{"id":126854,"date":"2018-02-26T14:00:58","date_gmt":"2018-02-26T06:00:58","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=126854"},"modified":"2018-02-24T20:06:32","modified_gmt":"2018-02-24T12:06:32","slug":"adv-funct-mater-%ef%bc%9a%e9%80%9a%e8%bf%87%e8%a1%a8%e9%9d%a2%e7%94%b5%e8%8d%b7%e8%bd%ac%e7%a7%bb%e6%8e%ba%e6%9d%82%e7%a1%ab%e5%8c%96%e9%95%89%e7%ba%b3%e7%b1%b3%e5%b8%a6%e6%9e%84%e7%ad%91%e8%b6%85","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=126854","title":{"rendered":"Adv. Funct. Mater.\uff1a\u901a\u8fc7\u8868\u9762\u7535\u8377\u8f6c\u79fb\u63ba\u6742\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u6784\u7b51\u8d85\u5bbd\u53ef\u8c03\u529f\u7387\u7684\u963b\u53d8\u5b58\u50a8\u5668"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u5728\u8fc7\u53bb\u7684\u51e0\u5341\u5e74\u4e2d\uff0c\u4fe1\u606f\u7206\u70b8\u6027\u589e\u957f\uff0c\u6570\u636e\u5b58\u53d6\u8fc7\u7a0b\u4ea7\u751f\u7684\u80fd\u8017\u53d8\u5f97\u4e0d\u53ef\u5ffd\u89c6\u3002\u4f20\u7edf\u7684\u57fa\u4e8e\u91d1\u5c5e-\u7edd\u7f18\u4f53-\u91d1\u5c5e\u7ed3\u6784\u7684\u963b\u53d8\u5b58\u50a8\u5668\u5177\u6709\u5f88\u9ad8\u7684\u5de5\u4f5c\u7535\u6d41\uff0c\u56e0\u6b64\u6570\u636e\u5b58\u53d6\u8fc7\u7a0b\u4e2d\u4fe1\u53f7\u53ef\u4ee5\u5728\u6ca1\u6709\u653e\u5927\u5668\u7684\u60c5\u51b5\u4e0b\u88ab\u76f4\u63a5\u8bfb\u53d6\uff0c\u4f46\u8fd9\u4e5f\u5c06\u4e0d\u53ef\u907f\u514d\u5730\u4f1a\u4ea7\u751f\u5927\u7684\u80fd\u8017\u3002\u4e3a\u4e86\u5728\u5404\u79cd\u5b9e\u9645\u5e94\u7528\u4e2d\u8282\u7ea6\u80fd\u8017\uff0c\u5408\u7406\u63a7\u5236\u963b\u53d8\u5b58\u50a8\u5668\u7684\u80fd\u8017\u662f\u975e\u5e38\u5fc5\u8981\u7684\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u6765\u81ea<strong>\u82cf\u5dde\u5927\u5b66\u7684\u5f20\u6653\u5b8f\u6559\u6388\uff08\u901a\u8baf\u4f5c\u8005\uff09\u548c\u63ed\u5efa\u80dc\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u7684\u7814\u7a76\u56e2\u961f\u5728<strong><em>Adv. Funct. Mater.<\/em><\/strong>\u53d1\u8868\u4e86\u9898\u4e3a\u201c<strong>CdS Nanoribbon-Based Resistive Switches with Ultrawidely Tunable Power by Surface Charge Transfer Doping<\/strong>\u201d\u7684\u6587\u7ae0\u3002\u8be5\u7814\u7a76\u56e2\u961f\u901a\u8fc7\u7535\u8377\u8f6c\u79fb\u63ba\u6742\u786b\u5316\u9549\u7eb3\u7c73\u5e26\uff0c\u5e76\u4ee5\u63ba\u6742\u7684\u7eb3\u7c73\u5e26\u4f5c\u4e3a\u53d8\u963b\u5668\u6784\u7b51\u963b\u53d8\u5b58\u50a8\u5668\u4ee5\u63a7\u5236\u5176\u5de5\u4f5c\u7535\u6d41\u548c\u529f\u8017\u3002\u901a\u8fc7\u63a7\u5236\u8868\u9762\u63ba\u6742\u5242\u6c27\u5316\u94bc\u7684\u63ba\u6742\u6d53\u5ea6\uff0c\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684\u7535\u5bfc\u7387\u53ef\u4ee5\u57289\u4e2a\u6570\u91cf\u7ea7\u7684\u5bbd\u8303\u56f4\u5185\u8c03\u8282\uff0c\u5e76\u663e\u793a\u51fa\u4ece\u7edd\u7f18\u4f53\u5230\u534a\u5bfc\u4f53\u548c\u5bfc\u4f53\u7684\u8f6c\u53d8\u3002\u5728\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7535\u5bfc\