{"id":122476,"date":"2018-01-21T12:43:09","date_gmt":"2018-01-21T04:43:09","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=122476"},"modified":"2018-01-24T05:57:42","modified_gmt":"2018-01-23T21:57:42","slug":"__trashed-15","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=122476","title":{"rendered":"Mater. Sci. Eng. A\uff1aTRIP\u94a2\u6405\u62cc\u6469\u64e6\u710a\u63a5\u5934\u7ec4\u7ec7\u4e0e\u62c9\u4f38\u6027\u80fd"},"content":{"rendered":"<p>\u3010<strong>\u5f15\u8a00<\/strong>\u3011<\/p>\n<p>TRIP\u94a2\u5c5e\u4e8e\u4e00\u79cd\u65b0\u578b\u94a2\u6750\uff0c\u76ee\u524d\u4e3b\u8981\u7528\u4e8e\u8f7b\u91cf\u5316\u7684\u6c7d\u8f66\u6784\u4ef6\u4e2d\uff0c\u4e0d\u4ec5\u80fd\u5b9e\u73b0\u8f7b\u91cf\u5316\u3001\u8282\u7ea6\u80fd\u6e90\uff0c\u8fd8\u80fd\u4fdd\u8bc1\u7ed3\u6784\u7684\u5b89\u5168\u6027\u3002\u4f46\u4f20\u7edf\u710a\u63a5\u6280\u672f\u4f1a\u4f7fTRIP\u94a2\u7684\u7ec4\u7ec7\u53d1\u751f\u8f6c\u53d8\uff0c\u964d\u4f4e\u63a5\u5934\u7684\u673a\u68b0\u6027\u80fd\uff0c\u800c\u6405\u62cc\u6469\u64e6\u710a\u662f\u4e00\u79cd\u65b0\u578b\u56fa\u76f8\u8fde\u63a5\u6280\u672f\uff0c\u6240\u4ee5\u6405\u62cc\u6469\u64e6\u710a\u5728\u8fde\u63a5TRIP\u94a2\u6709\u5f88\u5927\u4f18\u52bf\u3002\u4f46\u76ee\u524d\u8fd8\u9c9c\u6709\u7814\u7a76\u4eba\u5458\u5bf9\u710a\u7f1d\u7ec4\u7ec7\u548c\u6027\u80fd\u4e4b\u95f4\u7684\u5173\u7cfb\u8fdb\u884c\u7814\u7a76\u3002<\/p>\n<p>\u3010<strong>\u6210\u679c\u7b80\u4ecb<\/strong>\u3011<\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u65e5\u672c<\/strong><strong>\u4e1c\u5317\u5927\u5b66<\/strong>\u7684<strong>S.Mironov<\/strong><strong>\u3001<\/strong><strong>Y.S.Sato<\/strong><strong>\u3001<\/strong><strong>H.Kokawa<\/strong><strong>\u3001<\/strong><strong>H.T.Fujii<\/strong><strong>\u548c\u9752\u5c71\u5b66\u9662\u5927\u5b66<\/strong><strong>S.Yoneyama<\/strong>\u4ee5\u53ca<strong>\u65e5\u7acb\u7684<\/strong><strong>S.Hirano<\/strong>\u5408\u4f5c\u5728<strong>Materials Science and Engineering: A<\/strong>\u53d1\u8868\u4e86\u6700\u65b0\u7684\u7814\u7a76\u6210\u679c<strong>\u201c<\/strong><strong>Microstructure and tensile behavior of friction-stir welded TRIP steel\u201d<\/strong>\u3002\u5728\u8be5\u6587\u4e2d\uff0c\u7814\u7a76\u4eba\u5458\u5bf9TRIP\u94a2\u8fdb\u884c\u4e86\u6405\u62cc\u6469\u64e6\u710a\uff0c\u5e76\u7528\u7535\u5b50\u80cc\u6563\u5c04\u884d\u5c04\uff08EBSD\uff09\u548c\u6570\u5b57\u56fe\u50cf\u76f8\u5173\u6280\u672f\u7814\u7a76\u4e86\u7ec4\u7ec7\u4e0e\u6027\u80fd\u7684\u5173\u7cfb\u3002<\/p>\n<p>\u3010<strong>\u56fe\u6587\u5bfc\u8bfb<\/strong>\u3011<\/p>\n<p><strong>\u56fe<\/strong><strong>1 <\/strong><strong>\u710a\u63a5\u63a5\u5934\u6a2a\u622a\u9762\u7684\u5b8f\u89c2\u5f62\u8c8c\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122484\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-1.png\" alt=\"\" width=\"600\" height=\"120\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-1-300x60.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>RS\u548cAS\u5206\u522b\u662f\uff1a\u540e\u9000\u4fa7\u548c\u524d\u8fdb\u4fa7\u3002TD\u3001ND\u548cWD\u5206\u522b\u662f\u6a2a\u5411\u3001\u7eb5\u5411\u548c\u710a\u63a5\u65b9\u5411\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>2 <\/strong><strong>\u710a\u63a5\u63a5\u5934\u5404\u4e2a\u533a\u57df\u7684<\/strong><strong>SEM<\/strong><strong>\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122485\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-2.png\" alt=\"\" width=\"600\" height=\"300\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-2.