{"id":139531,"date":"2018-05-22T14:00:54","date_gmt":"2018-05-22T06:00:54","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=139531"},"modified":"2018-05-20T21:43:39","modified_gmt":"2018-05-20T13:43:39","slug":"acta-mater-%ef%bc%9a%e5%80%9f%e5%8a%a9stem%e7%9a%84%e4%bd%8d%e7%9b%b8%e8%a1%ac%e5%ba%a6%e8%af%86%e5%88%ab%e5%b9%b3%e8%a1%a1%e6%80%81ni-ysz%e7%95%8c%e9%9d%a2%e5%8e%9f%e5%ad%90%e7%bb%93%e6%9e%84","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=139531","title":{"rendered":"Acta Mater.\uff1a\u501f\u52a9STEM\u7684\u4f4d\u76f8\u886c\u5ea6\u8bc6\u522b\u5e73\u8861\u6001Ni-YSZ\u754c\u9762\u539f\u5b50\u7ed3\u6784"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u56fa\u6001\u6c27\u5316\u7269\u71c3\u6599\u7535\u6c60\u5728\u9ad8\u6548\u80fd\u6e90\u5b58\u50a8\u548c\u7535\u529b\u4f9b\u5e94\u7684\u524d\u666f\u5e7f\u9614\u3002\u5728\u4f17\u591a\u56fa\u6001\u6c27\u5316\u7269\u71c3\u6599\u7535\u6c60\u4f53\u7cfb\u4e2d\uff0cNi\u548c\u9487\u7a33\u5b9a\u6c27\u5316\u7269\uff08YSZ\uff09\u4e4b\u95f4\u7684\u754c\u9762\u662f\u5173\u952e\u90e8\u5206\uff0c\u6b64\u5904Ni\u4f5c\u4e3a\u9633\u6781\u6750\u6599\u3002\u56e0\u6b64\uff0c\u754c\u9762\u7a33\u5b9a\u6027\u81f3\u5173\u91cd\u8981\u3002\u5728\u7535\u6c60\u5de5\u4f5c\u671f\u95f4\uff0cNi-YSZ\u754c\u9762\u66b4\u9732\u5728\u9ad8\u6e29\u4e0b\u5f15\u8d77Ni\u9897\u7c92\u7684\u7c97\u5316\uff0c\u603b\u7684\u754c\u9762\u80fd\u51cf\u5c11\uff0c\u9a71\u52a8\u754c\u9762\u603b\u9762\u79ef\u7684\u51cf\u5c11\uff0c\u4ece\u800c\u5bfc\u81f4\u7535\u6c60\u5de5\u4f5c\u6548\u7387\u7684\u52a3\u5316\u3002\u63d0\u9ad8\u7535\u6781\u4e2d\u754c\u9762\u7a33\u5b9a\u6027\u548c\u6301\u4e45\u6027\u662f\u56fa\u6001\u6c27\u5316\u7269\u71c3\u6599\u7535\u6c60\u9886\u57df\u7684\u4e00\u4e2a\u5173\u952e\u6311\u6218\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u4ee5\u8272\u5217\u7406\u5de5\u5b66\u9662<\/strong>\u7684<strong>Wayne D. Kaplan\u6559\u6388<\/strong>\uff08\u901a\u8baf\u4f5c\u8005\uff09\u5728<strong>Acta Materialia<\/strong>\u4e0a\u53d1\u8868\u4e86\u9898\u4e3a\u201c<strong>Discerning Interface Atomistic Structure by Phase Contrast in STEM:The Equilibrated Ni-YSZ Interface<\/strong>\u201d\u7684\u6587\u7ae0\u3002Ni\u548c\u9487\u7a33\u5b9a\u6c27\u5316\u9506\uff08YSZ\uff09\u7684\u5e73\u8861\u754c\u9762\u662f1350\u2103\uff0c\u6c27\u504f\u538b\u4e3a10-20atm\u6761\u4ef6\u4e0b\uff0cNi\u8584\u819c\u5728YSZ\u5355\u6676\u7684(111)\u8868\u9762\u901a\u8fc7\u56fa\u6001\u6da6\u6e7f\u5f62\u6210\u7684\u3002\u5e73\u8861\u56fa-\u56fa\u754c\u9762\u7684\u539f\u5b50\u7ed3\u6784\u501f\u52a9\u5355\u8272\u6d88\u50cf\u5dee\u77eb\u6b63\u7684\u626b\u63cf\u900f\u5c04\u7535\u5b50\u663e\u5fae\u955c\uff08STEM\uff09\u4f7f\u7528\u4e0d\u540c\u6280\u672f\u6765\u786e\u5b9a\u3002\u7ed3\u679c\u663e\u793a\u7531\u4e8eNi\u548cYSZ\u91cd\u6784\u754c\u9762\u4e4b\u95f4\u53d1\u751f\u4e86\u5927\u7684\u6676\u683c\u9519\u914d\uff0c\u5f62\u6210\u4e86\u4e00\u79cd\u5305\u542b\u9ad8\u5bc6\u5ea6\u5931\u914d\u4f4d\u9519\u7684\u7279\u6b8a\u7ed3\u6784\u3002\u7136\u800c\uff0c\u5c3d\u7ba1\u6709\u5927\u7684\u6676\u683c\u9519\u914d\uff0c\u754c\u9762\u4e5f\u4e0d\u662f\u975e\u5171\u683c\u7684\u3002\u754c\u9762\u7531\u9633\u79bb\u5b50\u7ec8\u6b62\uff0c\u8fd9\u53ef\u80fd\u662f\u7531\u4e8e\u4f4e\u6c27\u504f\u538b\u4e0b\u8fbe\u