6027\u80fd\u3002\u6b64\u5916\uff0c\u77f3\u58a8\u70ef\u57fa\u591a\u5b54\u6750\u6599\u63d0\u4f9b\u7684\u76f8\u4e92\u8d2f\u7a7f\u7684\u5b54\u9053\u7ed3\u6784\u80fd\u591f\u6709\u5229\u4e8e\u7535\u5b50\u548c\u9502\u79bb\u5b50\u7684\u6269\u6563\u548c\u8f6c\u79fb\uff0c\u6709\u6548\u5730\u51cf\u5c11\u4f20\u9012\u8def\u5f84\uff0c\u8fd9\u6837\u4e5f\u5c31\u4e0d\u9700\u8981\u63d0\u4f9b\u5176\u4ed6\u7684\u5bfc\u7535\u5242\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-114043\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image006.png\" alt=\"\" width=\"445\" height=\"240\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image006.png 445w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image006-300x162.png 300w\" sizes=\"(max-width: 445px) 100vw, 445px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe\u4e94 \u591a\u5b54\u6750\u6599\u5728\u9502\u7535\u6c60\u4e2d\u7684\u5e94\u7528<\/p>\n<p>\u5bf9\u4e8e\u4f20\u611f\u5668\u6765\u8bf4\uff0c\u591a\u5b54\u6750\u6599\u4e0e\u751f\u8272\u57fa\u56e2\u4e4b\u95f4\u6709\u8f83\u5f3a\u7684\u534f\u540c\u6548\u5e94\u4ee5\u53ca\u5b83\u5177\u6709\u8f83\u9ad8\u7684\u6bd4\u8868\u9762\u79ef\u80fd\u591f\u63d0\u9ad8\u4e0e\u88ab\u68c0\u6d4b\u7269\u8d28\u7684\u63a5\u89e6\u9762\u79ef\uff0c\u8fd9\u4f7f\u5f97\u5b83\u5728\u4f20\u611f\u5668\u9886\u57df\u7684\u5e94\u7528\u5177\u6709\u5de8\u5927\u7684\u4f18\u52bf\u3002\u6b64\u5916\uff0c\u77f3\u58a8\u70ef\u57fa\u591a\u5b54\u6750\u6599\u7684\u7535\u963b\u7387\u975e\u5e38\u4f4e\uff0c\u7535\u5b50\u5728\u8fde\u7eed\u7684\u548c\u76f8\u4e92\u8d2f\u7a7f\u7684\u9aa8\u67b6\u4e0a\u7684\u4f20\u8f93\u901f\u5ea6\u975e\u5e38\u5feb\uff0c\u8fd9\u53ef\u4ee5\u6781\u5927\u5730\u63d0\u9ad8\u4f20\u611f\u5668\u7684\u7075\u654f\u5ea6\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-114044\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image008-2.jpg\" alt=\"\" width=\"480\" height=\"338\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image008-2.jpg 480w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2017\/11\/image008-2-300x211.jpg 300w\" sizes=\"(max-width: 480px) 100vw, 480px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe\u516d \u591a\u5b54\u6750\u6599\u5728\u4f20\u611f\u5668\u4e2d\u7684\u5e94\u7528<\/p>\n<p><strong>\u53c2\u8003\u6587\u732e<\/strong><\/p>\n<p>1.\u7eb3\u7c73\u6750\u6599\u7ed3\u6784\u8c03\u63a7\u5bf9\u7535\u8377\u4f20\u8f93\u548c\u50a8\u5b58\u6027\u80fd\u7684\u5f71\u54cd. \u8d75\u632f\u73af\uff0c\u5c71\u4e1c\u5927\u5b66\uff0c2015\u5e74.<\/p>\n<p>2.\u591a\u5b54\u6750\u6599\u7684\u5236\u5907\u53ca\u5176\u5728\u7535\u5316\u5b66\u4f20\u611f\u5668\u4e2d\u7684\u5e94\u7528. \u6768\u6d77\u9759\uff0c\u4e1c\u5317\u5e08\u8303\u5927\u5b66\uff0c2012\u5e74.<\/p>\n<p>3.\u8d85\u7ea7\u7535\u5bb9\u5668\u7528\u78b3\u8d28\u591a\u5b54\u6750\u6599\u7684\u5236\u5907\u53ca\u5176\u7535\u5316\u5b66\u6027\u80fd. \u5510\u4e3d\uff0c\u534e\u4e1c\u7406\u5de5\u5927\u5b66\uff0c2011\u5e74.<\/p>\n<p>4.\u57fa\u4e8e\u77f3\u58a8\u70ef\u7684\u529f\u80fd\u591a\u5b54\u6750\u6599\u7684\u5236\u5907\u53ca\u5176\u6027\u80fd\u7814\u7a76. \u6768\u5168\u80dc\uff0c\u71d5\u5c71\u5927\u5b66\uff0c2016\u5e74.<\/p>\n<p>5.\u591a\u5b54\u6750\u6599\u7684\u673a\u68b0\u6027\u80fd. \u0410.\u0410.\u0428\u0430\u0446\u043e\uff0c\u56fd\u5916\u673a\u8f66\u8f66\u8f86\u5de5\u827a\uff0c2005\u5e74.<\/p>\n<p>6.\u591a\u5b54\u6750\u6599\u7684\u591a\u79cd\u5438\u9644\u6027\u80fd\u7684\u7814\u7a76. \u9648\u6625\u5f71\uff0c\u5409\u6797\u5927\u5b66\uff0c2012\u5e74.<\/p>\n<p>7.\u5e94\u7528\u5c42\u72b6\u7845\u9178\u76d0\u77ff\u7269\u5236\u5907\u591a\u5b54\u6750\u6599\u53ca\u5176\u5438\u9644\u6027\u80fd\u7814\u7a76. \u7a0b\u4f1f\uff0c\u4e2d\u5357\u5927\u5b66\uff0c2011\u5e74.