{"id":121614,"date":"2018-01-16T06:30:38","date_gmt":"2018-01-15T22:30:38","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=121614"},"modified":"2018-01-15T23:35:43","modified_gmt":"2018-01-15T15:35:43","slug":"%e4%b8%9c%e5%8d%8e%e5%a4%a7%e5%ad%a6%e4%b8%81%e5%bd%acadv-mater-%e6%b7%b7%e5%90%88%e7%a6%bb%e5%ad%90-%e7%94%b5%e5%ad%90%e5%af%bc%e4%bd%93%e7%94%a8%e4%ba%8e%e9%94%82%e9%87%91%e5%b1%9e%e8%b4%9f","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=121614","title":{"rendered":"\u4e1c\u534e\u5927\u5b66\u4e01\u5f6cAdv. Mater.: \u6df7\u5408\u79bb\u5b50-\u7535\u5b50\u5bfc\u4f53\u7528\u4e8e\u9502\u91d1\u5c5e\u8d1f\u6781\u4fdd\u62a4"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u7531\u4e8e\u9502\u91d1\u5c5e\u8d1f\u6781\u5177\u6709\u8f83\u9ad8\u7684\u7406\u8bba\u5bb9\u91cf\uff083840 mA h g<sup>-1<\/sup>\uff09\u548c\u6700\u4f4e\u7684\u7535\u5316\u5b66\u7535\u4f4d\uff08-3.04 V vs SHE\uff09\uff0c\u56e0\u6b64\uff0c\u8fd1\u5e74\u6765\u5bf9\u53ef\u5145\u7535\u9502\u91d1\u5c5e\u7535\u6c60\u8fdb\u884c\u4e86\u5e7f\u6cdb\u7684\u7814\u7a76\u3002\u4f46\u662f\uff0c\u5728\u6db2\u4f53\u7535\u89e3\u8d28\u4f53\u7cfb\u4e2d\uff0c\u9502\u679d\u6676\u7684\u751f\u957f\u548c\u9502\u91d1\u5c5e\u8d1f\u6781\u8150\u8680\u4f7f\u5f97\u9502\u91d1\u5c5e\u7535\u6c60\u7684\u53d1\u5c55\u9762\u4e34\u7740\u4e25\u91cd\u7684\u5b89\u5168\u95ee\u9898\u3002\u5728\u9502\u91d1\u5c5e\u7535\u6c60\u4e2d\uff0c\u9502\u679d\u6676\u7684\u751f\u957f\u4e3b\u8981\u662f\u7531\u5faa\u73af\u8fc7\u7a0b\u4e2d\u9502\u79bb\u5b50\u7684\u6d53\u5ea6\u68af\u5ea6\u548c\u9502\u6c89\u79ef\u65f6\u8d1f\u6781\u8868\u9762\u4e0d\u5747\u5300\u5f15\u8d77\u7684\u3002\u800c\u9502\u91d1\u5c5e\u4e0e\u4efb\u4f55\u6709\u673a\u6eb6\u5242\u5728\u70ed\u529b\u5b66\u4e0a\u90fd\u662f\u4e0d\u7a33\u5b9a\u7684\uff0c\u4f1a\u77ac\u95f4\u53d1\u751f\u53cd\u5e94\u5f62\u6210\u65b0\u7684\u949d\u5316\u5c42\uff1b\u56e0\u6b64\uff0c\u4e00\u65e6\u9502\u679d\u6676\u7a7f\u900f\u56fa\u6001\u7535\u89e3\u8d28\u819c\uff08SEI\uff09\u5411\u5916\u751f\u957f\uff0c\u9502\u91d1\u5c5e\u8d1f\u6781\u5c06\u88ab\u7535\u89e3\u8d28\u8150\u8680\uff0c\u5bfc\u81f4\u7535\u6c60\u7684\u5e93\u4f26\u6548\u7387\u504f\u4f4e\u3002\u76ee\u524d\uff0c\u7814\u7a76\u4eba\u5458\u5df2\u7ecf\u5f00\u53d1\u51fa\u591a\u79cd\u624b\u6bb5\u7528\u4ee5\u4fdd\u62a4\u9502\u91d1\u5c5e\u8d1f\u6781\uff0c\u5982\uff1a\u901a\u8fc7\u9502\u91d1\u5c5e\u548c\u6db2\u4f53\u7535\u89e3\u8d28\u4e2d\u7684\u5316\u5b66\u6dfb\u52a0\u5242\u53cd\u5e94\u5f62\u6210SEI\u819c\uff0c\u6216\u901a\u8fc7\u5bfc\u7535\u91d1\u5c5e\u6846\u67b6\/\u78b3\u819c\u5728\u9502\u91d1\u5c5e\u8868\u9762\u5236\u5907\u4fdd\u5f62\u6d82\u5c42\u819c\u4ee5\u53ca\u4f7f\u7528\u4e0d\u5bfc\u7535\u7684\u56fa\u6001\u7535\u89e3\u8d28\u7b49\u3002\u4f46\u4e0a\u8ff0\u65b9\u6cd5\u4e2d\uff0cSEI\u819c\u65e0\u6cd5\u627f\u53d7\u9502\u679d\u6676\u9020\u6210\u7684\u65e0\u9650\u5236\u4f53\u79ef\u53d8\u5316\uff0c\u56e0\u6b64\u5728\u5faa\u73af\u8fc7\u