{"id":123092,"date":"2018-01-29T06:30:27","date_gmt":"2018-01-28T22:30:27","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=123092"},"modified":"2018-01-29T10:08:08","modified_gmt":"2018-01-29T02:08:08","slug":"mater-sci-eng-a%ef%bc%9a%e5%bc%ba%e5%ba%a6%e5%92%8c%e5%bb%b6%e5%b1%95%e6%80%a7%e5%ae%8c%e7%be%8e%e7%bb%93%e5%90%88%e7%9a%84fcc%e9%ab%98%e7%a2%b3%e9%ab%98%e7%86%b5%e5%90%88%e9%87%91","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=123092","title":{"rendered":"Mater. Sci. Eng. A\uff1a\u5f3a\u5ea6\u548c\u5ef6\u5c55\u6027\u5b8c\u7f8e\u7ed3\u5408\u7684FCC\u9ad8\u78b3\u9ad8\u71b5\u5408\u91d1"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u9ad8\u71b5\u5408\u91d1\u56e0\u5176\u4f5c\u4e3a\u9ad8\u6027\u80fd\u7ed3\u6784\u6750\u6599\u7684\u6f5c\u5728\u5e94\u7528\u800c\u5907\u53d7\u5173\u6ce8\u3002FCC\uff08\u9762\u5fc3\u7acb\u65b9\uff09\u7ed3\u6784\u7684\u9ad8\u71b5\u5408\u91d1\u5177\u6709\u8f83\u597d\u7684\u5851\u6027\u548c\u4f4e\u6e29\u65ad\u88c2\u97e7\u6027\uff0c\u662f\u76ee\u524d\u5e7f\u4e3a\u7814\u7a76\u7684\u5408\u91d1\u4e4b\u4e00\u3002\u7136\u800c\uff0c\u6b64\u7c7b\u5408\u91d1\u7684\u5ba4\u6e29\u5f3a\u5ea6\u76f8\u5bf9\u8f83\u4f4e\uff08\u94f8\u6001\u4e0b\u5927\u7ea6\u53ea\u6709200MPa\uff09\uff0c\u8fdc\u4f4e\u4e8e\u91d1\u5c5e\u7ed3\u6784\u6750\u6599\u6240\u8981\u6c42\u7684\u5f3a\u5ea6\u3002\u4f4e\u5f3a\u5ea6\u8fd9\u4e00\u7f3a\u70b9\uff0c\u963b\u788d\u4e86\u5176\u4f5c\u4e3a\u4e00\u79cd\u5b9e\u7528\u578b\u7ed3\u6784\u6750\u6599\u7684\u5e94\u7528\u3002\u4f20\u7edf\u7684\u91d1\u5c5e\u5f3a\u5316\u673a\u5236\uff0c\u5982\u7ec6\u6676\u5f3a\u5316\uff0c\u6790\u51fa\u5f3a\u5316\u7b49\uff0c\u53ef\u4ee5\u63d0\u9ad8\u5408\u91d1\u5f3a\u5ea6\uff0c\u4f46\u540c\u65f6\u964d\u4f4e\u4e86\u5176\u5851\u6027\u3002\u8fd1\u671f\uff0c\u7814\u7a76\u4eba\u5458\u53d1\u73b0\uff0c\u95f4\u9699\u539f\u5b50\u5f3a\u5316\u53ef\u4ee5\u4e3a\u6539\u5584\u673a\u68b0\u6027\u80fd\u63d0\u4f9b\u53e6\u4e00\u79cd\u9014\u5f84\u3002\u56e0\u6b64\uff0c\u672c\u6587\u9009\u62e9FCC\u7ed3\u6784\u7684\u5b6a\u6676\u8bf1\u5bfc\u5851\u6027\uff08TWIP\uff09\u9ad8\u71b5\u5408\u91d1\u4f5c\u4e3a\u8d77\u59cb\u6750\u6599\uff0c\u5728\u6b64\u57fa\u7840\u4e0a\u6dfb\u52a0\u78b3\u7ec4\u5206\uff0c\u5bf9\u5176\u673a\u68b0\u6027\u80fd\u8fdb\u884c\u7cfb\u7edf\u7684\u7814\u7a76\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u6700\u8fd1\uff0c<strong>\u897f\u5b89\u4ea4\u901a\u5927\u5b66\u7684\u6c5f\u5cf0\u6559\u6388\uff08\u901a\u8baf\u4f5c\u8005<\/strong>\uff09\u7b49\u4eba\u5728<strong>Mater. Sci. Eng. A<\/strong>\u4e0a\u53d1\u8868\u9898\u4e3a<strong>\u201cHeavy carbon alloyed FCC-structured high entropy alloy with excellent combination of strength and ductility\u201d<\/strong>\u7684\u6587\u7ae0\u3002\u7814\u7a76\u56e2\u961f\u5bf9\u6210\u5206\u4e3a(Fe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub>)<sub>100<\/sub>-xC<sub>x<\/sub> (x = 0, 2.2, 3.3,4.4, 6.6 and 8.9 at.%)\u7684\u94f8\u6001\u9ad8\u71b5\u5408\u91d1\u8fdb\u884c\u7814\u7a76\u3002\u7ed3\u679c\u8868\u660e\uff0c\u9ad8\u542b\u91cf\u7684\u95f4\u9699\u78b3\u539f\u5b50\u901a\u8fc7\u6291\u5236\u4f4d\u9519\u8fd0\u52a8\u4ee5\u53ca\u4fc3\u8fdb\u5f62\u53d8\u8bf1\u5bfc\u5b6a\u6676\u8fc7\u7a0b\uff0c\u80fd\u591f\u663e\u8457\u5408\u91d1\u7684\u5f3a\u5ea6\u548c\u97e7\u6027\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>1.