{"id":124789,"date":"2018-02-08T06:30:29","date_gmt":"2018-02-07T22:30:29","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=124789"},"modified":"2018-02-06T10:48:44","modified_gmt":"2018-02-06T02:48:44","slug":"metall-mater-trans-a%ef%bc%9a%e7%84%8a%e6%8e%a5%e6%96%b9%e6%b3%95%e5%92%8c%e7%84%8a%e6%8e%a5%e6%9d%90%e6%96%99%e5%af%b9inconel-625%e5%92%8c316l%e4%b8%8d%e9%94%88%e9%92%a2%e5%bc%82%e7%a7%8d%e6%8e%a5","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=124789","title":{"rendered":"Metall. Mater. Trans. A\uff1a\u710a\u63a5\u65b9\u6cd5\u548c\u710a\u63a5\u6750\u6599\u5bf9Inconel 625\u548c316L\u4e0d\u9508\u94a2\u5f02\u79cd\u63a5\u5934\u6027\u80fd\u7684\u7814\u7a76"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>Inconel 625\u662f\u4e00\u79cd\u954d\u57fa\u56fa\u6eb6\u5408\u91d1\uff0c\u5177\u6709\u826f\u597d\u7684\u7269\u7406\u3001\u5316\u5b66\u6027\u80fd\uff0c\u5982\u5f3a\u5ea6\u9ad8\u3001\u8010\u8150\u8680\uff0c\u9ad8\u6e29\u8815\u53d8\u6027\u80fd\u597d\u7b49\u4f17\u591a\u4f18\u70b9\uff0c\u6240\u4ee5\u5e7f\u6cdb\u5e94\u7528\u5728\u822a\u7a7a\u822a\u5929\u3001\u77f3\u6cb9\u5316\u5de5\u548c\u8239\u8230\u7b49\u3002316L\u4e0d\u9508\u94a2\u5177\u6709\u8010\u8150\u8680\u3001\u5236\u9020\u6210\u672c\u4f4e\u7b49\u4f18\u70b9\uff0c\u6240\u4ee5\u5728\u77f3\u6cb9\u3001\u5316\u5de5\u548c\u6c14\u4f53\u5bb9\u5668\u7b49\u884c\u4e1a\u6709\u5e7f\u6cdb\u5e94\u7528\u3002\u800c\u76ee\u524d\u9488\u5bf9\u4e0d\u9508\u94a2\u7684\u710a\u63a5\u7814\u7a76\u4e3b\u8981\u96c6\u4e2d\u5728\u542b\u78b3\u91cf\u8f83\u9ad8\u7684310\u4e0d\u9508\u94a2\uff0c\u8fd8\u6ca1\u6709\u7814\u7a76\u4eba\u5458\u5bf9316L\u4e0d\u9508\u94a2\u548cInconel 625\u5408\u91d1\u5f02\u79cd\u63a5\u5934\u710a\u63a5\u6027\u8fdb\u884c\u7814\u7a76\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u4f0a\u65af\u5170\u81ea\u7531\u5927\u5b66<\/strong><strong>Reza Derakhshandeh-Haghighi<\/strong>\uff08\u901a\u8baf\u4f5c\u8005\uff09\u5728<strong>Metallurgical and Materials Transactions A<\/strong>\u53d1\u8868\u4e86\u6700\u65b0\u7684\u7814\u7a76\u6210\u679c\u201c<strong>Evaluating the Properties of Dissimilar Metal Welding Between Inconel 625 and 316L Stainless Steel by Applying Different Welding Methods and Consumables<\/strong>\u201d\u3002\u5728\u8be5\u6587\u4e2d\uff0c\u7814\u7a76\u4eba\u5458\u5229\u7528\u4e0d\u540c\u7684\u8868\u5f81\u6280\u672f\u7814\u7a76\u4e86\u710a\u63a5\u6750\u6599\u5bf9316L\u4e0d\u9508\u94a2\u548cInconel 625\u5408\u91d1\u5f02\u79cd\u63a5\u5934\u624b\u5de5\u7535\u5f27\u710a\u548c\u94a8\u6781\u60f0\u6027\u6c14\u4f53\u4fdd\u62a4\u710a\u7684\u710a\u63a5\u63a5\u5934\u7ec4\u7ec7\u4e0e\u6027\u80fd\u7684\u5173\u7cfb\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe1 \u710a\u63a5\u4ef6\u5761\u53e3\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124790\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/1-123.png\" alt=\"\" width=\"600\" height=\"280\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/1-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/1-123-300x140.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\n <strong>\u56fe2 \u710a\u63a5\u63a5\u5934\u6a2a\u622a\u9762\u5b8f\u89c2\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124791\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/2-123.png\" alt=\"\" width=\"600\" height=\"396\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/2-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/2-123-300x198.