7a0b\u4e2dSEI\u819c\u5c06\u4e0d\u65ad\u5730\u65ad\u88c2\/\u4fee\u590d\uff0c\u4ece\u800c\u5bfc\u81f4\u5e93\u4f26\u6548\u7387\u8f83\u4f4e\uff0c\u964d\u4f4e\u4e86\u7535\u6c60\u7684\u4f7f\u7528\u5bff\u547d\u3002\u5bfc\u7535\u91d1\u5c5e\u6846\u67b6\u6216\u78b3\u6d82\u5c42\u540c\u6837\u4f1a\u9020\u6210\u5e93\u4f26\u6548\u7387\u7684\u635f\u5931\u3002\u8fd9\u662f\u7531\u4e8e\u91d1\u5c5e\u6846\u67b6\u6216\u78b3\u819c\u5177\u6709\u8f83\u9ad8\u7684\u7535\u5b50\u7535\u5bfc\u7387\uff0c\u9502\u79bb\u5b50\u5728\u6e17\u5165\u8584\u819c\u65f6\u4f18\u5148\u5728\u8584\u819c\u8868\u9762\u53d1\u751f\u8fd8\u539f\u3002\u5c24\u5176\u662f\u5728\u5927\u7535\u6d41\u5145\u653e\u7535\u60c5\u51b5\u4e0b\uff0c\u5728\u4fdd\u62a4\u819c\/SEI\u819c\u8868\u9762\u7684\u7535\u8377\u8f6c\u79fb\u7684\u9502\u901a\u91cf\u6bd4\u8fdb\u5165\u819c\u7684\u9502\u6269\u6563\u901a\u91cf\u9ad8\uff0c\u8fdb\u800c\u5bfc\u81f4\u5bfc\u7535\u91d1\u5c5e\u6846\u67b6\u6216\u78b3\u6d82\u5c42\u8868\u9762\u7684\u9502\u6c89\u79ef\uff0c\u56e0\u6b64\uff0c\u9502\u679d\u6676\u7684\u95ee\u9898\u4ecd\u7136\u5b58\u5728\u3002<\/p>\n<p>\u4f7f\u7528\u5305\u62ec\u786b\u5316\u7269\uff0c\u6c27\u5316\u7269\uff0c\u805a\u5408\u7269\u548c\u6c2e\u6c27\u5316\u7269\u7b49\u5728\u5185\u7684\u56fa\u6001\u7535\u89e3\u8d28\u540c\u6837\u53ef\u4ee5\u6709\u6548\u963b\u6b62\u9502\u679d\u6676\u751f\u957f\uff0c\u9632\u6b62\u9502\u91d1\u5c5e\u8150\u8680\u3002\u4f5c\u4e3a\u4e00\u79cd\u4f18\u5f02\u7684\u56fa\u6001\u9502\u79bb\u5b50\u5bfc\u4f53\uff0cLi<sub>3x<\/sub>La<sub>2\/3-x<\/sub>TiO<sub>3<\/sub>\uff08LLTO\uff09\u5728\u6240\u6709\u56fa\u4f53\u7535\u89e3\u8d28\u5019\u9009\u6750\u6599\u4e2d\u53ef\u4ee5\u8868\u73b0\u51fa\u6700\u9ad8\u7684\u79bb\u5b50\u5bfc\u7535\u7387\uff1b\u6b64\u5916\uff0cLLTO\u662f\u4e00\u79cd\u5177\u6709\u9ad8\u526a\u5207\u6a21\u91cf\u7684\u9676\u74f7\u819c\uff0c\u8fd8\u53ef\u7528\u4e8e\u963b\u9694\u9502\u6c89\u79ef\u65f6\u6240\u4ea7\u751f\u7684\u65e0\u9650\u5236\u4f53\u79ef\u53d8\u5316\u3002\u4f46\u901a\u5e38\u60c5\u51b5\u4e0b\uff0cLLTO\u4e0e\u9502\u91d1\u5c5e\u754c\u9762\u63a5\u89e6\u4e0d\u826f\uff0c\u4f1a\u5f62\u6210\u7535\u6c60\u7535\u963b\uff0c\u5bfc\u81f4\u7535\u6c60\u5931\u6548\u3002\u800c\u4e14\uff0c\u5408\u6210\u5c0f\u5c3a\u5bf8LLTO\u8f83\u4e3a\u56f0\u96be\uff0c\u4f7f\u5f97\u56fa\u6001\u7535\u89e3\u8d28\u4e00\u822c\u4e3a\u51e0\u767e\u5fae\u7c73\u5230\u51e0\u6beb\u7c73\u539a\uff0c\u5927\u5927\u589e\u52a0\u4e86\u754c\u9762\u7684\u963b\u9694\uff0c\u964d\u4f4e\u4e86\u7535\u6c60\u7684\u7a33\u5b9a\u6027\u3002\u540c\u65f6\uff0cLLTO\u76f4\u63a5\u548c\u9502\u91d1\u5c5e\u63a5\u89e6\u65f6\u5e76\u4e0d\u7a33\u5b9a\uff0c\u9502\u79bb\u5b50\u4f1a\u5feb\u901f\u5730\u63d2\u5165\u4f7fTi<sup>4+<\/sup>\u8fd8\u539f\u6210Ti<sup>3+<\/sup>\uff0c\u5bfc\u81f4\u5176\u7535\u5b50\u7535\u5bfc\u7387\u8f83\u9ad8\u5f15\u8d77\u7535\u6c60\u5185\u90e8\u7684\u77ed\u8def\u3002\u56e0\u6b64\uff0c\u5982\u4f55\u5f00\u53d1\u51fa\u8d85\u8584\u7684LLTO\u6210\