{"id":139247,"date":"2018-05-20T14:00:14","date_gmt":"2018-05-20T06:00:14","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=139247"},"modified":"2018-05-20T20:20:27","modified_gmt":"2018-05-20T12:20:27","slug":"mater-sci-eng-a%ef%bc%9a%e9%92%a1%e6%94%b9%e6%80%a7%e5%af%b9al-7si%e5%90%88%e9%87%91%e7%bb%84%e7%bb%87%e4%b8%8e%e6%80%a7%e8%83%bd%e7%9a%84%e5%bd%b1%e5%93%8d","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=139247","title":{"rendered":"Mater. Sci. Eng., A\uff1a\u94a1\u6539\u6027\u5bf9Al-7Si\u5408\u91d1\u7ec4\u7ec7\u4e0e\u6027\u80fd\u7684\u5f71\u54cd"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<br \/>\n<\/strong><br \/>\n \u94dd\u5177\u6709\u50a8\u91cf\u5927\u3001\u6bd4\u5f3a\u5ea6\u9ad8\u3001\u826f\u597d\u7684\u8010\u78e8\u6027\u548c\u6297\u8150\u8680\u6027\u3001\u4f18\u826f\u7684\u5bfc\u7535\u6027\u4ee5\u53ca\u4ef7\u683c\u9002\u4e2d\u7b49\u7279\u70b9\uff0c\u662f\u5b9e\u73b0\u6c7d\u8f66\u548c\u822a\u7a7a\u5de5\u4e1a\u8f7b\u91cf\u5316\u7684\u5173\u952e\u6750\u6599\u3002\u5de5\u4e1a\u5316\u5e94\u7528\u7684\u94dd\u5408\u91d1\u5206\u4e3a\u94f8\u9020\u94dd\u5408\u91d1\u548c\u53d8\u5f62\u94dd\u5408\u91d1\uff0c\u800c\u94f8\u9020\u94dd\u5408\u91d1\u96f6\u4ef6\u5360\u94dd\u5408\u91d1\u768475%\u4ee5\u4e0a\u3002Al-Si\u57fa\u5408\u91d1\u4f5c\u4e3a\u6700\u4e3b\u8981\u7684\u94f8\u9020\u94dd\u5408\u91d1\uff0c\u7531\u4e8e\u5176\u4e2dSi\u5177\u6709\u4f4e\u7684\u5bc6\u5ea6\u548c\u7ebf\u81a8\u80c0\u7cfb\u6570\uff0c\u5927\u7684\u7ed3\u6676\u6f5c\u70ed\u548c\u4f4e\u7684\u6536\u7f29\u7387\uff0c\u4ece\u800c\u63d0\u9ad8\u4e86Al-Si\u94f8\u9020\u5408\u91d1\u7684\u6d41\u52a8\u6027\uff0c\u51cf\u5c0f\u6d47\u6ce8\u8fc7\u7a0b\u4e2d\u94f8\u4ef6\u7684\u7f29\u5b54\u3001\u7f29\u677e\u3001\u53d8\u5f62\u548c\u70ed\u88c2\u7b49\u7f3a\u9677\uff0c\u6539\u5584\u4e86Al-Si\u5408\u91d1\u7684\u94f8\u9020\u6027\u80fd\uff0c\u4f7f\u5176\u5360\u6240\u6709\u94f8\u9020\u94dd\u5408\u91d1\u768480\uff05\u4ee5\u4e0a\u3002\u6700\u5e38\u89c1\u7684\u94f8\u9020\u94dd\u5408\u91d1\u542b\u67095\u81f312\uff05\uff08\u8d28\u91cf\u5206\u6570\uff09\u7684\u7845\uff0c\u5e76\u4e14\u5408\u91d1\u4e2d\u542b\u6709\u786c\u8d28\u8106\u6027\u7845\u9897\u7c92\u7684\u5171\u6676\u4f53\u79ef\u5206\u6570\u901a\u5e38\u8d85\u8fc740\uff05\u3002\u5f71\u54cd\u5171\u6676Si\u6210\u6838\u548c\u751f\u957f\u7684\u5316\u5b66\u6539\u6027\u88ab\u8ba4\u4e3a\u662f\u6539\u5584\u673a\u68b0\u6027\u80fd\uff0c\u7279\u522b\u662f\u5ef6\u5c55\u6027\u7684\u6709\u6548\u65b9\u5f0f\u3002\u94a1\uff08Ba\uff09\u662f\u78b1\u571f\u91d1\u5c5e\uff0c\u636e\u62a5\u9053\u4f1a\u5f15\u8d77Al-Si\u5408\u91d1\u529b\u5b66\u6027\u80fd\u663e\u8457\u7684\u6539\u53d8\u3002\u7136\u800c\uff0c\u5173\u4e8eBa\u542b\u91cf\u5bf9Al-Si\u5408\u91d1\u7ec4\u7ec7\uff0c\u7279\u522b\u662f\u5171\u6676Si\uff0c\u91d1\u5c5e\u95f4\u5316\u5408\u7269\u548c\u5b54\u9699\u7387\u4ee5\u53ca\u529b\u5b66\u6027\u80fd\u7684\u5f71\u54cd\u7684\u8be6\u7ec6\u7814\u7a76\u662f\u6709\u9650\u7684\u3002<\/p>\n<p>\n <strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\n \u8fd1\u65e5\uff0c<strong>\u91cd\u5e86\u5927\u5b66\u90d1\u6c5f\u6559\u6388<\/strong>\u4ee5\u53ca<strong>\u897f\u5357\u4ea4\u901a\u5927\u5b66\u5c39\u51ac\u5f1f\u526f\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u56e2\u961f\u5728<strong>Mater. Sci. Eng. A<\/strong>\u53d1\u8868\u4e00\u7bc7\u9898\u4e3a\u201c<strong>Modification of eutectic Si and the microstructure in an Al-7Si alloy with barium addition<\/strong>\u201d\u7684\u6587\u7ae0\u3002\u8be5\u56e2\u961f\u63a2\u8ba8\u4e86Ba\u542b\u91cf\u5bf9\u5171\u6676Si\uff0c\u91d1\u5c5e\u95f4\u5316\u5408\u7269\u548c\u5b54\u9699\u7387\u4ee5\u53ca\u529b\u5b66\u6027\u80fd\u7b49\u5fae\u89c2\u7ed3\u6784\u7279\u5f81\u7684\u5f71\u54cd\uff0c\u5e76\u9610\u660eBa\u52a0\u5165\u5f15\u8d77\u7684\u6539\u6027\u673a\u5236\u3002\u7814\u7a76\u8868\u660e\uff0c\u5728Al-7Si\u5408\u91d1\u4e2d\u52a0\u51650.15wt. pct\uff08\u8d28\u91cf\u5206\u6570\uff09Ba\uff0c\u5c06\u5171\u6676Si\u7684\u5f62\u6001\u4ece\u7c97\u7247\u72b6\u6539\u53d8\u4e3a\u7ec6\u7ea4\u7ef4\u72b6\uff0c\u6781\u5927\u5730\u63d0\u9ad8\u4e86\u6781\u9650\u62c9\u4f38\u5f3a\u5ea6\u548c\u4f38\u957f\u7387\u3002\u7136\u800c\uff0cBa\u6dfb\u52a0\uff08\u22650.15wt. pct\uff09\u8bf1\u5bfc\u5f62\u6210\u7c97\u5927\u7684\u5757\u72b6\u542bBa\u76f8\uff08\u5373Al<sub>2<\/sub>Si<sub>2<\/sub>Ba\u76f8\uff09\u548c\u5b54\u9699\u5ea6\u589e\u91cf\uff0c\u5e76\u4e14\u7ed3\u679c\u5bf9\u5ef6\u5c55\u6027\u6709\u4e0d\u5229\u5f71\u54cd\u3002\u70ed\u5206\u6790\u8868\u660e\uff0c\u7531\u4e8eBa<sub>3<\/sub>P<sub>2<\/sub>\u76f8\u7684\u5f62\u6210\uff0cBa\u6dfb\u52a0\u6291\u5236\u4e86\u5171\u6676Si\u7684\u6210\u6838\u3002\u5728\u542bBa\u5408\u91d1\u4e2d\u89c2\u5bdf\u5230\u9ad8\u5bc6\u5ea6\u7684\u663e\u8457\u591a\u91cdSi\u5b6a\u6676\uff0c\u4e3a\u6742\u8d28\u8bf1\u5bfc\u5b6a\u6676\u751f\u957f\u673a\u5236\u63d0\u4f9b\u4e86\u5b9e\u9a8c\u652f\u6301\u3002<\/p>\n<p>\n <strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\n <strong>\u88681 \u6240\u7814\u7a76\u7684\u5408\u91d1\u7684\u5b9e\u9645\u5316\u5b66\u7ec4\u6210<\/strong><\/p>\n<table width=\"100%\">\n<tbody>\n<tr style=\"height: 24px;\">\n<td style=\"width: 136px; height: 48px; text-align: center;\" rowspan=\"2\">Composition<\/td>\n<td style=\"width: 422px; height: 24px; text-align: center;\" colspan=\"4\">\u00a0Element (Weight Percent)<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 109px; height: 24px; text-align: center;\">Si<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">Ba<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">Sr<\/td>\n<td style=\"width: 110px; height: 24px; text-align: center;\">Al<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 136px; height: 24px; text-align: center;\">Al-7Si<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">6.98<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">&#8211;<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">&#8211;<\/td>\n<td