u7387\u53ef\u63a7\u7684\u57fa\u7840\u4e0a\uff0c\u5236\u9020\u7684\u963b\u53d8\u5b58\u50a8\u5668\u7684\u529f\u8017\u53ef\u4ee5\u5728\u8d85\u5bbd\u7684\u8303\u56f4\u5185\u8c03\u8282\uff0c\u5176\u4e2d1\u94a0\u74e6\u7684\u529f\u8017\u6700\u4f4e\u503c\u662f\u76ee\u524d\u62a5\u9053\u7684\u963b\u53d8\u5b58\u50a8\u5668\u7684\u6700\u4f4e\u503c\uff0c0.1\u6beb\u74e6\u7684\u529f\u8017\u6700\u9ad8\u503c\u63a5\u8fd1\u4e8e\u91d1\u5c5e-\u7edd\u7f18\u4f53-\u91d1\u5c5e\u7ed3\u6784\u963b\u53d8\u5b58\u50a8\u5668\u7684\u529f\u8017\u3002\u9274\u4e8e\u8868\u9762\u7535\u8377\u8f6c\u79fb\u63ba\u6742\u65b9\u6cd5\u7684\u9ad8\u5ea6\u53ef\u63a7\u6027\uff0c\u8be5\u5de5\u4f5c\u5bf9\u53d1\u5c55\u9ad8\u80fd\u6548\u3001\u6027\u80fd\u53ef\u8c03\u548c\u591a\u529f\u80fd\u7684\u534a\u5bfc\u4f53\u7eb3\u7c73\u963b\u53d8\u5b58\u50a8\u5668\u5177\u6709\u91cd\u8981\u7684\u610f\u4e49\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong>1<\/strong><strong>\uff1a\u786b\u5316\u9549\u548c\u6c27\u5316\u94bc\u4e4b\u95f4\u7684\u8868\u9762\u7535\u8377\u8f6c\u79fb<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-126855 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/11-7.jpg\" alt=\"\" width=\"600\" height=\"341\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/11-7.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/11-7-300x171.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a): \u786b\u5316\u9549\u548c\u6c27\u5316\u94bc\u4f53\u7cfb\u7684\u5dee\u5206\u7535\u8377\u5206\u5e03\u56fe\uff1b<\/p>\n<p>(b-c): \u672c\u5f81\u53ca\u6c27\u5316\u94bc\u63ba\u6742\u786b\u5316\u9549\u7684\u80fd\u5e26\u7ed3\u6784\uff1b<\/p>\n<p>(d): \u672c\u5f81\u53ca\u6c27\u5316\u94bc\u63ba\u6742\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684XPS\u8c31\uff1b<\/p>\n<p>(e): \u6c27\u5316\u94bc\u63ba\u6742\u786b\u5316\u9549\u7684SNOM\u6d4b\u8bd5\u793a\u610f\u56fe\uff1b<\/p>\n<p>(f): SNOM\u6d4b\u91cf\u4e2d\u6563\u5c04\u5149\u4e8c\u6b21\u8c10\u6ce2\u7684\u632f\u5e45\uff1b<\/p>\n<p>(g): \u8ba1\u7b97\u5f97\u5230\u7684\u6563\u5c04\u5149\u4e8c\u6b21\u8c10\u6ce2\u7684\u632f\u5e45-\u786b\u5316\u9549\u8f7d\u6d41\u5b50\u6d53\u5ea6\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>2<\/strong><strong>\uff1a\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684\u7535\u5bfc\u8c03\u5236<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-126856 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/22-8.jpg\" alt=\"\" width=\"600\" height=\"427\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/22-8.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/22-8-300x214.