u4e3a\u4e86\u4fdd\u62a4\u9502\u91d1\u5c5e\u8d1f\u6781\u7684\u6709\u6548\u65b9\u6cd5\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u4e1c\u534e\u5927\u5b66\u4e01\u5f6c\u6559\u6388\uff08\u901a\u8baf\u4f5c\u8005\uff09\u3001\u4fde\u5efa\u52c7\u9662\u58eb\u548c\u95eb\u5efa\u534e\u6559\u6388\u7814\u7a76\u56e2\u961f<\/strong>\u63d0\u51fa\u4e86\u4e00\u79cd\u4f7f\u7528\u8d85\u8584\u5171\u6df7\u5408\u79bb\u5b50-\u7535\u5b50\u9676\u74f7\u5bfc\u4f53\uff08MIEC\uff09\u7a33\u5b9a\u9502\u8d1f\u6781\u7684\u6709\u6548\u65b9\u6cd5\u3002\u9996\u5148\uff0c\u8be5\u7814\u7a76\u56e2\u961f\u901a\u8fc7\u70e7\u7ed3\u5177\u6709\u53ef\u63a7\u8868\u9762\u548c\u7c92\u5f84\u7684\u5355\u6676LLTO\u7eb3\u7c73\u9897\u7c92\u83b7\u5f97\u5177\u6709\u4f18\u5f02\u79bb\u5b50\u7535\u5bfc\u7387\u7684\u8d85\u8584Li<sub>0.35<\/sub>La<sub>0.52<\/sub>[V]<sub>0.13<\/sub>TiO<sub>3<\/sub>\uff08LLTO\uff09\u9676\u74f7\u8584\u819c\u3002\u968f\u540e\uff0c\u901a\u8fc7\u5411LLTO\u8584\u819c\u4e2d\u5f15\u5165\u6db2\u6001\u6613\u6325\u53d1\u7684\u50ac\u5316\u5242\u5f00\u53d1\u5176MIEC\u7279\u6027\uff0c\u89e6\u53d1LLTO\u548c\u9502\u91d1\u5c5e\u4e4b\u95f4\u7684\u5316\u5b66\u53cd\u5e94\uff0c\u5f62\u6210\u5177\u6709\u9ad8\u7535\u5b50\u7535\u5bfc\u7387\u7684LLTO\u8584\u819c\uff1b\u540e\u5c06\u50ac\u5316\u5242\u84b8\u53d1\uff0c\u5373\u53ef\u5f62\u6210\u5177\u6709\u5171\u5f62\u548c\u7a33\u5b9a\u754c\u9762\u7684\u6df7\u5408LLTO\/Li\u8d1f\u6781\u3002\u5f53\u5728\u9502\u91d1\u5c5e\u7535\u6c60\u4e2d\u4f7f\u7528\u6df7\u5408\u8d1f\u6781\u65f6\uff0cMIEC\u9676\u74f7\u819c\u53ef\u4ee5\u7f13\u51b2\u9502\u79bb\u5b50\u7684\u6d53\u5ea6\u68af\u5ea6\uff0c\u5728\u9502\u91d1\u5c5e\u8868\u9762\u5e73\u8861\u4e8c\u6b21\u7535\u6d41\u5206\u5e03\uff0c\u4ece\u800c\u963b\u6b62\u7535\u89e3\u8d28\u9020\u6210\u7684\u9502\u8150\u8680\u548c\u9502\u679d\u6676\u7684\u5f62\u6210\uff0c\u4f7f\u7535\u6c60\u7684\u5e93\u4f26\u6548\u7387\u9ad8\u8fbe98%\u3002\u8fd9\u4e00\u7814\u7a76\u6210\u679c\u5df2\u7ecf\u53d1\u8868\u5728<strong>Advanced Materials<\/strong>\u4e0a\uff0c\u9898\u4e3a\u201c<strong>Mixed Ionic and Electronic Conductor for Li-Metal Anode Protection<\/strong>\u201d\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00<\/strong> <strong>\u5177\u6709<\/strong><strong>MIEC<\/strong><strong>\u7279\u6027\u7684<\/strong><strong>LLTO<\/strong><strong>\u8584\u819c\u4fdd\u62a4\u9502\u91d1\u5c5e\u8d1f\u6781\u7684\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-121615\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0001-m.png\" alt=\"\" width=\"600\" height=\"411\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0001-m.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0001-m-300x206.