style=\"width: 110px; height: 24px; text-align: center;\">Balance<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 136px; height: 24px; text-align: center;\">Al-7Si-0.05Ba<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">6.62<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">0.047<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">&#8211;<\/td>\n<td style=\"width: 110px; height: 24px; text-align: center;\">Balance<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 136px; height: 24px; text-align: center;\">Al-7Si-0.15Ba<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">6.79<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">0.158<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">&#8211;<\/td>\n<td style=\"width: 110px; height: 24px; text-align: center;\">Balance<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 136px; height: 24px; text-align: center;\">Al-7Si-0.5Ba<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">6.70<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">0.473<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">&#8211;<\/td>\n<td style=\"width: 110px; height: 24px; text-align: center;\">Balance<\/td>\n<\/tr>\n<tr style=\"height: 24px;\">\n<td style=\"width: 136px; height: 24px; text-align: center;\">Al-7Si-0.007\u202fSr<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">6.67<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">&#8211;<\/td>\n<td style=\"width: 109px; height: 24px; text-align: center;\">0.007<\/td>\n<td style=\"width: 110px; height: 24px; text-align: center;\">Balance<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\n <strong>\u56fe1 \u6dfb\u52a0\u4e0e\u4e0d\u6dfb\u52a0Ba\u7684Al-7Si\u5408\u91d1\u7684DSC\u66f2\u7ebf\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139256\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/1-19.png\" alt=\"\" width=\"600\" height=\"445\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/1-19.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/1-19-300x223.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u7b2c\u4e00\u6b21\u653e\u70ed\u5bf9\u5e94\u4e8e\u03b1-Al\u7684\u51dd\u56fa\uff0c\u7b2c\u4e8c\u6b21\u653e\u70ed\u4e0e\u5171\u6676Si\u6cbf\u6676\u754c\u7684\u51dd\u56fa\u6709\u5173\u3002<\/p>\n<p>\n <strong>\u88682 \u5171\u6676\u6210\u6838\u6e29\u5ea6\uff08TN\uff09\u2014\u2014\u7b2c\u4e8c\u6b21\u653e\u70ed\u7684\u8d77\u59cb\u6e29\u5ea6<\/strong><\/p>\n<table width=\"100%\">\n<tbody>\n<tr>\n<td style=\"width: 120px; text-align: center;\">Alloy<\/td>\n<td style=\"width: 120px; text-align: center;\">Al-7Si<\/td>\n<td style=\"width: 161px; text-align: center;\">Al-7Si-0.05Ba<\/td>\n<td style=\"width: 161px; text-align: center;\">Al-7Si-0.15Ba<\/td>\n<td style=\"width: 161px; text-align: center;\">Al-7Si-0.5Ba<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 120px; text-align: center;\">T<sub>N<\/sub> (\u2103)<\/td>\n<td