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\u00a0\uff08a\uff09\u624b\u5de5\u7535\u5f27\u710a\u7684\u710a\u63a5\u63a5\u5934\u6a2a\u622a\u9762\uff08\u710a\u6761\u4e3aERNiCrMo-3\uff09<\/p>\n<p>\uff08b\uff09\u94a8\u6781\u60f0\u6027\u6c14\u4f53\u4fdd\u62a4\u710a\u7684\u710a\u63a5\u63a5\u5934\u6a2a\u622a\u9762\uff08\u710a\u4e1d\u4e3aERNiCrMo-3\uff09<\/p>\n<p><strong>\u56fe3 \u672a\u7ecf\u5904\u7406\u7684\u6bcd\u6750\u7684\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124792\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/3-123.png\" alt=\"\" width=\"600\" height=\"227\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/3-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/3-123-300x114.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u672a\u7ecf\u5904\u7406\u7684Inconel625\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p>\uff08b\uff09\u672a\u7ecf\u5904\u7406\u7684316L\u4e0d\u9508\u94a2\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p><strong>\u56fe4 Inconel625\u6bcd\u6750\u7684\u626b\u63cf\u7535\u955c\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124793\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/4-123.png\" alt=\"\" width=\"600\" height=\"669\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/4-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/4-123-269x300.png 269w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe5 \u663e\u5fae\u7ec4\u7ec7\u4e2d\u78b3\u5316\u7269\u7684EDS\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124794\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/5-123.png\" alt=\"\" width=\"600\" height=\"239\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/5-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/5-123-300x120.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5757\u72b6\u78b3\u5316\u7269\u7684EDS\u56fe<\/p>\n<p>\uff08b\uff09\u6746\u72b6\u78b3\u5316\u7269\u7684EDS\u56fe<\/p>\n<p><strong>\u56fe6 ERNiCrMo-3\u710a\u4e1d\uff0cGTA\u710a\u7f1d\u5149\u955c\u4e0b\u7684\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124795\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/6-123.png\" alt=\"\" width=\"600\" height=\"223\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/6-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/6-123-300x112.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u710a\u7f1d\u663e\u5fae\u7ec4\u7ec7\uff08\u5965\u6c0f\u4f53\u4e0a\u6709\u679d\u6676\u95f4\u78b3\u5316\u7269\uff09<\/p>\n<p>\uff08b\uff09\u710a\u7f1d\u5728\u9ad8\u500d\u955c\u4e0b\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p><strong>\u56fe7 ERNiCrMo-3\u710a\u4e1d\uff0cGTA\u710a\u7f1d\u626b\u63cf\u7535\u955c\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124796\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/7-123.png\" alt=\"\" width=\"600\" height=\"220\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/7-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/7-123-300x110.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u4f7f\u7528ERNiCrMo-3\u710a\u4e1d\uff0cGTA\u710a\u7f1d\u7684\u6811\u679d\u6676\u9ad8\u500d\u4e0b\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p>\uff08b\uff09\u710a\u7f1d\u4e2d\u5fc3\u7ebf\u5230\u7194\u5408\u533a\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p>\uff08c\uff09\u4f7f\u7528ERNiCrMo-3\u710a\u4e1d\uff0cGTA\u710a\u7f1d\u7684\u7b49\u8f74\u6676\u9ad8\u500d\u4e0b\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p><strong>\u56fe8 ERNiCrMo-3\u710a\u4e1d\uff0cGTA\u710a\u7f1d\u91d1\u5c5e\u7684EDS\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124797\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/8-123.png\" alt=\"\" width=\"600\" height=\"236\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/8-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/8-123-300x118.