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a\uff09\u5177\u6709\u53ef\u63a7\u8868\u9762\u7684LLTO\u5355\u7eb3\u7c73\u6676\u4f53\u7684\u8bbe\u8ba1\u548c\u8584LLTO\u8584\u819c\u7684\u5236\u5907\uff1b<\/p>\n<p>b\uff09\u7532\u82ef\u4f5c\u4e3a\u50ac\u5316\u5242\u65f6\uff0cLLTO\u8584\u819c\u4e0e\u9502\u91d1\u5c5e\u5728\u754c\u9762\u5904\u53cd\u5e94\uff0c\u5f62\u6210\u5177\u6709\u7a33\u5b9a\u754c\u9762\u7684\u6df7\u5408LLTO\/Li\u8d1f\u6781\uff1b<\/p>\n<p>c\uff09\u6df7\u5408\u8d1f\u6781\u5728\u9502\u91d1\u5c5e\u7535\u6c60\u4e2d\u7684\u5e94\u7528\uff1b\u5176\u4e2d\uff0cLLTO\u8584\u819c\u53ef\u4ee5\u4fc3\u8fdb\u9502\u79bb\u5b50\u7684\u5feb\u901f\u5747\u5300\u6c89\u79ef\uff0c\u540c\u65f6\u5ef6\u7f13\u7535\u89e3\u6db2\u5bf9\u9502\u91d1\u5c5e\u7684\u4fb5\u8680\u3002<\/p>\n<p><strong>\u56fe\u4e8c<\/strong> <strong>\u6750\u6599\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-121617\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0003.png\" alt=\"\" width=\"600\" height=\"516\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0003.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0003-300x258.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a\uff09\u5177\u6709\u53ef\u63a7\u8868\u9762\u548c\u7c92\u5ea6\u7684LLTO NPs\uff1b<\/p>\n<p>b\uff09\u5355\u6676LLTO\u7eb3\u7c73\u9897\u7c92\u7684TEM\u56fe\uff1b<\/p>\n<p>c\uff09\u7d27\u5bc6\u5806\u79ef\u7684\u539a\u5ea6\u4e3a8.2 \u03bcm\u7684\u7eafLLTO\u819c\uff1b<\/p>\n<p>d\uff09\u6df7\u5408LLTO\/Li\u8d1f\u6781\uff1b<\/p>\n<p>e\uff09\u7eafLLTO\u8584\u819c\uff08\u9ed1\u7ebf\uff09\u548c\u539f\u4f4d\u96c6\u6210\u5de5\u827a\uff08\u7ea2\u7ebf\uff09\u540e\u7684\u9502\u91d1\u5c5e\u8868\u9762\u4e0aLLTO\u8584\u819c\u7684XPS\u56fe\uff1b<\/p>\n<p>f\uff09\u539f\u4f4d\u96c6\u6210\u5de5\u827a\u540e\uff0cLLTO\u7c89\u672b\uff0c\u7eafLLTO\u819c\u548c\u5728\u9502\u91d1\u5c5e\u8868\u9762\u4e0a\u7684LLTO\u819c\u7684XRD\u56fe\u3002<\/p>\n<p><strong>\u56fe\u4e09<\/strong> <strong>\u6df7\u5408<\/strong><strong>LLTO\/Li<\/strong><strong>\u8d1f\u6781\u7684\u7535\u5316\u5b66\u7a33\u5b9a\u6027<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-121618\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0004.png\" alt=\"\" width=\"600\" height=\"666\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0004.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0004-270x300.png 270w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a\uff09LLTO\/Li\u2016Li\u7535\u6c60\uff0cLLTO-Li\u2016Li\u7535\u6c60\u548c\u5bf9\u79f0LLTO\/Li\u2016LLTO\/Li\u7535\u6c60\u7684\u963b\u6297\u56fe\uff1b<\/p>\n<p>b\uff09\u7b2c1\u5708\uff0c\u7b2c100\u5708\u548c\u7b2c200\u5708\u5faa\u73af\u7684LLTO\/Li-S\u7535\u6c60\u7684\u963b\u6297\u56fe\uff1b<\/p>\n<p>c\uff09\u7b2c1\u5708\uff0c\u7b2c100\u5708\u548c\u7b2c200\u5708\u5faa\u73af\u7684\u7eafLi-S\u7535\u6c60\u7684\u963b\u6297\u56fe\uff1b<\/p>\n<p>d\uff09LLTO\/Li-S\u7535\u6c60\u57280.5C\u7535\u6d41\u5bc6\u5ea6\u4e0b\u7684\u6052\u6d41\u5145\u653e\u7535\u66f2\u7ebf\uff1b<\/p>\n<p>e\uff09\u626b\u63cf\u901f\u7387\u4e3a0.1 mV