<\/p>\n<p>8.\u91d1\u5c5e\u591a\u5b54\u6750\u6599\u6e17\u900f\u6027\u80fd\u7814\u7a76\u73b0\u72b6. \u8bb8\u4f69\u654f\uff0c\u529f\u80fd\u6750\u6599\uff0c2010\u5e74.<\/p>\n<p>9.\u591a\u5b54\u78b3\u6750\u6599\u7684\u5408\u6210\u53ca\u5176\u5728\u9502\u79bb\u5b50\u7535\u6c60\u8d1f\u6781\u4e2d\u7684\u5e94\u7528. \u97e9\u6c9b\uff0c\u6df1\u5733\u5927\u5b66.<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u5b66\u672f\u5e72\u8d27\u7ec4Jane915126\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u5b66\u672f\u5e72\u8d27\u81f4\u529b\u4e8e\u6210\u4e3a\u5e7f\u5927\u6750\u6599\u4eba\u8bfb\u8005\u9ad8\u6548\u83b7\u53d6\u77e5\u8bc6\u7684\u9014\u5f84\uff0c\u4e3a\u4e86\u66f4\u8d34\u5408\u5927\u4f17\u77e5\u8bc6\u9700\u6c42\uff0c\u73b0\u5411\u5927\u5bb6\u5f81\u96c6\u5e72\u8d27\u5199\u4f5c\u65b9\u5411\u3002\u5982\u679c\u4f60\u60f3\u4e86\u89e3\u54ea\u4e2a\u9886\u57df\u7684\u77e5\u8bc6\uff0c\u67d0\u4e2a\u8f6f\u4ef6\u7684\u5e94\u7528\u6216\u8005\u4efb\u4f55\u6709\u8da3\u7684\u60f3\u6cd5\u548c\u601d\u7ef4\u65b9\u5411\uff0c\u8bf7\u5728\u5fae\u4fe1\u4e0b\u65b9\u7559\u8a00\u677f\u7559\u8a00\uff0c\u6211\u4eec\u4f1a\u6536\u96c6\u5e76\u63a8\u51fa\u5927\u5bb6\u9700\u6c42\u7684\u5b66\u672f\u5e72\u8d27\uff0c\u6709\u5efa\u8bbe\u6027\u7684\u610f\u89c1\u6216\u8005\u60f3\u6cd5\u4e00\u7ecf\u91c7\u7eb3\uff0c\u6211\u4eec\u5c06\u63d0\u4f9b\u795e\u79d8\u5956\u52b1\u3002\u5feb\u5feb\u7559\u8a00\u5427\uff01\uff01<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u5411\u5404\u5927\u56e2\u961f\u8bda\u5fc3\u7ea6\u7a3f\uff0c\u8bfe\u9898\u7ec4\u6700\u65b0\u6210\u679c\u3001\u65b9\u5411\u603b\u7ed3\u3001\u56e2\u961f\u8bbf\u8c08\u3001\u5b9e\u9a8c\u6280\u80fd\u7b49\u7686\u53ef\u6295\u7a3f\uff0c\u8bf7\u8054\u7cfb\uff1a\u90ae\u7bb1tougao@cailiaoren.com \u6216 QQ\uff1a97482208\u3002<\/p>\n<p><strong>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c\u627e<\/strong><a href=\"http:\/\/www.cailiaoniu.com\/\"><strong>\u6750\u6599\u4eba<\/strong><\/a><strong>\u3001<\/strong><a href=\"http:\/\/www.ceshigu.com\/\"><strong>\u4e0a\u6d4b\u8bd5\u8c37<\/strong><\/a><strong>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e00.\u591a\u5b54\u6750\u6599\u5b9a\u4e49\u53ca\u5e94\u7528\u7b80\u4ecb \u591a\u5b54\u6750\u6599\u662f\u4e00\u79cd\u7531\u76f8\u4e92\u8d2f\u901a\u6216\u5c01\u95ed\u7684\u5b54\u6d1e\u6784\u6210\u7f51\u7edc\u7ed3\u6784\u7684\u6750\u6599\uff0c\u5b54\u6d1e\u7684\u8fb9\u754c\u6216\u8868\u9762\u7531\u652f\u67f1\u6216\u5e73\u677f\u6784\u6210\u3002\u5178\u578b\u7684\u5b54\u7ed3\u6784\u6709\uff1a\u4e00\u79cd\u662f\u7531\u5927\u91cf\u591a\u8fb9\u5f62\u5b54\u5728\u5e73\u9762&#8230;<\/p>\n","protected":false},"author":369,"featured_media":114039,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[54],"class_list":["post-114038","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-ganhuo","tag-making"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/114038"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/369"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=114038"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/114038\/revisions"}],"predecessor-version":[{"id":119084,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/114038\/revisions\/119084"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/114039"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=114038"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=114038"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=114038"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}