\u00a0<\/strong><strong>\u4e0d\u540c\u78b3\u542b\u91cf\u7684<\/strong><strong>Fe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub><\/strong><strong>\u9ad8\u71b5\u5408\u91d1\u7684<\/strong><strong>X<\/strong><strong>\u5c04\u7ebf\u884d\u5c04\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123101\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image001.jpg\" alt=\"\" width=\"600\" height=\"212\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image001.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image001-300x106.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>(a) \u4e0d\u540c\u78b3\u542b\u91cf\u7684XRD\u56fe\u8c31\uff0c\u5747\u4e3aFCC\u5355\u76f8<\/p>\n<p>(b) \u78b3\u542b\u91cf\u5bf9\u9ad8\u71b5\u5408\u91d1\u6676\u683c\u5e38\u6570\u7684\u5f71\u54cd<\/p>\n<p><strong>\u56fe<\/strong><strong>2. Fe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub><\/strong><strong>\u9ad8\u71b5\u5408\u91d1\u7684\u663e\u5fae\u5f62\u8c8c<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123102\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image003.jpg\" alt=\"\" width=\"600\" height=\"438\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image003.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image003-300x219.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u4e0d\u540c\u78b3\u542b\u91cf\u7684Fe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub>\u9ad8\u71b5\u5408\u91d1\u7684\u80cc\u6563\u5c04\u56fe\uff0c\u63d2\u56fe\u5bf9\u5e94\u9ad8\u500d\u7387\u4e0b\u7684\u5f62\u8c8c<\/p>\n<p>(b) C6.6\u548cC8.9\u9ad8\u71b5\u5408\u91d1\u4e2d\u78b3\u5316\u7269\u7684EDS\u80fd\u8c31<\/p>\n<p><strong>\u8868<\/strong><strong>1. <\/strong><strong>\u4e0d\u540c\u78b3\u542b\u91cf\u7684<\/strong><strong>Fe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub><\/strong><strong>\u9ad8\u71b5\u5408\u91d1\u7684\u673a\u68b0\u6027\u80fd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123103\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image005.png\" alt=\"\" width=\"600\" height=\"375\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image005.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image005-300x188.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong>3.<\/strong><strong>\u5de5\u7a0b\u5e94\u529b\u5e94\u53d8\u66f2\u7ebf\u53ca\u5176\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123104\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image007.jpg\" alt=\"\" width=\"600\" height=\"404\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image007.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image007-300x202.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u4e0d\u540c\u78b3\u542b\u91cf\u7684Fe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub>\u9ad8\u71b5\u5408\u91d1\u7684\u5178\u578b\u5de5\u7a0b\u5e94\u529b\u5e94\u53d8\u66f2\u7ebf<\/p>\n<p>(b) \u5c48\u670d\u5f3a\u5ea6\u3001\u6297\u62c9\u5f3a\u5ea6\u3001\u786c\u5ea6\u4ee5\u53ca\u65ad\u88c2\u5ef6\u4f38\u7387\u4e0e\u78b3\u542b\u91cf\u7684\u5173\u7cfb<\/p>\n<p>(c) \u521d\u59cb\u6837\u548cC0\u3001C3\u3001C4\u4e09\u4e2a\u62c9\u4f38\u65ad\u88c2\u6837\u54c1\u7684\u5f62\u72b6\u6bd4\u8f83<\/p>\n<p>(d) C0\u3001C2.2\u3001C3.3\u3001C4.4\u6837\u54c1\u7684\u5e94\u53d8\u5f3a\u5316\u7387\u968f\u5e94\u53d8\u7684\u53d8\u5316\u66f2\u7ebf<\/p>\n<p><strong>\u56fe4.