s<sup>-1<\/sup>\u65f6\uff0cLLTO\/Li-S\u7535\u6c60\u524d\u4e94\u5708\u7684CV\u66f2\u7ebf\uff1b<\/p>\n<p>f\uff09LLTO\/Li-S\u7535\u6c60\u7684\u957f\u5faa\u73af\u7a33\u5b9a\u6027\u548c\u5e93\u4ed1\u6548\u7387\u3002<\/p>\n<p><strong>\u00a0<\/strong><strong>\u56fe\u56db<\/strong> <strong>\u9502\u91d1\u5c5e\u8d1f\u6781\u4e0a\u9502\u6c89\u79ef\u7269\u7684\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-121616\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0002.png\" alt=\"\" width=\"600\" height=\"671\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0002.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/adma201705105-fig-0002-268x300.png 268w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a\uff09LLTO\u8584\u819c\u4e0b\u65b9\u9502\u6c89\u79ef\u5c42\u7684\u6a2a\u622a\u9762\u56fe\uff1b<\/p>\n<p>b\uff09200\u5708\u5faa\u73af\u540e\uff0cLLTO\u8584\u819c\u7684\u4e0a\u8868\u9762\uff1b<\/p>\n<p>c\uff09\u7eaf\u9502\u8d1f\u6781\u8868\u9762\u4e0a\u9502\u6c89\u79ef\u5c42\u7684\u6a2a\u622a\u9762\u56fe\uff1b<\/p>\n<p>d\uff09200\u5708\u5faa\u73af\u540e\uff0c\u7eaf\u9502\u8d1f\u6781\u7684\u4e0a\u8868\u9762\uff1b<\/p>\n<p>e\uff09\u653e\u7535\u81f3-0.09 V\u540e\u70ad\u9ed1\u819c\u7684\u8868\u9762\u5f62\u8c8c\uff0c\u5176\u4e2d\u78b3\u7eb3\u7c73\u9897\u7c92\u8868\u9762\u79ef\u7d2f\u6709\u9502\u679d\u6676\uff1b\uff08\u63d2\u56fe\uff1a\u5faa\u73af\u540e\u78b3\u9ed1\u7535\u6781\u7684\u7167\u7247\uff09<\/p>\n<p>f\uff09\u653e\u7535\u81f3-0.06 V\u540eLLTO\u819c\u7684\u8868\u9762\u5f62\u8c8c\u3002\uff08\u63d2\u56fe\uff1a\u5faa\u73af\u540eLLTO\u7535\u6781\u7684\u7167\u7247\uff09<\/p>\n<p><strong>\u00a0<\/strong><\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u5de5\u4f5c\u4e0d\u4ec5\u8bc1\u5b9e\u4e86\u4f7f\u7528\u5177\u6709MIEC\u7279\u6027\u7684LLTO\u8584\u819c\u53ef\u4ee5\u6709\u6548\u7a33\u5b9a\u9502\u91d1\u5c5e\u8d1f\u6781\uff0c\u8fd8\u8868\u660e\u4f7f\u7528\u6df7\u5408\u8d1f\u6781\u65f6\u53ef\u4ee5\u6709\u6548\u63d0\u9ad8\u9502\u91d1\u5c5e\u7535\u6c60\u7684\u7a33\u5b9a\u6027\u3002\u5f53\u4ee5\u6db2\u6001\u7532\u82ef\u4e3a\u50ac\u5316\u5242\u65f6\uff0c\u5408\u6210\u6240\u5f97\u6df7\u5408LLTO\/Li\u8d1f\u6781\u5177\u6709\u7a33\u5b9a\u7684\u754c\u9762\u548c\u4ec5\u4e3a294 \u03a9 cm<sup>-2<\/sup>\u7684\u8f83\u5c0f\u754c\u9762\u7535\u963b\u3002LLTO\u8584\u819c\u5728\u4fdd\u62a4\u9502\u91d1\u5c5e\u8d1f\u6781\u65f6\u4f1a\u4ea7\u751f\u534f\u540c\u4f5c\u7528\u3002\u4e00\u65b9\u9762\uff0c\u8be5\u819c\u5728\u6db2\u4f53\u7535\u89e3\u8d28\u4e2d\u662f\u673a\u68b0\u7a33\u5b9a\u548c\u5316\u5b66\u7a33\u5b9a\u7684\uff0c\u53ef\u7528\u4f5c\u56fa\u6001\u7684\u7269\u7406\u963b\u6321\u5c42\uff0c\u9002\u5e94\u9502\u8d1f\u6781\u7684\u4f53\u79ef\u53d8\u5316\uff1b\u540c\u65f6\u8fd8\u53ef\u4f5c\u4e3a\u963b\u6321\u5c42\uff0c\u9632\u6b62\u6db2\u4f53\u7535\u89e3\u8d28\u5bf9\u9502\u91d1\u5c5e\u7684\u8150\u8680\u3002\u53e6\u4e00\u65b9\u9762\uff0cMIEC\u8584\u819c\u53ef\u4ee5\u8d77\u5230\u7f13\u51b2\u9502\u79bb\u5b50\u6d53\u5ea6\u68af\u5ea6\u7684\u4f5c\u7528\uff0c\u901a\u8fc7\u4f7f\u9502\u91d1\u5c5e\u8868\u9762\u7684\u4e8c\u6b21\u7535\u6d41\u5206\u5e03\u5747\u5300\u5316\uff0c\u4ece\u800c\u4f7f\u5f62\u6210\u9502\u679d\u6676\u7684\u9a71\u52a8\u529b\u6700\u5c0f\u5316\uff0c\u51cf\u5c11\u9502\u679d\u6676\u7684\u5f62\u6210\u3002\u5b9e\u9a8c\u7ed3\u679c\u8868\u660e\uff0c\u5373\u4f7f\u57283 