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-2-300x150.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u6bcd\u6750\u7684SEM\u56fe<\/p>\n<p>\uff08b\uff09\u533a\u57df1\u7684SEM\u56fe<\/p>\n<p>\uff08c\uff09\u533a\u57df2\u7684SEM\u56fe<\/p>\n<p>\uff08d\uff09\u6405\u62cc\u533a\u4e2d\u95f4\u533a\u57df\u7684SEM\u56fe<\/p>\n<p>\uff08e\uff09\u6405\u62cc\u5e26\u533a\u57df\u7684SEM\u56fe<\/p>\n<p><strong>\u56fe<\/strong><strong>3\u00a0<\/strong><strong>\u710a\u7f1d\u663e\u5fae\u786c\u5ea6\u548c\u529b\u5b66\u6027\u80fd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122486\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-3.png\" alt=\"\" width=\"600\" height=\"225\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-3.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-3-300x113.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u6cbf\u710a\u7f1d\u65b9\u5411\u7684\u663e\u5fae\u786c\u5ea6<\/p>\n<p>\uff08b\uff09\u6bcd\u6750\u548c\u710a\u63a5\u63a5\u5934\u7684\u5e94\u529b\u5e94\u53d8\u66f2\u7ebf<\/p>\n<p><strong>\u56fe<\/strong><strong>4 <\/strong><strong>\u52a0\u8f7d\u4ee5\u540e\u710a\u63a5\u63a5\u5934\u4e0a\u8868\u9762\u7684\u771f\u5e94\u53d8\u5206\u5e03\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122477\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-4.png\" alt=\"\" width=\"600\" height=\"289\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-4-300x145.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5f39\u6027\u8f7d\u8377\u4e0b\u7684\u710a\u63a5\u63a5\u5934\u4e0a\u8868\u9762\u7684\u771f\u5e94\u53d8\u5206\u5e03\u56fe<\/p>\n<p>\uff08b\uff09\u5851\u6027\u5e94\u53d8\u4e3a0.2%\u65f6\u7684\u710a\u63a5\u63a5\u5934\u4e0a\u8868\u9762\u7684\u771f\u5e94\u53d8\u5206\u5e03\u56fe<\/p>\n<p>\uff08c\uff09\u5851\u6027\u5e94\u53d8\u4e3a1.5%\u65f6\u7684\u710a\u63a5\u63a5\u5934\u4e0a\u8868\u9762\u7684\u771f\u5e94\u53d8\u5206\u5e03\u56fe<\/p>\n<p>\uff08d\uff09\u5851\u6027\u5e94\u53d8\u4e3a3.2%\u65f6\u7684\u710a\u63a5\u63a5\u5934\u4e0a\u8868\u9762\u7684\u771f\u5e94\u53d8\u5206\u5e03\u56fe<\/p>\n<p>\uff08e\uff09\u5851\u6027\u5e94\u53d8\u4e3a3.6%\u65f6\u7684\u710a\u63a5\u63a5\u5934\u4e0a\u8868\u9762\u7684\u771f\u5e94\u53d8\u5206\u5e03\u56fe<\/p>\n<p><strong>\u56fe<\/strong><strong>5 <\/strong><strong>\u70ed\u5f71\u54cd\u533a\u5965\u6c0f\u4f53\u76f8\u8f6c\u53d8\u7684<\/strong><strong>EBSD<\/strong><strong>\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122478\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-5.png\" alt=\"\" width=\"600\" height=\"314\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-5-300x157.