5230\u5e73\u8861\u5bfc\u81f4\u7684\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe1\uff1a\u901a\u8fc7\u56fa\u6001\u6da6\u6e7f\u65b9\u6cd5\u5236\u5907\uff0c\u5e73\u8861\u6001Ni\u9897\u7c92\u5728YSZ\u57fa\u5e95\u4e0a\u7684\u4e8c\u6b21\u7535\u5b50HRSEM\u56fe\u50cf\u3002<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139533\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/1-20.png\" alt=\"\" width=\"600\" height=\"597\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/1-20.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/1-20-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/1-20-300x300.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u9897\u7c92\u7684(111)\u9762\u4e0eYSZ\u57fa\u5e95\u8868\u9762\u7684(111)\u9762\u5e73\u884c\u3002\u70b9\u5212\u7ebf\u77e9\u5f62\u4e3aFIB\u9009\u62e9\u7684\u533a\u57df\uff0c\u7528\u4e8eTEM\u5206\u6790\u3002<\/p>\n<p><strong>\u56fe2\uff1a\u540c\u65f6\u83b7\u5f97\u7684\u5e73\u8861\u6001Ni\u9897\u7c92\u6cbfNi[-110]\u8f74\u5411\u7684\u754c\u9762\u533a\u57dfSTEM\u56fe\u50cf\u3002<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139534\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/2-18.png\" alt=\"\" width=\"600\" height=\"294\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/2-18.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/2-18-300x147.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a)\u9ad8\u89d2\u5ea6\u73af\u5f62\u6697\u573aSTEM\u56fe\u50cf\uff1b<\/p>\n<p>(b)\u73af\u5f62\u660e\u573aSTEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe3\uff1a\u754c\u9762\u533a\u57df\u7684iDPC-STEM\u8868\u5f81\u3002<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139535\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/3-20.png\" alt=\"\" width=\"600\" height=\"1846\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/3-20.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/3-20-333x1024.png 333w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a)\u5e73\u8861\u6001Ni\u9897\u7c92\u6cbfNi[-110]\u8f74\u5411\u7684\u754c\u9762\u533a\u57df\u7684iDPC-STEM\u56fe\u50cf\uff0c\u754c\u9762\u5904Ni\u539f\u5b50\u548cZr\u539f\u5b50\u4e4b\u95f4\u7684\u7535\u8377\u8f6c\u79fb\u660e\u663e\u53ef\u89c1;<\/p>\n<p>(b)\u5c06(a)\u56fe\u4f7f\u7528\u9ad8\u901a\u6ee4\u6ce2\u5668\u8fdb\u884c\u8fc7\u6ee4\u540e\u7684\u56fe\u50cf\uff0c\u539f\u5b50\u67f1\u4f4d\u7f6e\u53ef\u5728\u754c\u9762\u4e24\u4fa7\u90fd\u770b\u5230\uff1b<\/p>\n<p>(c)\u767d\u8272\u65b9\u6846\u5212\u5b9a\u7684\u6cbf\u754c\u9762\u4ea4\u66ff\u6392\u5e03\u7684\u91cd\u590d\u5355\u5143\u5b9a\u4e49\u4e3aA\u548cB\uff0c\u4e00\u4e2a\u5269\u4f59\u8fde\u7eed\u5e73\u9762\uff08B\u5355\u5143\uff09\u5728\u4e00\u5217\u7ed3\u6784\u5355\u5143\u4e4b\u95f4\u5206\u79bb\u3002<\/p>\n<p><strong>\u56fe4\uff1a\u754c\u9762\u533a\u57df\u7684EDS\u5206\u5e03\u56fe\u3002<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-139536\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/4-17.png\" alt=\"\" width=\"600\" height=\"473\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/4-17.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/05\/4-17-300x237.