\u4e0d\u540c\u78b3\u542b\u91cfFe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub>\u9ad8\u71b5\u5408\u91d1\u7684\u65ad\u53e3\u5f62\u8c8c<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123096\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image009.jpg\" alt=\"\" width=\"520\" height=\"724\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image009.jpg 520w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image009-215x300.jpg 215w\" sizes=\"(max-width: 520px) 100vw, 520px\" \/><\/p>\n<p>(a)\u3001(b)\u5206\u522b\u662fC0\u9ad8\u71b5\u5408\u91d1\u7684\u65ad\u53e3\u8868\u9762\u5f62\u8c8c\u7684\u4f4e\u500d\u56fe\u548c\u9ad8\u500d\u56fe<\/p>\n<p>(c)\u3001(d)\u5206\u522b\u662fC3.3\u9ad8\u71b5\u5408\u91d1\u7684\u65ad\u53e3\u8868\u9762\u5f62\u8c8c\u7684\u4f4e\u500d\u56fe\u548c\u9ad8\u500d\u56fe<\/p>\n<p>(e)\u3001(f)\u5206\u522b\u662fC4.4\u9ad8\u71b5\u5408\u91d1\u7684\u65ad\u53e3\u8868\u9762\u5f62\u8c8c\u7684\u4f4e\u500d\u56fe\u548c\u9ad8\u500d\u56fe<\/p>\n<p>(g)\u3001(h)\u5206\u522b\u662fC8.9\u9ad8\u71b5\u5408\u91d1\u7684\u65ad\u53e3\u8868\u9762\u5f62\u8c8c\u7684\u4f4e\u500d\u56fe\u548c\u9ad8\u500d\u56fe<\/p>\n<p>\u56fe(a)\u3001(c)\u3001(e)\u3001(g)\u4e2d\u7684\u9ed1\u8272\u70b9\u7ebf\u8868\u793a\u65ad\u88c2\u8868\u9762\u7684\u8f6e\u5ed3\uff0c\u6bcf\u4e2a\u6837\u54c1\u7684\u622a\u9762\u6536\u7f29\u7387\uff08RA\uff09\u548c\u65ad\u88c2\u5ef6\u4f38\u7387\u4e5f\u5217\u5728\u56fe\u4e2d<\/p>\n<p><strong>\u56fe<\/strong><strong>5.\u00a0<\/strong><strong>\u9ad8\u71b5\u5408\u91d1\u65ad\u88c2\u622a\u9762\u9644\u8fd1\u7684\u7269\u76f8\u53ca\u663e\u5fae\u7ec4\u7ec7\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123097\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image011.jpg\" alt=\"\" width=\"449\" height=\"470\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image011.jpg 449w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image011-287x300.jpg 287w\" sizes=\"(max-width: 449px) 100vw, 449px\" \/><\/p>\n<p>XRD\u56fe\u8c31\u3001EBSD\u76f8\u5206\u5e03\u56fe\u4ee5\u53ca\u53cd\u6781\u56fe(IPF) \u663e\u793a\u4e86C0\u9ad8\u71b5\u5408\u91d1(a)\u548cC3.3\u9ad8\u71b5\u5408\u91d1(b)\u65ad\u88c2\u540e\u622a\u9762\u9644\u8fd1\u7684\u5fae\u89c2\u7ec4\u7ec7\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>6. C3.3<\/strong><strong>\u9ad8\u71b5\u5408\u91d1<\/strong><strong>20%<\/strong><strong>\u771f\u5b9e\u5e94\u53d8\u540e\u53d8\u5f62\u5b6a\u6676\u7684\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123098\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image013.jpg\" alt=\"\" width=\"600\" height=\"296\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image013.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image013-300x148.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c(TEM)\u4e0b\u7684\u6697\u573a\u50cf<\/p>\n<p>(b)\u5bf9\u5e94\u4e8e\u56fe(a)\u7684\u9009\u533a\u884d\u5c04\u82b1\u6837<\/p>\n<p><strong>\u56fe<\/strong><strong>7.<\/strong> <strong>\u94f8\u6001\u548c\u56fa\u6eb6\u6001C3.3\u9ad8\u71b5\u5408\u91d1\u7684\u5de5\u7a0b\u5e94\u529b\u5e94\u53d8\u66f2\u7ebf\u53ca\u5fae\u89c2\u7ec4\u7ec7\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123099\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image015.jpg\" alt=\"\" width=\"600\" height=\"210\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image015.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image015-300x105.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u94f8\u6001\u548c\u56fa\u6eb6\u6001(re-processed)C3.3\u9ad8\u71b5\u5408\u91d1\u4ee5\u53ca\u94f8\u6001C0\u9ad8\u71b5\u5408\u91d1\u7684\u5de5\u7a0b\u5e94\u529b\u5e94\u53d8\u66f2\u7ebf<\/p>\n<p>(b) \u56fa\u6eb6\u6001C3.3\u5408\u91d1\u7684\u80cc\u6563\u5c04\u56fe\u548cEDS\u80fd\u8c31<\/p>\n<p><strong>\u56fe<\/strong><strong>8.