mA cm<sup>-2<\/sup>\u7684\u5927\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0cLi-S\u7535\u6c60\u7ecf\u8fc7200\u5708\u5faa\u73af\u540e\u4ecd\u53ef\u663e\u793a\u51fa&gt; 98\uff05\u7684\u9ad8\u5e93\u4ed1\u6548\u7387\u548c&gt; 700 mA h g<sup>-1<\/sup>\u9ad8\u5bb9\u91cf\u3002\u672c\u5de5\u4f5c\u4f7f\u7528MIEC\u4f5c\u4e3a\u949d\u5316\u5c42\u4e0d\u4ec5\u5de7\u5999\u5730\u89e3\u51b3\u4e86\u9502\u91d1\u5c5e\u8d1f\u6781\u7684\u56fa\u6709\u95ee\u9898\uff0c\u8fd8\u4e3a\u751f\u4ea7\u51fa\u66f4\u9ad8\u6548\u8010\u7528\u4e14\u5177\u6709\u6781\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u548c\u529f\u7387\u5bc6\u5ea6\u7684\u9502\u91d1\u5c5e\u7535\u6c60\u5960\u5b9a\u4e86\u57fa\u7840\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.201705105\/full\">Mixed Ionic and Electronic Conductor for Li-Metal Anode Protection<\/a><\/strong>\uff08Adv. Mater. 2018, DOI: 10.1002\/adma.201705105\uff09<\/p>\n<p><strong>\u4f5c\u8005\u7b80\u4ecb<\/strong><\/p>\n<p><strong>\u95eb\u5efa\u534e<\/strong> <strong>\u7537\uff0c\u4e1c\u534e\u5927\u5b66\u7eba\u7ec7\u5b66\u9662\uff0c\u975e\u7ec7\u9020\u6750\u6599\u4e0e\u5de5\u7a0b\u5b66\u79d1\u7814\u7a76\u5458\u3001\u535a\u58eb\u751f\u5bfc\u5e08<\/strong><\/p>\n<p>\u66fe\u83b7\u5f97\u5305\u62ec\u201c\u56fd\u5bb6\u4f18\u79c0\u81ea\u8d39\u7559\u5b66\u751f\u5956\u5b66\u91d1\u201d\uff082016\u5e74\uff09\u3001\u201c\u4e2d\u79d1\u9662\u5fae\u7535\u5b50\u7814\u7a76\u6240\u7279\u7b49\u8363\u8a89\u5956\u5b66\u91d1\u201d\uff082012\u5e74\uff09\u7b49\u5956\u9879\u3002\u957f\u671f\u62c5\u4efbNat. Commun.\u3001Chem. Mater.\u3001ACS Nano\u3001Adv. Mater.\u7b49\u591a\u4e2a\u56fd\u9645\u671f\u520a\u7684\u5ba1\u7a3f\u4eba\u3002\u53d1\u8868SCI\u8bba\u658720\u4f59\u7bc7\uff0c\u5176\u4e2d\u7b2c\u4e00\/\u901a\u8baf\u4f5c\u800515\u7bc7\uff0cIF&gt;3: 12\u7bc7\uff0c\u5c01\u9762\u8bba\u65871\u7bc7\uff0c\u83b7\u6388\u6743\u4e2d\u56fd\u53d1\u660e\u4e13\u52294\u9879\uff0c\u7f8e\u56fd\u4e13\u52292\u9879\u3002<\/p>\n<p><strong>\u4fde\u5efa\u52c7<\/strong> <strong>\u4e2d\u56fd\u5de5\u7a0b\u9662\u9662\u58eb\uff0c\u6559\u6388\uff0c\u535a\u5bfc<\/strong> <strong>\u7eba\u7ec7\u79d1\u5b66\u4e0e\u5de5\u7a0b\u4e00\u7ea7\u56fd\u5bb6\u91cd\u70b9\u5b66\u79d1\u8d23\u4efb\u4eba\u3001\u517c\u4efb\u4e2d\u56fd\u7eba\u7ec7\u5de5\u7a0b\u5b66\u4f1a\u526f\u7406\u4e8b\u957f\u3001\u4e0a\u6d77\u5e02\u7eba\u7ec7\u5de5\u7a0b\u5b66\u4f1a\u526f\u7406\u4e8b\u957f\u3001\u4e0a\u6d77\u5e02\u590d\u5408\u6750\u6599\u5b66\u4f1a\u7406\u4e8b\u957f\u7b49<\/strong><\/p>\n<p>\u957f\u671f\u81f4\u529b\u4e8e\u7eba\u7ec7\u6750\u6599\u9886\u57df\u7684\u79d1\u7814\u4e0e\u6559\u5b66\uff0c\u5728\u5929\u7136\u7ea4\u7ef4\u8d