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a): \u901a\u8fc7\u8868\u9762\u7535\u8377\u8f6c\u79fb\u63ba\u6742\u63a7\u5236\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7535\u5bfc\u7684\u5668\u4ef6\u793a\u610f\u56fe\uff1b<\/p>\n<p>(b): \u672a\u63ba\u6742\u7684\u548c\u63ba\u6742\u7684\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684I-V\u66f2\u7ebf\uff1b<\/p>\n<p>(c): \u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684\u7535\u963b\u7387\u4e0e\u63ba\u6742\u5242\u6c27\u5316\u94bc\u6eb6\u6db2\u6d53\u5ea6\u7684\u5173\u7cfb\uff1b<\/p>\n<p>(d-f): \u4e0d\u540c\u63ba\u6742\u7a0b\u5ea6\u7684\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7535\u963b\u7387\u7684\u6e29\u5ea6\u4f9d\u8d56\u6027\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>3<\/strong><strong>\uff1a\u57fa\u4e8e\u6c27\u5316\u94bc\u7eb3\u7c73\u70b9\u63ba\u6742\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684\u963b\u53d8\u50a8\u5b58\u5668<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-126857 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/33-5.jpg\" alt=\"\" width=\"600\" height=\"283\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/33-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/33-5-300x142.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a): \u963b\u53d8\u50a8\u5b58\u5668\u793a\u610f\u56fe\uff1b<\/p>\n<p>(b): \u963b\u53d8\u50a8\u5b58\u5668\u7684\u5149\u5b66\u663e\u5fae\u955c\u56fe\u50cf\uff1b<\/p>\n<p>(c): \u963b\u53d8\u50a8\u5b58\u5668\u7684I-V\u66f2\u7ebf\uff1b\u00a0\u00a0\u00a0\u00a0<\/p>\n<p>(d-e): \u963b\u53d8\u50a8\u5b58\u5668\u7684\u4fdd\u6301\u548c\u8010\u4e45\u6027\u6d4b\u8bd5\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>4<\/strong><strong>\uff1a<\/strong><strong>\u91d1<\/strong><strong>\/<\/strong><strong>\u94dc<\/strong><strong>\/<\/strong><strong>\u63ba\u6742\u786b\u5316\u9549\u7eb3\u7c73\u5e26<\/strong><strong>\/<\/strong><strong>\u94f6\u57fa\u963b\u53d8\u5b58\u50a8\u5668\u7684\u5de5\u4f5c\u673a\u7406<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-126858 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/44-4.jpg\" alt=\"\" width=\"600\" height=\"456\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/44-4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/44-4-300x228.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a): \u94f6\/\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u754c\u9762\u7684STEM\u56fe\uff1b<\/p>\n<p>(b-d): \u94f6\/\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u754c\u9762\u7684EDS\u5143\u7d20\u5206\u5e03\u56fe\uff1b<\/p>\n<p>(e): \u94f6\/\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u754c\u9762\u7684HRTEM\u56fe\uff1b<\/p>\n<p>(f): \u4ee50.01V\/s\u7684\u626b\u63cf\u901f\u5ea6\u6d4b\u91cf\u7684\u963b\u53d8\u5b58\u50a8\u5668\u7684<em>I-V<\/em>\u66f2\u7ebf\uff1b<\/p>\n<p>(g): \u91d1\/\u94dc\/\u63ba\u6742\u786b\u5316\u9549\u7eb3\u7c73\u5e26\/\u94f6\u57fa\u963b\u53d8\u5b58\u50a8\u5668\u7684\u963b\u53d8\u8fc7\u7a0b\u793a\u610f\u56fe\uff1b<\/p>\n<p>(h): \u4e0d\u540c\u6d4b\u8bd5\u6e29\u5ea6\u4e0b\u963b\u53d8\u5b58\u50a8\u5668\u7684<em>I-V<\/em>\u7279\u6027\uff1b<\/p>\n<p>(i-k): \u9608\u503c\u7535\u538b\u53ca\u5de5\u4f5c\u7535\u6d41\u7684\u6e29\u5ea6\u4f9d\u8d56\u5173\u7cfb\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>5<\/strong><strong>\uff1a\u91d1<\/strong><strong>\/<\/strong><strong>\u94dc<\/strong><strong>\/<\/strong><strong>\u63ba\u6742\u786b\u5316\u9549\u7eb3\u7c73\u5e26<\/strong><strong>\/<\/strong><strong>\u94f6\u57fa\u963b\u53d8\u5b58\u50a8\u5668\u7684\u529f\u8017\u8c03\u5236<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-126859 