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(A)\u754c\u9762\u7684\u73af\u5f62\u6697\u573aSTEM\u56fe\u50cf\uff1b<\/p>\n<p>(B-F)\u540c\u4e00\u533a\u57df\u7684EDS\u80fd\u8c31\u5206\u5e03\u56fe\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u5de5\u4f5c\u501f\u52a9IDPC STEM\u548cEDS\u80fd\u8c31\u5206\u5e03\u56fe\u786e\u5b9a\u5e73\u8861Ni[-110]||YSZ[1-10](111)\u754c\u9762\u7684\u5c40\u57df\u539f\u5b50\u7ed3\u6784\u3002\u5b9e\u9a8c\u56fe\u50cf\u663e\u793a\u754c\u9762\u91c7\u7528\u4e00\u79cd\u542b\u6709\u9ad8\u5bc6\u5ea6\u5931\u914d\u4f4d\u9519\u7684\u7279\u6b8a\u7ed3\u6784\uff0c\u8fd9\u662f\u7531\u4e8e\u4e24\u76f8\u5177\u6709\u7279\u6b8a\u7684\u53d6\u5411\u5173\u7cfb\uff0c\u4ea7\u751f\u5927\u7684\u6676\u683c\u5931\u914d\u5bfc\u81f4\u7684\u3002\u7136\u800c\uff0c\u5c3d\u7ba1\u5177\u6709\u8f83\u5927\u7684\u6676\u683c\u5931\u914d\uff0c\u754c\u9762\u4ecd\u4e0d\u662f\u975e\u5171\u683c\u7684\u3002\u89c2\u5bdf\u5230\u7684\u4f4d\u9519\u5e8f\u5217\u5b9a\u4e49\u4e86\u754c\u9762\u7684\u91cd\u6784\u7ed3\u6784\uff0c\u901a\u8fc7\u5438\u6536\u9519\u914d\u5e94\u53d8\u80fd\u4f7f\u5f97\u754c\u9762\u80fd\u6700\u5c0f\u5316\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"https:\/\/www.sciencedirect.com\/science\/article\/pii\/S135964541830363X\" target=\"_blank\" rel=\"noopener\">Discerning Interface Atomistic Structure by Phase Contrast in STEM: The Equilibrated Ni-YSZ Interface<\/a>\uff08Acta Mater.\uff0c2018\uff0cDOI\uff1a10.1016\/j.actamat.2018.05.011\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u91d1\u5c5e\u6750\u6599\u7ec4Isobel\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\">\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8\u5927\u5bb6\u5ead<\/a>\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaokefu<\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u4e0a<\/strong><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\"><strong>\u6d4b\u8bd5\u8c37<\/strong><\/a><strong>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u56fa\u6001\u6c27\u5316\u7269\u71c3\u6599\u7535\u6c60\u5728\u9ad8\u6548\u80fd\u6e90\u5b58\u50a8\u548c\u7535\u529b\u4f9b\u5e94\u7684\u524d\u666f\u5e7f\u9614\u3002\u5728\u4f17\u591a\u56fa\u6001\u6c27\u5316\u7269\u71c3\u6599\u7535\u6c60\u4f53\u7cfb\u4e2d\uff0cNi\u548c\u9487\u7a33\u5b9a\u6c27\u5316\u7269\uff08YSZ\uff09\u4e4b\u95f4\u7684\u754c\u9762\u662f\u5173\u952e\u90e8\u5206\uff0c\u6b64\u5904Ni\u4f5c\u4e3a\u9633&#8230;<\/p>\n","protected":false},"author":4765,"featured_media":139536,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[3225,27,3224],"class_list":["post-139531","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","category-keji","tag-3225","tag-cell","tag-3224"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/139531"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/4765"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=139531"}],"version-history":[{"count":5,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/139531\/revisions"}],"predecessor-version":[{"id":139587,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/139531\/revisions\/139587"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/139536"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=139531"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=139531"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=139531"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}