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u679d\u6676\u95f4\u7269\u8d28\u7684EDS\u5206\u6790\uff08\u56fe7\u4e2d\u7bad\u5934\u201cA\u201d\u5904\uff09<\/p>\n<p>\uff08b\uff09\u679d\u6676\u6838\u7684EDS\u5206\u6790\uff08\u56fe7\u4e2d\u7bad\u5934\u201cB\u201d\u5904\uff09<\/p>\n<p><strong>\u56fe9 ERSS-316L\u710a\u4e1d\uff0cGTA\u710a\u7f1d\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124798\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/9-123.png\" alt=\"\" width=\"600\" height=\"321\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/9-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/9-123-300x161.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u710a\u7f1d\u67f1\u72b6\u6676\u7684\u626b\u63cf\u7535\u955c\u56fe<\/p>\n<p>\uff08b\uff09\u679d\u6676\u95f4\u663e\u5fae\u7ec4\u7ec7\u4e2d\u03b4\u94c1\u7d20\u4f53\u7684\u5149\u955c\u56fe<\/p>\n<p><strong>\u56fe10 ENiCrMo-3\u710a\u6761\u8fdb\u884c\u624b\u5de5\u7535\u5f27\u710a\u5f97\u5230\u7684\u710a\u7f1d<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124799\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/10-123.png\" alt=\"\" width=\"600\" height=\"281\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/10-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/10-123-300x141.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u710a\u7f1d\u7684\u663e\u5fae\u7ec4\u7ec7\uff08\u5b58\u5728laves\u76f8\uff09<\/p>\n<p>\uff08b\uff09\u5de6\u56fe\u7bad\u5934\u201cA\u201d\u5904\u7684EDS\u5206\u6790<\/p>\n<p><strong>\u56fe11 \u70ed\u8f93\u5165\u5bf9\u710a\u7f1d\u663e\u5fae\u7ec4\u7ec7\u7684\u5f71\u54cd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124800\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/11-123.png\" alt=\"\" width=\"600\" height=\"354\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/11-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/11-123-300x177.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u94a8\u6781\u60f0\u6027\u6c14\u4f53\u4fdd\u62a4\u710a\u5f97\u5230\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p>\uff08b\uff09\u624b\u5de5\u7535\u5f27\u710a\u5f97\u5230\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p><strong>\u56fe12 \u710a\u7f1d\u548c\u6bcd\u6750Inconel 625\u754c\u9762\u7684\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124801\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/12-123.png\" alt=\"\" width=\"600\" height=\"331\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/12-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/12-123-300x166.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u710a\u7f1d\u548c\u6bcd\u6750Inconel 625\u8f83\u597d\u7194\u5408<\/p>\n<p>\uff08b\uff09\u710a\u7f1d\u548c\u6bcd\u6750Inconel 625\u51e0\u4e4e\u4e0d\u7194\u5408<\/p>\n<p><strong>\u56fe13 316L\u4e0d\u9508\u94a2\u6bcd\u6750\u548cERSS316L\u710a\u7f1d\u754c\u9762\u7684\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124802\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/13-123.png\" alt=\"\" width=\"600\" height=\"331\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/13-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/13-123-300x166.