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/55-3.jpg\" alt=\"\" width=\"600\" height=\"336\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/55-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/55-3-300x168.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a): \u4e0d\u540c\u63ba\u6742\u7a0b\u5ea6\u963b\u53d8\u5b58\u50a8\u5668\u7684<em>I-V<\/em>\u66f2\u7ebf\uff1b<\/p>\n<p>(b-c): \u5df2\u62a5\u9053\u7684\u963b\u53d8\u5b58\u50a8\u5668\u5de5\u4f5c\u7535\u6d41\u3001\u529f\u8017\u53ca\u5de5\u4f5c\u7535\u538b\u7684\u603b\u7ed3\uff1b<\/p>\n<p>(d,e): \u4e0d\u540c\u63ba\u6742\u7a0b\u5ea6\u963b\u53d8\u5b58\u50a8\u5668\u7684\u4fdd\u6301\u548c\u8010\u4e45\u6027\u6d4b\u8bd5\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>6<\/strong><strong>\uff1a\u57fa\u4e8e\u63ba\u6742\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684\u96c6\u6210\u548c\u67d4\u6027\u5668\u4ef6<\/strong><\/p>\n<p><strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-126861 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/66-3.jpg\" alt=\"\" width=\"600\" height=\"524\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/66-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/02\/66-3-300x262.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/p>\n<p>(a): \u5355\u6839\u7eb3\u7c73\u5e26\u4e0a\u96c6\u62106\u7ec4\u963b\u53d8\u5b58\u50a8\u5668\u7684\u5149\u5b66\u663e\u5fae\u955c\u56fe\u50cf\uff1b<\/p>\n<p>(b): \u96c6\u6210\u76846\u7ec4\u963b\u53d8\u5b58\u50a8\u5668\u7684<em>I-V<\/em>\u66f2\u7ebf\uff1b<\/p>\n<p>(c): \u5728\u67d4\u6027PET\u886c\u5e95\u4e0a\u6784\u7b51\u7684\u963b\u53d8\u5b58\u50a8\u5668\uff1b<\/p>\n<p>(d): \u963b\u53d8\u5b58\u50a8\u5668\u5728\u4e0d\u540c\u5f2f\u66f2\u534a\u5f84\u4e0b\u6d4b\u91cf\u7684<em>I-V<\/em>\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u8be5\u7814\u7a76\u56e2\u961f\u901a\u8fc7\u5728\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u4e0a\u65cb\u6d82\u8868\u9762\u63ba\u6742\u5242\u6c27\u5316\u94bc\u7eb3\u7c73\u70b9\u6765\u5b9e\u73b0\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7535\u963b\u7387\u7684\u5bbd\u8303\u56f4\u8c03\u5236\u3002\u901a\u8fc7\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\uff0cXPS\u548cSNOM\u6d4b\u8bd5\u8bc1\u660e\u4e86\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u548c\u6c27\u5316\u94bc\u7eb3\u7c73\u70b9\u4e4b\u95f4\u7684\u7535\u8377\u8f6c\u79fb\u73b0\u8c61\u3002\u901a\u8fc7\u589e\u5927\u7535\u8377\u8f6c\u79fb\u7684\u7a0b\u5ea6\uff0c\u5373\u6c27\u5316\u94bc\u7684\u63ba\u6742\u91cf\uff0c\u53ef\u4ee5\u628a\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684\u7535\u963b\u7387\u4ece10<sup>6<\/sup>\u964d\u4f4e\u523010<sup>-3 <\/sup>\u03a9\u2022cm\uff0c\u8fd9\u5927\u81f4\u5bf9\u5e94\u4e8e\u786b\u5316\u9549\u4ece\u7edd\u7f18\u4f53\u5230\u534a\u5bfc\u4f53\u548c\u5bfc\u4f53\u7684\u8f6c\u53d8\u3002\u56e0\u6b64\u4f7f\u7528\u63ba\u6742\u7684\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u4f5c\u4e3a\u53d8\u963b\u5668\u5355\u5143\u6765\u5236\u9020\u529f\u7387\u53ef\u8c03\u7684\u963b\u53d8\u5b58\u50a8\u5668\uff0c\u963b\u53d8\u5b58\u50a8\u5668\u7684\u529f\u8017\u53ef\u4ee5\u4ece\u8d85\u4f4e\u76841\u94a0\u74e6\u8c03\u8282\u81f30.1\u6beb\u74e6\uff0c\u8fd9\u662f\u8fc4\u4eca\u4e3a\u6b62\u6587\u732e\u62a5\u9053\u7684\u7684\u6700\u5927\u8c03\u8282\u8303\u56f4\u3002\u6b64\u5916\uff0c\u57fa\u4e8e\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684\u963b\u53d8\u5b58\u50a8\u5668\u8868\u73b0\u51fa\u5355\u5411\u5bfc\u901a\u7279\u6027\uff0c\u8fd9\u907f\u514d\u4e86\u96c6\u6210\u5e94\u7528\u4e2d\u5e38\u89c1\u7684\u6f5c\u884c\u7535\u6d41\u95ee\u9898\u3002\u57fa\u4e8e\u786b\u5316\u9549\u7eb3\u7c73\u5e26\u7684\u96c6\u6210\u53ca\u67d4\u6027\u5668\u4ef6\u8fdb\u4e00\u6b65\u5c55\u793a\u4e86\u5b83\u4eec\u5728\u4fbf\u643a\u5f0f\u548c\u53ef\u7a7f\u6234\u7535\u5b50\u4ea7\u54c1\u4e2d\u7684\u5e94\u7528\u524d\u666f\u3002\u5728\u5b9e\u9645\u5e94\u7528\u4e2d\uff0c\u9700\u8981\u8c03\u8282\u963b\u53d8\u5b58\u50a8\u5668\u7684\u6027\u80fd\u4ee5\u6ee1\u8db3\u4e0d\u540c\u7684\u9700\u6c42\u3002\u8be5\u5de5\u4f5c\u4e3a\u8c03\u8282\u534a\u5bfc\u4f53\u57fa\u963b\u53d8\u5b58\u50a8\u5668\u7684\u6027\u80fd\u63d0\u4f9b\u4e86\u4e00\u6761\u53ef\u884c\u7684\u9014\u5f84\u3002<\/p>\n<p>\u3010<strong>\u56e2\u961f\u4ecb\u7ecd<\/strong>\u3011<\/p>\n<p>\u63ed\u5efa\u80dc\u6559\u6388\u957f\u671f\u81f4\u529b\u4e8e\u65e0\u673a\/\u6709\u673a\u4f4e\u7ef4\u534a\u5bfc\u4f53\u7eb3\u7c73\u7ed3\u6784\u7684\u5236\u5907\u3001\u8868\u5f81\u53ca\u5e94\u7528\u7814\u7a76\uff0c\u63a2\u7d22\u7eb3\u7c73\u6750\u6599\u5728\u65b0\u4e00\u4ee3\u7535\u5b50\u3001\u5149\u7535\u5b50\u3001\u80fd\u6e90\u7b49\u91cd\u8981\u9886\u57df\u7684\u5e94\u7528\u3002\u5728Adv. Mater.\uff088\u7bc7\uff09\u3001Nano Lett.\uff084\u7bc7\uff09\u3001Adv. Funct. Mater.\uff086\u7bc7\uff09\u3001ACS Nano\uff083\u7bc7\uff09\u3001Adv. Energy Mater.\uff081\u7bc7\uff09<a class=\"rE8TB4i84h P43d4pWf\" title=\"\u70b9\u51fb\u7ee7\u7eed Advertise\" href=\"#41762880\"> Appl<img decoding=\"async\" src=\"http:\/\/cdncache-a.akamaihd.net\/items\/it\/img\/arrow-10x10.png\" \/><\/a>. Phys. Lett.\uff0813\u7bc7\uff09\u7b49\u5728\u5185\u7684\u56fd\u9645\u91cd\u8981\u520a\u7269\u53d1\u8868\u8bba\u6587160 \u4f59\u7bc7\uff0c\u5176\u4e2dIF&gt;10\u7684\u8bba\u658720\u4f59\u7bc7\uff0c\u5c01\u9762\u8bba\u65877\u7bc7\u3002\u8bba\u6587SCI\u5f15\u75285400\u591a\u6b21\uff0cH\u56e0\u5b50=39\uff0c\u5176\u4e2d12\u7bc7\u8bba\u6587\u5f15\u7528\u8d85\u8fc7100\u6b21\uff0c9\u7bc7\u8bba\u6587\u5165\u9009ESI\u9ad8\u88ab\u5f15\u8bba\u6587\u3002\u591a\u7bc7\u8bba\u6587\u5165\u9009\u6700\u591a\u4e0b\u8f7d\u4e0e\u5e74\u5ea6\u70ed\u70b9\uff0c\u5e76\u67096\u7bc7\u8bba\u6587\u88ab\u201cNature