style=\"width: 120px; text-align: center;\">571.4<\/td>\n<td style=\"width: 161px; text-align: center;\">568.1<\/td>\n<td style=\"width: 161px; text-align: center;\">567.8<\/td>\n<td style=\"width: 161px; text-align: center; vertical-align: middle;\">567.5<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\n <strong>\u56fe2 Al-7Si\u5408\u91d1\u57fa\u7684\u5149\u5b66\u663e\u5fae\u955c\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139248\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/2x-1.jpeg\" alt=\"\" width=\"600\" height=\"1186\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/2x-1.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/2x-1-152x300.jpeg 152w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/2x-1-518x1024.jpeg 518w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \uff08<strong>a<\/strong>\uff09\u548c\uff08<strong>b<\/strong>\uff09\u672a\u6539\u6027\u7684\uff1b<\/p>\n<p>\n \uff08<strong>c<\/strong>\uff09\u548c\uff08<strong>d<\/strong>\uff090.05 pct Ba;<\/p>\n<p>\n \uff08<strong>e<\/strong>\uff09\u548c\uff08<strong>f<\/strong>\uff090.15 pct Ba;<\/p>\n<p>\n \uff08<strong>g<\/strong>\uff09\u548c\uff08<strong>h<\/strong>\uff090.50 pct Ba;<\/p>\n<p>\n \uff08<strong>i<\/strong>\uff09\u548c\uff08<strong>j<\/strong>\uff0970\u2009ppm\u2009Sr.<\/p>\n<p>\n <strong>\u56fe3 Al-7Si-0.15Ba and Al-7Si-0.5Ba\u5408\u91d1\u7684SEM\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139249\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/3x-1.jpeg\" alt=\"\" width=\"600\" height=\"670\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/3x-1.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/3x-1-269x300.jpeg 269w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \uff08<strong>a<\/strong>\uff09Al-7Si-0.15Ba\u7684SEM\u56fe;<\/p>\n<p>\n \uff08<strong>b<\/strong>\uff09Al-7Si-0.15Ba\u5408\u91d1\u7684\u80cc\u6563\u5c04\u7535\u5b50\uff08BSE\uff09\u56fe\u50cf;<\/p>\n<p>\n \uff08<strong>c<\/strong>\uff09Al-7Si-0.5Ba\u7684SEM\u56fe;<\/p>\n<p>\n \uff08<strong>d<\/strong>\uff09Al-7Si-0.5Ba\u5408\u91d1\u7684\u80cc\u6563\u5c04\u7535\u5b50\uff08BSE\uff09\u56fe\u50cf\u3002<\/p>\n<p>\n <strong>\u88683 \u5bf9Al-7Si-0.15Ba\u548cAl-7Si-0.5Ba\u5408\u91d1\u4e2d\u542bBa\u76f8\u7684EDS\u70b9\u6d4b\u91cf<\/strong><\/p>\n<table width=\"100%\">\n<tbody>\n<tr>\n<td style=\"width: 266px; text-align: center;\">Alloy\u00a0<\/td>\n<td style=\"width: 405px; text-align: center;\">Points<\/td>\n<td style=\"width: 190px; text-align: center;\">Al (at. pct)<\/td>\n<td style=\"width: 190px; text-align: center;\">\u00a0Si(at. pct)<\/td>\n<td style=\"width: 190px; text-align: center;\">\u00a0Ba(at. pct)<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 266px; text-align: center;\">Al-7Si-0.15Ba<\/td>\n<td style=\"width: 405px; text-align: center;\">A in Fig. 3(a) and (b)<\/td>\n<td style=\"width: 190px; text-align: center;\">\u00a064.6<\/td>\n<td style=\"width: 