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u70ed\u5f71\u54cd\u533a\u7684\u5965\u6c0f\u4f53\u76f8\u8f6c\u53d8\u7684\u4e0d\u540c\u533a\u57df\u7ec4\u5408EBSD\u56fe<\/p>\n<p>\uff08b\uff09b\u533a\u57df\u7684\u9ad8\u5206\u8fa8\u653e\u5927\u56fe<\/p>\n<p>\uff08c\uff09c\u533a\u57df\u7684\u9ad8\u5206\u8fa8\u653e\u5927\u56fe<\/p>\n<p>\uff08d\uff09d\u533a\u57df\u7684\u9ad8\u5206\u8fa8\u653e\u5927\u56fe<\/p>\n<p><strong>\u56fe<\/strong><strong>6 <\/strong><strong>\u533a\u57df<\/strong><strong>1<\/strong><strong>\u7684\u7ec4\u7ec7\u53d8\u5316\u60c5\u51b5<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122479\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-6.png\" alt=\"\" width=\"600\" height=\"148\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-6-300x74.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u6b8b\u4f59\u5965\u6c0f\u4f53\u7684\u5206\u89e3<\/p>\n<p>\uff08b\uff09\u6b8b\u4f59\u5965\u6c0f\u4f53\u7684\u7403\u5316<\/p>\n<p>\uff08c\uff09\u8d1d\u6c0f\u4f53\u94c1\u7d20\u4f53\u7684\u56de\u590d<\/p>\n<p><strong>\u56fe<\/strong><strong>7 <\/strong><strong>\u62c9\u4f38\u8fc7\u7a0b\u4e2d\u710a\u7f1d\u663e\u5fae\u7ec4\u7ec7\u7684\u53d8\u5316<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122480\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-7.png\" alt=\"\" width=\"600\" height=\"293\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-7.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-7-300x147.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09EBSD\u56fe\u8868\u660e\u6b8b\u4f59\u5965\u6c0f\u4f53\u7684\u51cf\u5c11<\/p>\n<p>\uff08b\uff09\u9ad8\u5206\u8fa8EBSD\u56fe\u7684\u5965\u6c0f\u4f53\u5448\u53e0\u5c42\u5206\u5e03\u7684\u8868\u660e\u53ef\u80fd\u5b58\u5728\u5965\u6c0f\u4f53\u8f6c\u53d8\u4e3a\u9a6c\u6c0f\u4f53<\/p>\n<p><strong>\u56fe<\/strong><strong>8 EBSD<\/strong><strong>\u53d6\u5411\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122481\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-8.png\" alt=\"\" width=\"600\" height=\"215\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-8.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-8-300x108.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09EBSD\u53d6\u5411\u56fe<\/p>\n<p>\uff08b\uff09\u6405\u62cc\u533a\u6b8b\u7559\u5965\u6c0f\u4f53\u548c\u9a6c\u6c0f\u4f53\u7684\u5178\u578b\u53d6\u5411\u5173\u7cfb<\/p>\n<p><strong>\u56fe<\/strong><strong>9 <\/strong><strong>\u9a6c\u6c0f\u4f53\u8f6c\u53d8\u6781\u5c04\u6295\u5f71\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122482\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-9.png\" alt=\"\" width=\"600\" height=\"193\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-9-300x97.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09K-S\u53d6\u5411\u5173\u7cfb\u4e0b\u7684\u6781\u5c04\u6295\u5f71\u56fe<\/p>\n<p>\uff08b\uff09N-W\u53d6\u5411\u5173\u7cfb\u4e0b\u7684\u6781\u5c04\u6295\u5f71\u56fe<\/p>\n<p>\uff08c\uff09\u5229\u7528\u56fe8\uff08a\uff09\u4e2d\u7684\u6676\u7c92\u5b9e\u6d4b\u7684\u6781\u56fe<\/p>\n<p><strong>\u56fe<\/strong><strong>10 <\/strong><strong>\u710a\u7f1d\u533a\u9a6c\u6c0f\u4f53\u8f6c\u53d8\u7684\u9a8c\u8bc1<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-122483\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-10.png\" alt=\"\" width=\"600\" height=\"230\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/mse.2018-10-300x115.