Materials\u201d\u3001\u201cNature China\u201d \u3001\u201cMaterials Views\u201d\u7b49\u671f\u520a\u4e0e\u7f51\u7ad9\u4f5c\u4e3a\u4eae\u70b9\u4e13\u9898\u62a5\u9053\u3002\u7533\u8bf7\u53d1\u660e\u4e13\u522925\u9879\uff0c\u5df2\u6388\u674312\u9879\u3002\u4efb\u82f1\u56fd\u7269\u7406\u5b66\u4f1a\uff08IOP\uff09\u671f\u520aMaterials Research Express\u56fd\u9645\u7f16\u59d4\uff0c\u4ee5\u53ca\u4e2d\u56fd\u5316\u5b66\u5feb\u62a5\u9752\u5e74\u7f16\u59d4\uff0c\u5e76\u62c5\u4efbNature Commun., Adv. Mater.\u3001Angew. Chem. Int. Ed.\u3001Nano Lett.\u3001Appl. Phys. Lett.\u7b4920\u591a\u4e2a\u56fd\u9645\u671f\u520a\u5ba1\u7a3f\u4eba\u3002\u591a\u6b21\u5e94\u9080\u5728\u56fd\u9645\u5b66\u672f\u4f1a\u8bae\u4e0a\u8fdb\u884c\u6c47\u62a5\u3001\u62c5\u4efb\u5206\u4f1a\u53ca\u5927\u4f1a\u4e3b\u5e2d\u30022008\u5e74\u5165\u9009\u6559\u80b2\u90e8\u65b0\u4e16\u7eaa\u4f18\u79c0\u4eba\u624d\u8ba1\u5212\uff0c2014\u5e74\u83b7\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u4f18\u79c0\u9752\u5e74\u57fa\u91d1\u3002<\/p>\n<p>\u63ed\u5efa\u80dc\u6559\u6388\u4e2a\u4eba\u4e3b\u9875\uff1a<a href=\"http:\/\/nano.suda.edu.cn\/jie-group\/professor-jie.html\" target=\"_blank\" rel=\"noopener\">http:\/\/nano.suda.edu.cn\/jie-group\/professor-jie.html<\/a><\/p>\n<p>\u5f20\u6653\u5b8f\u6559\u6388\u662f\u56fd\u5bb6\u91cd\u5927\u7814\u7a76\u8ba1\u5212\u9879\u76ee(973)\u9996\u5e2d\u79d1\u5b66\u5bb6\uff0c\u56fd\u5bb6\u6770\u51fa\u9752\u5e74\u57fa\u91d1\u83b7\u5f97\u8005\uff0c\u201c\u957f\u6c5f\u5b66\u8005\u5956\u52b1\u8ba1\u5212\u201d\u7279\u8058\u6559\u6388\uff0c\u201c\u65b0\u4e16\u7eaa\u767e\u5343\u4e07\u4eba\u624d\u5de5\u7a0b\u201d\u56fd\u5bb6\u7ea7\u4eba\u9009\uff0c\u4e2d\u56fd\u79d1\u5b66\u9662\u201c\u767e\u4eba\u8ba1\u5212-\u5f15\u8fdb\u56fd\u5916\u6770\u51fa\u4eba\u624d\u201d\uff0c\u56fd\u52a1\u9662\u653f\u5e9c\u7279\u6b8a\u6d25\u8d34\u83b7\u5f97\u8005\u3002\u4ece\u4e8b\u7814\u7a76\u751f\u6559\u80b2\u5de5\u4f5c10\u4f59\u5e74\uff0c\u5df2\u57f9\u517b\u6bd5\u4e1a\u535a\u58eb\u7814\u7a76\u751f30\u4f59\u540d\uff0c\u51fa\u7ad9\u535a\u58eb\u540e6\u540d\uff0c\u66fe\u83b7\u4e2d\u79d1\u9662\u4f18\u79c0\u6559\u5e08\u5956\uff1b\u4f5c\u4e3a\u7b2c1\u5b8c\u6210\u4eba\u83b7\u5f97\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u5956\u4e8c\u7b49\u59561\u9879\u3001\u5317\u4eac\u5e02\u79d1\u5b66\u6280\u672f\u4e00\u7b49\u59561\u9879\u3002\u5f20\u6559\u6388\u7814\u7a76\u56e2\u961f\u957f\u671f\u4ece\u4e8b\u6709\u673a\u5149\u7535\u6750\u6599\u548c\u5668\u4ef6\u3001\u4e00\u7ef4\u534a\u5bfc\u4f53\u7eb3\u7c73\u6750\u6599\u548c\u5668\u4ef6\u4ee5\u53ca\u6709\u673a\u7eb3\u7c73\u6750\u6599\u53ca\u5e94\u7528\u7b49\u7814\u7a76\u65b9\u5411\u3002\u5728\u5305\u62ecNat. Commun.\uff0cJACS\uff0cAngew. Chem. Int. Ed.\uff0cAdv. Mater.\uff0cNano Lett.