{"id":131426,"date":"2018-03-24T14:00:46","date_gmt":"2018-03-24T06:00:46","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=131426"},"modified":"2018-03-22T09:19:02","modified_gmt":"2018-03-22T01:19:02","slug":"%e5%86%af%e6%96%b0%e4%ba%aeangew-chem-int-ed-%ef%bc%9a%e5%b8%a6%e4%bd%a0%e4%ba%86%e8%a7%a3%e7%a5%9e%e7%a7%98%e7%9a%84%e9%bb%91%e9%b3%9e-%e6%96%b0%e5%9e%8b%e5%85%89%e7%94%b5","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=131426","title":{"rendered":"\u51af\u65b0\u4eaeAngew. Chem. Int. Ed.\uff1a\u5e26\u4f60\u4e86\u89e3\u795e\u79d8\u7684\u9ed1\u9cde\u2014\u2014\u65b0\u578b\u5149\u7535\u5b50\u6750\u6599"},"content":{"rendered":"<p>\u3010<strong>\u5f15\u8a00<\/strong>\u3011<\/p>\n<p>\u9ed1\u9cde(BP), \u7531\u4e8e\u5176\u524d\u6240\u672a\u6709\u7684\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\uff0c\u5355\u5c42\u7684\u76f4\u63a5\u5e26\u9699\u53ef\u4ece0.3eV\u52302.0eV\uff0c\u6210\u4e3a\u4e86\u4e8c\u7ef4\u6750\u6599\u4e2d\u4e00\u9897\u5189\u5189\u5347\u8d77\u7684\u65b0\u661f\u3002BP\u4e0e\u96f6\u95f4\u9699\u77f3\u58a8\u70ef\u548c\u534a\u5bfc\u4f53\u8fc7\u6e21\u91d1\u5c5e\u4e8c\u786b\u5c5e\u5143\u7d20\u5316\u7269\u76f8\u6bd4\uff0c\u5177\u6709\u663e\u8457\u7684\u4f18\u52bf\uff0c\u8fd9\u79cd\u4e8c\u786b\u65cf\u5143\u7d20\u5316\u7269\u4ec5\u5728\u5355\u5c42\u4e2d\u5448\u73b0\u76f8\u5bf9\u8f83\u5927\u7684\u5e26\u9699\uff081.5-2.5eV\uff09\u3002\u6b64\u5916\uff0cBP\u8fd8\u5177\u6709\u9762\u5185\u5404\u5411\u5f02\u6027\uff0c\u7535\u8377\u8f7d\u6d41\u5b50\u8fc1\u79fb\u7387\u548c\u4f18\u5f02\u7684\u5149\u5b66\/\u58f0\u5b50\u7279\u6027\u3002\u7136\u800c\uff0c\u5728\u5236\u5907\u5de5\u827a\u4e0a\uff0c\u4f7f\u7528\u900f\u660e\u80f6\u5e26\u8fdb\u884c\u673a\u68b0\u5265\u79bb\u5df2\u88ab\u5e7f\u6cdb\u7528\u4e8e\u751f\u4ea7\u5355\u4e2a\u975e\u5e38\u8584\u7684\u539f\u59cbBP\u7247\u6750\uff0c\u4f46\u5177\u6709\u6781\u4f4e\u7684\u5265\u79bb\u6536\u7387\uff0c\u9650\u5236\u4e86\u57fa\u7840\u5230\u5e94\u7528\u7684\u8fc7\u7a0b\u3002\u6700\u8fd1\uff0c\u6709\u5b66\u8005\u7814\u7a76\u4e86\u7528\u7535\u5316\u5b66\u5206\u5c42\u5265\u79bb\u7684\u65b9\u6cd5\u6765\u5236\u5907\u9ed1\u9cde\u3002<\/p>\n<p>\u3010<strong>\u6210\u679c\u7b80\u4ecb<\/strong>\u3011<\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u5fb7\u56fd\u5fb7\u96f7\u65af\u987f\u5de5\u4e1a\u5927\u5b66\u51af\u65b0\u4eae\u6559\u6388 (\u901a\u8baf\u4f5c\u8005)<\/strong>\u7b49\u4eba\u5728<strong>Angew. Chem. Int. Ed.