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09316L\u4e0d\u9508\u94a2\u6bcd\u6750\u548cERSS316L\u710a\u63a5\u6750\u6599\u5b8c\u5168\u7194\u5408\u65f6\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p>\uff08b\uff09316L\u4e0d\u9508\u94a2\u6bcd\u6750\u548cERSS316L\u710a\u63a5\u6750\u6599\u5f88\u96be\u7194\u5408\u65f6\u7684\u663e\u5fae\u7ec4\u7ec7<\/p>\n<p><strong>\u56fe14 316L\u4e0d\u9508\u94a2\u6bcd\u6750\u548cERSS316L\u710a\u63a5\u754c\u9762\u5916\u5ef6\u751f\u957f\u65f6\u7684\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124803\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/14-123.png\" alt=\"\" width=\"600\" height=\"454\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/14-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/14-123-300x227.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe15 316L\u6bcd\u6750\u548cERNiCrMo-3\u710a\u63a5\u6750\u6599\u975e\u7194\u5408\u533a\u7684\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124804\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/15-123.png\" alt=\"\" width=\"600\" height=\"348\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/15-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/15-123-300x174.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u710a\u63a5\u65b9\u6cd5\u4e3a\u94a8\u6781\u60f0\u6027\u6c14\u4f53\u4fdd\u62a4\u710a\u65f6\u7684\u672a\u7194\u5408\u533a<\/p>\n<p>\uff08b\uff09\u710a\u63a5\u65b9\u6cd5\u4e3a\u624b\u5de5\u7535\u5f27\u710a\u65f6\u7684\u672a\u7194\u5408\u533a<\/p>\n<p><strong>\u56fe16 Inconel 625\u70ed\u5f71\u54cd\u533a\u7c97\u5316\u7684\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124805\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/16-123.png\" alt=\"\" width=\"600\" height=\"221\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/16-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/16-123-300x111.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \uff08a\uff09\u94a8\u6781\u60f0\u6027\u6c14\u4f53\u4fdd\u62a4\u710a\u710a\u63a5\u63a5\u5934<\/p>\n<p>\uff08b\uff09\u624b\u5de5\u7535\u5f27\u710a\u710a\u63a5\u63a5\u5934<\/p>\n<p><strong>\u56fe17 \u70ed\u5f71\u54cd\u533a\u78b3\u5316\u7269\u8f6c\u53d8\u7684\u663e\u5fae\u7ec4\u7ec7<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124806\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/17-123.png\" alt=\"\" width=\"600\" height=\"320\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/17-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/17-123-300x160.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Inconel625\u70ed\u5f71\u54cd\u533a\u78b3\u5316\u7269\u6d88\u5931\u7684\u626b\u63cf\u7535\u955c\u56fe<\/p>\n<p>\uff08b\uff09\u6676\u7c92\u8fb9\u754c\u6cbf\u7ec6\u5c0f\u78b3\u5316\u7269\u6790\u51fa\u7c97\u5927\u78b3\u5316\u7269\u7684\u5149\u955c\u56fe<\/p>\n<p><strong>\u56fe18 \u710a\u7f1d\u786c\u5ea6\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-124807\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/18-123.png\" alt=\"\" width=\"600\" height=\"516\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/18-123.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/18-123-300x258.