<\/strong><strong>\u9ad8\u78b3\u9ad8\u71b5\u5408\u91d1\u548c\u5404\u79cd\u94a2\u7684\u65ad\u88c2\u4f38\u957f\u7387\u53ca\u6781\u9650\u6297\u62c9\u5f3a\u5ea6\u7684\u6bd4\u8f83<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-123100\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image017.jpg\" alt=\"\" width=\"600\" height=\"418\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image017.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/01\/image017-300x209.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u7ea2\u8272\u65b9\u5757\u8868\u793a\u94f8\u6001\u548c\u56fa\u6eb6\u6001C3.3\u9ad8\u71b5\u5408\u91d1\u7684\u673a\u68b0\u6027\u80fd<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u6587\u7cfb\u7edf\u7814\u7a76\u4e86\u78b3\u5bf9Fe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub>\u9ad8\u71b5\u5408\u91d1\u5fae\u89c2\u7ec4\u7ec7\u548c\u673a\u68b0\u6027\u80fd\u7684\u5f71\u54cd\u3002\u9ad8\u78b3\u5408\u91d1\uff08\u5927\u7ea63.3 at.%\uff09\u5728\u63d0\u9ad8\u5c48\u670d\u5f3a\u5ea6\u7684\u540c\u65f6\u4e5f\u63d0\u9ad8\u4e86\u6781\u9650\u6297\u62c9\u5f3a\u5ea6\u4ee5\u53ca\u5851\u6027\u3002\u8fd9\u662f\u56e0\u4e3a\u95f4\u9699\u78b3\u539f\u5b50\u80fd\u591f\u6291\u5236\u4f4d\u9519\u8fd0\u52a8\u5e76\u4fc3\u8fdb\u9ad8\u71b5\u5408\u91d1\u4e2d\u7684\u53d8\u5f62\u8bf1\u53d1\u5b6a\u6676\u7684\u53d1\u751f\u3002\u94f8\u6001\u548c\u56fa\u6eb6\u6001\u7684(Fe<sub>40<\/sub>Mn<sub>40<\/sub>Co<sub>10<\/sub>Cr<sub>10<\/sub>)<sub>96.7<\/sub>C<sub>3.3<\/sub>\u9ad8\u71b5\u5408\u91d1\u7684\u7efc\u5408\u673a\u68b0\u6027\u80fd\u4f18\u4e8e\u5927\u591a\u6570\u7684\u9ad8\u71b5\u5408\u91d1\u548c\u91d1\u5c5e\u6750\u6599\u3002\u6b64\u7814\u7a76\u4e3a\u5f00\u53d1\u9ad8\u6027\u80fd\u9ad8\u71b5\u5408\u91d1\u63d0\u4f9b\u4e86\u65b0\u7684\u601d\u8def\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"http:\/\/www.sciencedirect.com\/science\/article\/pii\/S0921509318300650\" target=\"_blank\" rel=\"noopener\">Heavy carbon alloyed FCC-structured high entropy alloy with excellent combination of strength and ductility<\/a> (Mater. Sci. Eng. A, 2018, DOI: 10.1016\/j.msea.2018.01.045 )<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u53f2\u79c0\u4e3d\u7f16\u8bd1\uff0c\u4e07\u946b\u6d69\u5ba1\u6838\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u3002<\/a><\/p>\n<p>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u4e0a\u6d4b\u8bd5\u8c37<\/a>\uff01<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u8fd1\u5e74\u6765\uff0c\u9ad8\u71b5\u5408\u91d1\u56e0\u5176\u4f5c\u4e3a\u9ad8\u6027\u80fd\u7ed3\u6784\u6750\u6599\u7684\u6f5c\u5728\u5e94\u7528\u800c\u5907\u53d7\u5173\u6ce8\u3002FCC\uff08\u9762\u5fc3\u7acb\u65b9\uff09\u7ed3\u6784\u7684\u9ad8\u71b5\u5408\u91d1\u5177\u6709\u8f83\u597d\u7684\u5851\u6027\u548c\u4f4e\u6e29\u65ad\u88c2\u97e7\u6027\uff0c\u662f\u76ee\u524d\u5e7f\u4e3a\u7814\u7a76\u7684\u5408\u91d1\u4e4b\u4e00\u3002\u7136&#8230;<\/p>\n","protected":false},"author":230,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[306],"class_list":["post-123092","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-high-entropy"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/123092"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/230"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=123092"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/123092\/revisions"}],"predecessor-version":[{"id":123600,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/123092\/revisions\/123600"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=123092"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=123092"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=123092"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}