<\/strong>\u4e0a\u53d1\u5e03\u4e86\u4e00\u7bc7\u5173\u4e8e\u4e8c\u7ef4\u6750\u6599\u9ed1\u9cde\u7684\u6587\u7ae0\uff0c\u9898\u4e3a\u201c<strong>A Delamination Strategy for Thinly Layered Defect\u2010Free High\u2010Mobility Black Phosphorus Flakes<\/strong>\u201d\u3002\u672c\u6587\u7814\u7a76\u4e86\u901a\u8fc7\u975e\u6c34\u7535\u89e3\u8d28\u4e2d\u7684\u7535\u5316\u5b66\u5de5\u7a0b\u6765\u8bc1\u660e\u975e\u6c27\u5316\u7b56\u7565\u53ef\u7528\u4e8e\u5206\u89e3\u4f53\u79efBP\u3002\u56db\u6b63\u4e01\u57fa\u94f5\u9633\u79bb\u5b50\u548c\u786b\u9178\u6c22\u6839\u9634\u79bb\u5b50\u4e4b\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\u4fc3\u8fdb\u9ad8\u8fbe78\uff05\u7684\u8131\u843d\u4ea7\u7387\u548c\u9ad8\u8fbe20.6\u03bcm\u7684\u5927BP\u8584\u7247\u3002\u5e95\u90e8\u6805\u6781\u548c\u5e95\u90e8\u63a5\u89e6\u573a\u6548\u5e94\u6676\u4f53\u7ba1(\u5305\u62ec\u4ec5\u4ec5\u51e0\u5c42\u539a\u7684\u5355\u4e2aBP\u8584\u7247)\u8868\u73b0\u51fa252\u00b118cm2 V<sup>-1<\/sup>s<sup>-1<\/sup>\u7684\u9ad8\u7a7a\u7a74\u8fc1\u79fb\u7387\u548c\u663e\u8457\u7684\u5f00\/\u5173\u6bd4\u3002\u8fd9\u79cd\u9ad8\u6548\u548c\u53ef\u6269\u5c55\u7684\u5206\u5c42\u65b9\u6cd5\u5bf9\u4e8e\u5f00\u53d1\u57fa\u4e8eBP\u7684\u590d\u5408\u6750\u6599\u548c\u5149\u7535\u5b50\u5668\u4ef6\u6709\u7740\u5f88\u5927\u7684\u5e94\u7528\u524d\u666f\u3002<\/p>\n<p>\u3010<strong>\u56fe\u7247\u5bfc\u8bfb<\/strong>\u3011<\/p>\n<p><strong>\u56fe1 \u9ed1\u9cde\u7ed3\u6784\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-131428\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/03\/1-27.png\" alt=\"\" width=\"600\" height=\"300\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/03\/1-27.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/03\/1-27-300x150.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(<strong>a,b<\/strong>) \u5206\u5c42\u8fc7\u7a0b\u548c\u53cd\u5e94\u6c60\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>(<strong>c<\/strong>) \u79bb\u5fc3\u7387\u5bf9\u5f02\u4e19\u9187\u4e2dBP\u5206\u6563\u4f53\u6d53\u5ea6\u7684\u5f71\u54cd\uff1b<\/p>\n<p>(<strong>d<\/strong>) \u5d4c\u5165\u9633\u79bb\u5b50\u4e0e\u5206\u5c42\u4ea7\u7387\u7684\u53d8\u5316\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe2 \u6837\u54c1\u5fae\u89c2\u7ed3\u6784\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-131429 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/03\/2-29-e1521681460445.png\" alt=\"\" width=\"600\" height=\"413\" \/><\/p>\n<p>(<strong>a<\/strong>) \u63d2\u5c42\u7684\u8fc7\u7a0b\u6765\u89e3\u91ca\u673a\u7406\uff1b<\/p>\n<p>(<strong>b<\/strong>) \u4e0d\u540c\u65f6\u671f\u7684\u63d2\u5c42\u540e\uff0c\u5728BP\u9634\u6781\u5904\u7684\u7ed3\u6784\u53d8\u5f62\uff1b<\/p>\n<p><strong>\u56fe3 SEM\u7167\u7247<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-131430 