44\u6e90\u5f00\u53d1\u3001\u5316\u5b66\u7ea4\u7ef4\u521b\u65b0\u5e94\u7528\u3001\u65b0\u578b\u7ed3\u6784\u548c\u529f\u80fd\u7eba\u7ec7\u6750\u6599\u7b49\u9886\u57df\u5f00\u5c55\u57fa\u7840\u7406\u8bba\u3001\u5173\u952e\u6280\u672f\u548c\u5e94\u7528\u5f00\u53d1\u7814\u7a76\uff0c\u53d6\u5f97\u4e86\u7cfb\u5217\u521b\u65b0\u6027\u6210\u679c\u3002\u83b7\u56fd\u5bb6\u6280\u672f\u53d1\u660e\u4e8c\u7b49\u59562\u9879\uff0c\u56fd\u5bb6\u79d1\u6280\u8fdb\u6b65\u4e8c\u7b49\u59562\u9879\uff0c\u7701\u90e8\u7ea7\u79d1\u6280\u6210\u679c\u595613\u9879\uff1b\u5408\u8457\u4e66\u7c4d3\u90e8\uff1b\u53d1\u8868\u8bba\u6587200\u4f59\u7bc7\uff1b\u6388\u6743\u56fd\u5bb6\u53d1\u660e\u4e13\u522980\u4f59\u9879\uff1b\u6307\u5bfc\u7814\u7a76\u751f100\u4f59\u540d\uff0c\u5176\u4e2d1\u7bc7\u535a\u58eb\u5b66\u4f4d\u8bba\u6587\u88ab\u8bc4\u4e3a2011\u5e74\u5ea6\u5168\u56fd\u767e\u7bc7\u4f18\u79c0\u535a\u58eb\u5b66\u4f4d\u8bba\u6587\u3002\u83b72007\u5e74\u7eba\u7ec7\u5de5\u4e1a\u5e74\u5ea6\u521b\u65b0\u4eba\u7269\uff0c2008\u5e74\u5b9d\u94a2\u6559\u80b2\u57fa\u91d1\u4f18\u79c0\u6559\u5e08\u5956\uff0c2010\u5e74\u5168\u56fd\u4f18\u79c0\u79d1\u6280\u5de5\u4f5c\u8005\uff0c2011\u5e74\u4e2d\u56fd\u7eba\u7ec7\u5de5\u7a0b\u5b66\u4f1a\u9996\u5c4a\u4e2d\u56fd\u7eba\u7ec7\u5b66\u672f\u5927\u5956\u7b49\u8363\u8a89\u3002<\/p>\n<p><strong>\u901a\u8baf\u4f5c\u8005\u7b80\u4ecb<\/strong><\/p>\n<p><strong>\u4e01\u5f6c<\/strong> <strong>\u7537\uff0c\u6559\u6388\u3001\u535a\u58eb\u751f\u5bfc\u5e08<\/strong> <strong>\u6559\u80b2\u90e8\u201c\u957f\u6c5f\u5b66\u8005\u5956\u52b1\u8ba1\u5212\u201d\u7279\u8058\u6559\u6388\u3001\u56fd\u5bb6\u81ea\u79d1\u57fa\u91d1\u59d4\u4f18\u79c0\u9752\u5e74\u57fa\u91d1\u83b7\u5f97\u8005\u3001\u6559\u80b2\u90e8\u65b0\u4e16\u7eaa\u4f18\u79c0\u4eba\u624d\u3001\u4e0a\u6d77\u5e02\u201c\u66d9\u5149\u5b66\u8005\u201d\u3001\u6559\u80b2\u90e8\u970d\u82f1\u4e1c\u6559\u80b2\u57fa\u91d1\u83b7\u5f97\u8005<\/strong><\/p>\n<p>\u957f\u671f\u4ece\u4e8b\u529f\u80fd\u5fae\u7eb3\u7c73\u7ea4\u7ef4\u7eba\u7ec7\u6750\u6599\u7814\u7a76\uff0c\u5728\u5fae\u7eb3\u7c73\u7ea4\u7ef4\u6750\u6599\u6210\u578b\u7406\u8bba\u3001\u7ed3\u6784\u8bbe\u8ba1\u53ca\u6280\u672f\u5e94\u7528\u65b9\u9762\u53d6\u5f97\u4e86\u4e00\u7cfb\u5217\u8fdb\u5c55\u3002\u5176\u76f8\u5173\u7814\u7a76\u6210\u679c\u53d1\u8868\u5728Nat. Commun.\u3001Adv. Mater.\u3001Prog. Mater. Sci.\u7b49\u671f\u520a\u5171206\u7bc7\uff0c\u4ee5\u7b2c\u4e00\u4f5c\u8005\/\u8054\u7cfb\u4eba\u53d1\u8868\u7684SCI\u8bba\u6587\u6709172\u7bc7\uff08\u5176\u4e2dIF&gt;3: 168\u7bc7\uff0cIF&gt;6: 71\u7bc7\uff09\uff0c\u603b\u5f157004\u6b21\uff0c\u4ed6\u5f155351\u6b21\uff0cH\u6307\u657045\uff1b\u7533\u8bf7\u56fd\u5bb6\u53d1\u660e\u4e13\u5229131\u9879\uff0c\u83b7\u6388\u674355\u9879\uff1b\u4e3b\u7f16\u6211\u56fd\u7b2c\u4e00\u90e8\u9759\u7535\u7eba\u4e1d\u4e66\u7c4d\u300a\u9759\u7535\u7eba\u4e1d\u4e0e\u7eb3\u7c73\u7ea4\u7ef4\u300b\uff0c\u5728\u5fb7\u56fdSpringer\u51fa\u7248\u793e\u51fa\u7248\u4e3b\u7f16\u4e66\u7c4d\u300aElectrospun