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u5728ERNiCrMo-3\u710a\u6750\u51dd\u56fa\u8fc7\u7a0b\u4e2d\uff0cNb\u548cMo\u4f1a\u8fdc\u79bb\u679d\u6676\u7684\u6676\u6838\u5e76\u8fdc\u79bb\u679d\u6676\u7684\u6676\u95f4\uff0c\u800cERSS316L\u710a\u6750\u5b58\u5728\u5c11\u91cf\u504f\u6790\u7684\u5143\u7d20\u3002\u6240\u4ee5\u901a\u8fc7\u5b9e\u73b0\u8fc7\u51b7\uff0c\u8fdb\u800c\u5b9e\u73b0\u4ece\u5305\u6676\u5230\u6811\u679d\u6676\u6216\u7b49\u8f74\u6676\u7684\u8f6c\u53d8\u662f\u4e0d\u592a\u53ef\u80fd\u3002\u91c7\u7528\u94a8\u6781\u60f0\u6027\u6c14\u4f53\u4fdd\u62a4\u710a\u65f6\uff0c\u964d\u4f4e\u70ed\u8f93\u5165\u4f1a\u83b7\u5f97\u66f4\u5927\u7684\u51b7\u5374\u901f\u5ea6\u3001\u7ec6\u5c0f\u7684\u663e\u5fae\u7ec4\u7ec7\u5e76\u80fd\u964d\u4f4eNb\u7684\u504f\u6790\u3002\u91c7\u7528ERNiCrMo-3\u710a\u4e1d\u8fdb\u884cGMAW\u710a\u63a5\u5f97\u5230\u7684\u63a5\u5934\u5177\u6709\u6700\u9ad8\u7684\u6297\u62c9\u5f3a\u5ea6\u3001\u4f38\u957f\u7387\uff0c\u51b2\u51fb\u529f\u6700\u9ad8\u3002\u800c\u4f7f\u7528ERSS316L\u710a\u4e1d\u8fdb\u884cGMAW\u710a\u63a5\u5f97\u5230\u7684\u63a5\u5934\u5177\u6709\u6700\u4f4e\u7684\u6297\u62c9\u5f3a\u5ea6\u3001\u6700\u5c0f\u7684\u4f38\u957f\u7387\u548c\u6700\u4f4e\u7684\u51b2\u51fb\u529f\u3002\u624b\u5de5\u7535\u5f27\u710a\u5f97\u5230\u7684\u710a\u63a5\u63a5\u5934\u6bd4GMAW\u710a\u63a5\u5f97\u5230\u7684\u63a5\u5934\u6027\u80fd\u8981\u5dee\uff0c\u8fd9\u662f\u56e0\u4e3aSMAW\u710a\u63a5\u5f97\u5230\u7684\u710a\u7f1d\u6676\u7c92\u8f83\u7c97\u5927\u3002\u6240\u4ee5\u91c7\u7528ERNiCrMo-3\u710a\u4e1d\u8fdb\u884cGMAW\u710a\u63a5\u662f\u6700\u9002\u5408\u8fde\u63a5Inconel 625\u5408\u91d1\u548c316L\u4e0d\u9508\u94a2\u7684\u710a\u63a5\u65b9\u6cd5\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5<\/strong>\uff1a<a href=\"https:\/\/link.springer.com\/article\/10.1007\/s11661-018-4469-7\" target=\"_blank\" rel=\"noopener\">Evaluating the Properties of Dissimilar Metal Welding Between Inconel 625 and 316L Stainless Steel by Applying Different Welding Methods and Consumables<\/a>\uff08Metallurgical and Materials Transactions A\uff0c2018\uff0cdoi.org\/10.1007\/s11661-018-4469-7\uff09\u3002<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u91d1\u5c5e\u7ec4 \u6768\u6811 \u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u4eba\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1aRDD-2011-CHERISH\uff0c\u4efb\u4e39\u4e39\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/p>\n<p>\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 Inconel 625\u662f\u4e00\u79cd\u954d\u57fa\u56fa\u6eb6\u5408\u91d1\uff0c\u5177\u6709\u826f\u597d\u7684\u7269\u7406\u3001\u5316\u5b66\u6027\u80fd\uff0c\u5982\u5f3a\u5ea6\u9ad8\u3001\u8010\u8150\u8680\uff0c\u9ad8\u6e29\u8815\u53d8\u6027\u80fd\u597d\u7b49\u4f17\u591a\u4f18\u70b9\uff0c\u6240\u4ee5\u5e7f\u6cdb\u5e94\u7528\u5728\u822a\u7a7a\u822a\u5929\u3001\u77f3\u6cb9\u5316\u5de5\u548c\u8239\u8230&#8230;<\/p>\n","protected":false},"author":7335,"featured_media":124807,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[19],"class_list":["post-124789","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-steel"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/124789"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7335"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=124789"}],"version-history":[{"count":9,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/124789\/revisions"}],"predecessor-version":[{"id":125037,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/124789\/revisions\/125037"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/124807"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=124789"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=124789"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=124789"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}