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/03\/3-28-e1521681477563.png\" alt=\"\" width=\"600\" height=\"364\" \/><\/p>\n<p>(<strong>a,b<\/strong>) \u7535\u5316\u5b66\u5206\u5c42\u7684BP\u8584\u7247\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>(<strong>c,d<\/strong>) \u78b3\u8f7d\u4f53\u7684\u4f4e\u5206\u8fa8\u7387TEM\u56fe\u50cf\uff1b<\/p>\n<p>(<strong>e<\/strong>) \u76f8\u5e94\u7684\u884d\u5c04\u56fe\u6848\uff1b<\/p>\n<p>(<strong>f,g<\/strong>) BP\u8584\u7247\u7684\u9ad8\u5206\u8fa8\u7387TEM\u548cAFM\u56fe\u50cf\uff1b<\/p>\n<p>(<strong>h<\/strong>) \u5c3a\u5bf8\u5206\u5e03\u7684\u76f4\u65b9\u56fe\uff1b<\/p>\n<p>(<strong>i<\/strong>) AFM\u56fe\u50cf\u7684\u9ad8\u5ea6\u5206\u5e03\u8fdb\u884c\u7edf\u8ba1\u8ba1\u7b97\u3002<\/p>\n<p><strong>\u56fe4 \u6837\u54c1\u62c9\u66fc\u5149\u8c31\u5206\u6790<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-131431 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/03\/4-29-e1521681492183.png\" alt=\"\" width=\"582\" height=\"480\" \/><\/p>\n<p>(<strong>a<\/strong>) \u7531633nm\u6fc0\u5149\u6fc0\u53d1\u7684\u5927\u5757BP\u548c\u5206\u79bb\u8584\u7247\u7684\u62c9\u66fc\u5149\u8c31\uff1b<\/p>\n<p>(<strong>b<\/strong>) \u7531\u62c9\u66fc\u5149\u8c31\u5f97\u51fa\u7684Ag1\/Ag2\u5f3a\u5ea6\u6bd4\u7684\u76f4\u65b9\u56fe\uff1b<\/p>\n<p>(c,d) BP\u819c\u7684XRD\u548cXPS\u8c31\u3002<\/p>\n<p><strong>\u56fe5 BP\u7535\u5b50\u6027\u8d28\u6d4b\u8bd5<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-131427 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/03\/5-21-e1521681506761.png\" alt=\"\" width=\"600\" height=\"657\" \/><\/p>\n<p>(<strong>a<\/strong>) \u57fa\u4e8e\u8584\u5c42BP\u7247\u7684\u573a\u6548\u5e94\u6676\u4f53\u7ba1\uff1b<\/p>\n<p>(<strong>b<\/strong>) \u6865\u63a5\u6e90\u7535\u6781\u548c\u6f0f\u7535\u6781BP\u8584\u7247\u7684BP-FET\u6c9f\u9053\u7684AFM\u56fe\u50cf\uff1b<\/p>\n<p>(<strong>c<\/strong>) \u4e0d\u540c\u6e90\u6f0f\u6781\u504f\u538b\u7684BP-FET\u7684\u4f20\u8f93\u66f2\u7ebf\uff1b<\/p>\n<p>(<strong>d<\/strong>) \u540c\u4e00\u4e2aBP-FET\u7684I-V\u7279\u6027\uff1b<\/p>\n<p>(<strong>e<\/strong>) \u4ece300\u81f3143K\u6d4b\u91cf\u7684\u6e29\u5ea6\u4f9d\u8d56\u6027\u8f6c\u79fb\u66f2\u7ebf\uff1b<\/p>\n<p>(<strong>f<\/strong>) \u753113\u4e2a\u5668\u4ef6\u83b7\u5f97\u7684\u6e29\u5ea6\u4f9d\u8d56\u6027\u7a7a\u7a74\u8fc1\u79fb\u7387\u3002<\/p>\n<p>\u3010<strong>\u5c0f\u7ed3<\/strong>\u3011<\/p>\n<p>\u672c\u6587\u7cfb\u7edf\u5730\u7814\u7a76\u4e86\u901a\u8fc7\u7535\u5316\u5b66\u7b56\u7565\u5b9e\u73b0\u5927\u5757BP\u6676\u4f53\u7684\u6709\u6548\u5206\u5c42\u3002\u5b63\u94f5\u9633\u79bb\u5b50\u5728\u65e0\u6c27\u6761\u4ef6\u4e0b\u7684\u9634\u6781\u63d2\u5c42\u963