Nanofibers for Energy and Environmental Applications\u300b\uff0c\u5728\u7f8e\u56fd\u7ebd\u7ea6Nova\u548c\u82f1\u56fd\u5251\u6865Woodhead\u79d1\u6280\u51fa\u7248\u793e\u5408\u8457\u82f1\u6587\u4e66\u7c4d12\u90e8\u3002\u4e3b\u6301\u56fd\u5bb6\u79d1\u6280\u652f\u6491\u8ba1\u5212\u9879\u76ee\u8bfe\u9898\u3001\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\uff08\u4f18\u9752\u3001\u9762\u4e0a\u3001\u8054\u5408\u57fa\u91d1\u3001\u9752\u57fa\uff09\u3001\u4e0a\u6d77\u5e02\u79d1\u59d4\u57fa\u7840\u91cd\u70b9\u9879\u76ee\u3001\u5fb7\u56fd\u535a\u4e16\u3001\u8054\u5408\u5229\u534e\u516c\u53f8\u7b49\u9879\u76ee31\u9879\u3002\u83b7\u7f8e\u56fd\u7ea4\u7ef4\u5b66\u4f1a\u6770\u51fa\u6210\u5c31\u5956\u3001\u4e2d\u56fd\u7eba\u7ec7\u5de5\u4e1a\u8054\u5408\u4f1a\u79d1\u5b66\u6280\u672f\u8fdb\u6b65\u4e00\u7b49\u5956\u3001\u4e0a\u6d77\u5e02\u79d1\u5b66\u6280\u672f\uff08\u53d1\u660e\uff09\u5956\u4e00\u7b49\u5956\u3001\u5929\u6d25\u5e02\u79d1\u6280\u8fdb\u6b65\u4e8c\u7b49\u5956\u30012017\u4e2d\u56fd\u7eba\u7ec7\u5b66\u672f\u5e26\u5934\u4eba\u7b49\u5956\u52b1\u53ca\u8363\u8a89\u79f0\u53f710\u4f59\u9879\u3002<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8<strong>\u65b0\u4eba\u7ec4NeverSayBye<\/strong>\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002\u540c\u65f6\uff0c\u611f\u8c22<strong>\u4e01\u5f6c\u8001\u5e08<\/strong>\u5bf9\u672c\u6587\u7684\u6307\u5bfc\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1aRDD-2011-CHERISH\uff0c\u4efb\u4e39\u4e39\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/p>\n<p>\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/p>\n<p>&nbsp;<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u7531\u4e8e\u9502\u91d1\u5c5e\u8d1f\u6781\u5177\u6709\u8f83\u9ad8\u7684\u7406\u8bba\u5bb9\u91cf\uff083840 mA h g-1\uff09\u548c\u6700\u4f4e\u7684\u7535\u5316\u5b66\u7535\u4f4d\uff08-3.04 V vs SHE\uff09\uff0c\u56e0\u6b64\uff0c\u8fd1\u5e74\u6765\u5bf9\u53ef\u5145\u7535\u9502\u91d1\u5c5e\u7535\u6c60\u8fdb\u884c\u4e86&#8230;<\/p>\n","protected":false},"author":230,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[2736,1839,2735],"class_list":["post-121614","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-2736","tag-1839","tag-2735"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/121614"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/230"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=121614"}],"version-history":[{"count":6,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/121614\/revisions"}],"predecessor-version":[{"id":121808,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/121614\/revisions\/121808"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=121614"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=121614"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=121614"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}