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u710a\u7f1d\u533a\u9a6c\u6c0f\u4f53\u7684\u53d6\u5411\u5dee\u5206\u5e03\u56fe<\/p>\n<p>\uff08b\uff09\u710a\u7f1d\u533a\u9a6c\u6c0f\u4f53\u53d8\u4f53\u5339\u914d\u9891\u7387\u56fe<\/p>\n<p>\u3010<strong>\u5c0f\u7ed3<\/strong>\u3011<\/p>\n<p>\u7814\u7a76\u4eba\u5458\u5229\u7528EBSD\u548c\u7535\u5b50\u80cc\u6563\u5c04\u884d\u5c04\u6280\u672f\u7cfb\u7edf\u7814\u7a76\u4e86TRIP\u94a2\u6405\u62cc\u6469\u64e6\u710a\u63a5\u5934\u7ec4\u7ec7\u548c\u62c9\u4f38\u6027\u80fd\u3002\u7814\u7a76\u53d1\u73b0\u710a\u63a5\u8fc7\u7a0b\u4e2d\u7684\u70ed\u91cf\u4f1a\u4f7f\u63a5\u5934\u70ed\u5f71\u54cd\u533a\u4ea7\u751f\u4e00\u5b9a\u7684\u8f6f\u5316\uff0c\u710a\u7f1d\u533a\u4f1a\u53d1\u751f\u9a6c\u6c0f\u4f53\u76f8\u53d8\u3002\u7ec4\u7ec7\u4e0a\u7684\u53d8\u5316\u4f1a\u4f7f\u710a\u63a5\u63a5\u5934\u62c9\u4f38\u8fc7\u7a0b\u4e2d\u8fc7\u65e9\u65ad\u88c2\uff0c\u6240\u4ee5\u8bc1\u660e\u7ec4\u7ec7\u8f6c\u53d8\u662f\u5f71\u54cd\u63a5\u5934\u529b\u5b66\u6027\u80fd\u7684\u5173\u952e\u56e0\u7d20\u3002\u6b8b\u4f59\u5965\u6c0f\u4f53\u7684\u5206\u89e3\u548c\u7403\u5316\u4ee5\u53ca\u8d1d\u6c0f\u4f53\u94c1\u7d20\u4f53\u7684\u56de\u590d\u662f\u70ed\u5f71\u54cd\u533a\u6750\u6599\u8f6f\u5316\u7684\u4e3b\u8981\u539f\u56e0\u3002\u6b64\u5916\uff0c\u9a6c\u6c0f\u4f53\u8f6c\u53d8\u53d7\u53d8\u4f53\u9009\u62e9\u7684\u5f71\u54cd\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0921509318300716\" target=\"_blank\" rel=\"noopener\">Microstructure and tensile behavior of friction-stir welded TRIP steel<\/a>\uff08Mater.\u00a0Sci.\u00a0Eng. A\uff0c2018\uff0cdoi:10.1016\/j.msea.2018.01.053\uff09\u3002<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u65b0\u4eba\u7ec4\u6768\u6811\u4f9b\u7a3f\uff0c\u8d75\u98de\u9f99\u5ba1\u6838\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u3002<\/a><\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c<\/strong><strong><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u4e0a\u6d4b\u8bd5\u8c37<\/a><\/strong><strong>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 TRIP\u94a2\u5c5e\u4e8e\u4e00\u79cd\u65b0\u578b\u94a2\u6750\uff0c\u76ee\u524d\u4e3b\u8981\u7528\u4e8e\u8f7b\u91cf\u5316\u7684\u6c7d\u8f66\u6784\u4ef6\u4e2d\uff0c\u4e0d\u4ec5\u80fd\u5b9e\u73b0\u8f7b\u91cf\u5316\u3001\u8282\u7ea6\u80fd\u6e90\uff0c\u8fd8\u80fd\u4fdd\u8bc1\u7ed3\u6784\u7684\u5b89\u5168\u6027\u3002\u4f46\u4f20\u7edf\u710a\u63a5\u6280\u672f\u4f1a\u4f7fTRIP\u94a2\u7684\u7ec4\u7ec7\u53d1\u751f\u8f6c&#8230;<\/p>\n","protected":false},"author":230,"featured_media":122484,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[2762,2686],"class_list":["post-122476","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","category-keji","tag-trip","tag-2686"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/122476"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/230"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=122476"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/122476\/revisions"}],"predecessor-version":[{"id":122947,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/122476\/revisions\/122947"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/122484"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=122476"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=122476"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=122476"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}