b\u788d\u4e86BP\u7247\u4e2d\u7f3a\u9677\u662f\u7684\u5f62\u6210\uff0c\u5bfc\u81f4\u9ad8\u8131\u843d\u4ea7\u7387\u548c\u5265\u79bb\u7247\u7684\u5927\u6a2a\u5411\u5c3a\u5bf8\u3002\u67d4\u6027\u6b63\u4e01\u57fa\u94fe\u7684\u53ef\u53d8\u5782\u76f4\u76f4\u5f84\u4e0eBP\u5c42\u95f4\u8ddd\u79bb\u6eb6\u5242\u5316\u8d28\u5b50\u7a7f\u900f\u548c\u51cf\u5c11\u8fdb\u4e00\u6b65\u589e\u52a0\u4e86\u4e24\u4e2a\u76f8\u90bbBP\u5c42\u4e4b\u95f4\u7684\u8ddd\u79bb\uff0c\u6eb6\u5242(\u78b3\u9178\u4e9a\u4e19\u916f)\u7a33\u5b9a\u5265\u843d\u7684\u7247\u72b6\u7269\u6709\u6548\u5730\u9632\u6b62\u5176\u518d\u805a\u96c6\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5<\/strong>\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/full\/10.1002\/anie.201801265\" target=\"_blank\" rel=\"noopener\">A Delamination Strategy for Thinly Layered Defect\u2010Free High\u2010Mobility Black Phosphorus Flakes<\/a> (Angew. Chem. Int. Ed., 15 March, 2018 , DOI: 10.1002\/anie.201801265)<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u7eb3\u7c73\u5b66\u672f\u7ec4jcfxs01\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p><strong>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1aRDD-2011-CHERISH\uff0c\u4efb\u4e39\u4e39\uff0c\u6211\u4eec\u4f1a\u9080\u8bf7\u5404\u4f4d\u8001\u5e08\u52a0\u5165\u4e13\u5bb6\u7fa4\u3002<\/strong><\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u9ed1\u9cde(BP), \u7531\u4e8e\u5176\u524d\u6240\u672a\u6709\u7684\u7535\u5b50\u80fd\u5e26\u7ed3\u6784\uff0c\u5355\u5c42\u7684\u76f4\u63a5\u5e26\u9699\u53ef\u4ece0.3eV\u52302.0eV\uff0c\u6210\u4e3a\u4e86\u4e8c\u7ef4\u6750\u6599\u4e2d\u4e00\u9897\u5189\u5189\u5347\u8d77\u7684\u65b0\u661f\u3002BP\u4e0e\u96f6\u95f4\u9699\u77f3\u58a8\u70ef\u548c\u534a\u5bfc\u4f53&#8230;<\/p>\n","protected":false},"author":4915,"featured_media":131428,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[31],"class_list":["post-131426","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-dianzi"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/131426"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/4915"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=131426"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/131426\/revisions"}],"predecessor-version":[{"id":131501,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/131426\/revisions\/131501"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/131428"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=131426"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=131426"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=131426"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}