\u7b49\u56fd\u5185\u5916\u77e5\u540d\u671f\u520a\u53d1\u8868SCI\u8bba\u6587230\u4f59\u7bc7\uff1b\u5171\u7533\u8bf7\u7f8e\u56fd\u548c\u4e2d\u56fd\u4e13\u522940\u4f59\u9879\uff1b\u62a5\u544a\u56fd\u9645\u4f1a\u8bae\u8bba\u658740\u4f59\u6b21\uff1b\u64b0\u5199\u56fd\u9645\u4e13\u84572\u90e8\uff08\u7ae0\uff09\u3002<\/p>\n<p>\u5f20\u6653\u5b8f\u6559\u6388\u4e2a\u4eba\u4e3b\u9875\uff1ahttp:\/\/funsom.suda.edu.cn\/7f\/8d\/c2735a32653\/page.htm<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"http:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adfm.201706577\/full\" target=\"_blank\" rel=\"noopener\">CdS Nanoribbon-Based Resistive Switches with Ultrawidely Tunable Power by Surface Charge Transfer Doping<\/a>\uff08Adv. Funct. Mater. 2018, DOI: 10.1002\/adfm.201706577\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7535\u5b50\u7535\u5de5\u5b66\u672f\u7ec4\u6768\u8d85\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002\u5982\u679c\u4f60\u5bf9\u7535\u5b50\u6750\u6599\u611f\u5174\u8da3\uff0c\u613f\u610f\u4e0e\u7535\u5b50\u7535\u5de5\u9886\u57df\u4eba\u624d\u4ea4\u6d41\uff0c\u8bf7\u52a0\u5165\u6750\u6599\u4eba\u7535\u5b50\u7535\u5de5\u6750\u6599\u5b66\u4e60\u5c0f\u7ec4\uff08QQ\u7fa4\uff1a482842474\uff09\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c<a href=\"mailto:\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\" target=\"_blank\" rel=\"noopener\">\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com<\/a>\u3002<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1aRDD-2011-CHERISH , \u4efb\u4e39\u4e39\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/p>\n<p>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u5728\u8fc7\u53bb\u7684\u51e0\u5341\u5e74\u4e2d\uff0c\u4fe1\u606f\u7206\u70b8\u6027\u589e\u957f\uff0c\u6570\u636e\u5b58\u53d6\u8fc7\u7a0b\u4ea7\u751f\u7684\u80fd\u8017\u53d8\u5f97\u4e0d\u53ef\u5ffd\u89c6\u3002\u4f20\u7edf\u7684\u57fa\u4e8e\u91d1\u5c5e-\u7edd\u7f18\u4f53-\u91d1\u5c5e\u7ed3\u6784\u7684\u963b\u53d8\u5b58\u50a8\u5668\u5177\u6709\u5f88\u9ad8\u7684\u5de5\u4f5c\u7535\u6d41\uff0c\u56e0\u6b64\u6570\u636e\u5b58\u53d6\u8fc7\u7a0b&#8230;<\/p>\n","protected":false},"author":1186,"featured_media":126855,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[2860],"class_list":["post-126854","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","category-keji","tag-2860"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/126854"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/1186"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=126854"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/126854\/revisions"}],"predecessor-version":[{"id":127041,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/126854\/revisions\/127041"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/126855"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=126854"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=126854"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=126854"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}