190px; text-align: center;\">23.82<\/td>\n<td style=\"width: 190px; text-align: center;\">11.58<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 266px; text-align: center;\">Al-7Si-0.5Ba<\/td>\n<td style=\"width: 405px; text-align: center;\">B in Fig. 3(c) and (d)<\/td>\n<td style=\"width: 190px; text-align: center;\">49.4<\/td>\n<td style=\"width: 190px; text-align: center;\">35.82<\/td>\n<td style=\"width: 190px; vertical-align: middle; text-align: center;\">14.78<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\n <strong>\u56fe4 Al-7Si-xBa\u5408\u91d1\u7684\u5b54\u9699\u7387\uff08x = 0,0.05,0.15\u548c0.5\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139250\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/4x-1.jpeg\" alt=\"\" width=\"600\" height=\"468\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/4x-1.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/4x-1-300x234.jpeg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n Ba\u542b\u91cf\u4ece0.05pct\u589e\u52a0\u52300.5pct\u65f6\uff0c\u5b54\u9699\u7387\u4ece0.04\uff05\u4e0a\u5347\u52300.40\uff05\uff0c\u679d\u6676\u95f4\u533a\u57df\u5171\u6676\u6676\u7c92\u7684\u5f62\u6838\u5bfc\u81f4\u8fdb\u6599\u6548\u7387\u7684\u964d\u4f4e\uff0c\u800c\u5171\u6676\u6676\u7c92\u963b\u585e\u8fdb\u6599\u901a\u9053\u5bfc\u81f4\u5b54\u9699\u7387\u589e\u52a0\u3002<\/p>\n<p>\n <strong>\u56fe5 Al-7Si\u5408\u91d1\u7684Si\u9897\u7c92\u7684TEM\u660e\u573a\u56fe(\u5165\u5c04\u7535\u5b50\u675f\u5e73\u884c\u4e8e&lt;011&gt; <sub>Si<\/sub>)<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139251\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/5x-1.jpeg\" alt=\"\" width=\"600\" height=\"300\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/5x-1.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/5x-1-300x150.jpeg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \uff08<strong>a<\/strong>\uff09\u672a\u6539\u6027\u7684;<\/p>\n<p>\n \uff08<strong>b<\/strong>\uff09Al-7Si-0.15Ba.<\/p>\n<p>\n <strong>\u56fe6 Al-7Si-xBa\u5408\u91d1\u7684\u62c9\u4f38\u6027\u80fd\uff08x = 0,0.05,0.15\u548c0.5\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139252\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/6-2.jpeg\" alt=\"\" width=\"600\" height=\"421\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/6-2.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/6-2-300x211.jpeg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u5f53Ba\u542b\u91cf\u8fbe\u52300.15pct\u65f6\uff0cSi\u9897\u7c92\u88ab\u5b8c\u5168\u6539\u6027\u6210\u7ea4\u7ef4\uff0c\u4ece\u800c\u6539\u5584\u5ef6\u5c55\u6027\u548cUTS\uff1b\u6dfb\u52a0\u91cf\u66f4\u591a\uff080.5pct\uff09\u65f6\uff0cAl<sub>2<\/sub>Si<sub>2<\/sub>Ba\u76f8\u7684\u5f62\u6210\u4ee5\u53ca\u5b54\u9699\u7387\u7684\u589e\u52a0\u5bfc\u81f4\u62c9\u4f38\u6027\u80fd\u4e0b\u964d\uff1bSi\u9897\u7c92\u7684\u6539\u6027\u4e0e\u5b54\u9699\u5ea6\u5bf9YS\u5f71\u54cd\u8f83\u5c0f\u3002<\/p>\n<p>\n <strong>\u56fe7 \u62c9\u4f38\u8bd5\u9a8c\u65ad\u88c2\u540e\u7684Al-7Si-xBa\u5408\u91d1\u7684\u5149\u5b66\u663e\u5fae\u56fe\uff08x = 0,0.05,0.15\u548c0.5\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139254\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/8-4.png\" alt=\"\" width=\"600\" height=\"691\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/8-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/8-4-260x300.png 260w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \uff08<strong>a<\/strong>\uff09Al-7Si;<\/p>\n<p>\n \uff08<strong>b<\/strong>\uff09Al-7Si-0.05Ba;<\/p>\n<p>\n \uff08<strong>c<\/strong>\uff09Al-7Si-0.15Ba;<\/p>\n<p>\n \uff08<strong>d<\/strong>\uff09Al-7Si-0.5Ba.<\/p>\n<p>\n <strong>\u56fe8 Al-7Si-xBa\u5408\u91d1\u65ad\u88c2\u8868\u9762\u7684SEM\u56fe\uff08x = 0,0.05,0.15\u548c0.5\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139255\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/8x-1.jpeg\" alt=\"\" width=\"600\" height=\"691\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/8x-1.jpeg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/8x-1-260x300.jpeg 260w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \uff08<strong>a<\/strong>\uff09Al-7Si;<\/p>\n<p>\n \uff08<strong>b<\/strong>\uff09Al-7Si-0.05Ba;<\/p>\n<p>\n \uff08<strong>c<\/strong>\uff09Al-7Si-0.15Ba;<\/p>\n<p>\n \uff08<strong>d<\/strong>\uff09Al-7Si-0.5Ba.<\/p>\n<p>\n <strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\n \u672c\u6587\u7814\u7a76\u4e86Al-7Si\u5408\u91d1\u4e2dBa\u542b\u91cf\u5bf9\u5171\u6676Si\uff0c\u91d1\u5c5e\u95f4\u5316\u5408\u7269\u548c\u5b54\u9699\u7387\u4ee5\u53ca\u529b\u5b66\u6027\u80fd\u7b49\u5fae\u89c2\u7ed3\u6784\u7279\u5f81\u7684\u5f71\u54cd\u3002\u6dfb\u52a00.05\uff05Ba\u65f6\uff0cAl-7Si\u5408\u91d1\u4e2d\u7684\u5171\u6676Si\u90e8\u5206\u6539\u6027\uff0c\u800c0.15\uff05Ba\u6dfb\u52a0\u91cf\u5c06\u5171\u6676Si\u9897\u7c92\u4ece\u7c97\u7247\u72b6\u6539\u53d8\u6210\u7ec6\u7ea4\u7ef4\u72b6\uff0c\u5bfc\u81f4\u5f62\u6210Al<sub>2<\/sub>Si<sub>2<\/sub>Ba\u76f8\uff0c\u4ee5\u53ca\u8f83\u9ad8\u7684\u5b54\u9699\u5ea6\u3002\u66f4\u591a\u7684Ba\u6dfb\u52a0\uff08\u53730.5pct\uff09\u4f7f\u5f97\u5171\u6676Si\u66f4\u7c97\u7cd9\uff0c\u5e76\u4e14Al<sub>2<\/sub>Si<sub>2<\/sub>Ba\u76f8\u7684\u91cf\u548c\u5c3a\u5bf8\u90fd\u589e\u52a0\u3002Ba\u7684\u52a0\u5165\u5bfc\u81f4\u5f62\u6210\u70ed\u529b\u5b66\u7a33\u5b9a\u7684Ba<sub>3<\/sub>P<sub>2<\/sub>\u76f8\uff0c\u5e76\u4f7fAlP\u9897\u7c92\u5931\u6d3b\uff0c\u6210\u6838\u4f4d\u7f6e\uff08\u5373AlP\uff09\u7684\u91cf\u51cf\u5c11\uff0c\u56e0\u6b64\u5171\u6676\u6210\u6838\u6e29\u5ea6\uff08TN\uff09\u964d\u4f4e\u3002\u968f\u7740Ba\u542b\u91cf\u4e0a\u5347\u52300.15pct\uff0cSi\u6676\u7c92\u7684\u6539\u6027\u964d\u4f4e\u4e86\u5e94\u529b\u96c6\u4e2d\uff0c\u662f\u63d0\u9ad8UTS\u548c\u5ef6\u6027\u7684\u4e3b\u8981\u673a\u5236\uff0c\u800cYS\u6ca1\u6709\u660e\u663e\u53d8\u5316\u3002\u5728\u542b\u6709\u8f83\u591aBa\uff080.5pct\uff09\u7684\u5408\u91d1\u4e2d\uff0c\u7c97\u5927\u7684Al<sub>2<\/sub>Si<sub>2<\/sub>Ba\u76f8\u7684\u5f62\u6210\u548c\u5b54\u9699\u7387\u7684\u589e\u52a0\u6210\u4e3a\u5f15\u8d77\u7684\u5e94\u529b\u96c6\u4e2d\u7684\u4e3b\u8981\u673a\u5236\uff0c\u5bf9UTS\u548c\u5851\u6027\u6709\u4e0d\u5229\u5f71\u54cd\u3002\u7c97\u5927\u7684Al<sub>2<\/sub>Si<sub>2<\/sub>Ba\u76f8\u7684\u5f62\u6210\u7531\u4e8eSi\u7684\u6d88\u8017\uff0c\u964d\u4f4e\u4e86\u56fa\u6eb6\u5f3a\u5316\u6548\u5e94\uff0c\u5171\u6676Si\u9897\u7c92\u5f3a\u5316\u6548\u5e94\u4e5f\u964d\u4f4e\u4e86YS\u30020.15\uff05Ba\u6dfb\u52a0\u4fc3\u8fdb\u4e86\u9ad8\u5bc6\u5ea6\u591a\u91cdSi\u5b6a\u6676\u7684\u751f\u957f\uff0c\u4e3a\u6742\u8d28\u8bf1\u5bfc\u5b6a\u6676\u673a\u5236\uff08IIT\uff09IIT\u63d0\u4f9b\u4e86\u5b9e\u9a8c\u652f\u6301\u3002<\/p>\n<p>\n <strong>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/www.sciencedirect.com\/science\/article\/pii\/S0921509318306592\" target=\"_blank\" rel=\"noopener\">Modification of eutectic Si and the microstructure in an Al-7Si alloy with barium addition<\/a><\/strong>\uff08Mater. Sci. Eng. A, 2018, DOI: 10.1016\/j.msea.2018.05.010\uff09<\/p>\n<p>\u00a0<br \/>\n \u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u65b0\u4eba\u7ec4\u674e\u5cf0\u7f16\u8f91\uff0c\u9648\u70b3\u65ed\u5ba1\u6838\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/a>\u3002<\/p>\n<p>\n <strong>\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\">\u6d4b\u8bd5\u8c37<\/a>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u94dd\u5177\u6709\u50a8\u91cf\u5927\u3001\u6bd4\u5f3a\u5ea6\u9ad8\u3001\u826f\u597d\u7684\u8010\u78e8\u6027\u548c\u6297\u8150\u8680\u6027\u3001\u4f18\u826f\u7684\u5bfc\u7535\u6027\u4ee5\u53ca\u4ef7\u683c\u9002\u4e2d\u7b49\u7279\u70b9\uff0c\u662f\u5b9e\u73b0\u6c7d\u8f66\u548c\u822a\u7a7a\u5de5\u4e1a\u8f7b\u91cf\u5316\u7684\u5173\u952e\u6750\u6599\u3002\u5de5\u4e1a\u5316\u5e94\u7528\u7684\u94dd\u5408\u91d1\u5206\u4e3a\u94f8\u9020\u94dd\u5408\u91d1&#8230;<\/p>\n","protected":false},"author":230,"featured_media":139251,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[346],"class_list":["post-139247","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-metal"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/139247"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/230"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=139247"}],"version-history":[{"count":8,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/139247\/revisions"}],"predecessor-version":[{"id":139564,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/139247\/revisions\/139564"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/139251"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=139247"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=139247"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=139247"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}