{"id":14095,"date":"2016-05-17T19:50:46","date_gmt":"2016-05-17T11:50:46","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=14095"},"modified":"2016-05-17T20:09:28","modified_gmt":"2016-05-17T12:09:28","slug":"%e5%ad%a6%e6%9c%af%e5%b9%b2%e8%b4%a7%e4%b8%a8%e6%89%8b%e6%8a%8a%e6%89%8b%e6%95%99%e4%bd%a0%e9%94%82%e7%a6%bb%e5%ad%90%e7%94%b5%e6%b1%a0%e6%b5%86%e6%96%99%e5%88%b6%e5%a4%87%e5%92%8c%e6%89%a3%e5%bc%8f","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=14095","title":{"rendered":"\u5b66\u672f\u5e72\u8d27\u4e28\u624b\u628a\u624b\u6559\u4f60\u9502\u79bb\u5b50\u7535\u6c60\u6d46\u6599\u5236\u5907\u548c\u6263\u5f0f\u7535\u6c60\u7ec4\u88c5"},"content":{"rendered":"<p>\u672c\u6587\u4e3b\u8981\u5bf9\u5b9e\u9a8c\u5ba4\u7ec4\u88c5\u6263\u5f0f\u7535\u6c60\u7684\u6d41\u7a0b\u8fdb\u884c\u4ecb\u7ecd\uff0c\u4e3b\u8981\u53c2\u8003\u5317\u5de5\u4e1a\u738b\u7426\u5e08\u5144\u7684\u300a\u9502\u79bb\u5b50\u6a21\u62df\u7535\u6c60\u7ec4\u88c5\u624b\u518c\u300b\u3001\u90d1\u5dde\u8f7b\u5de5\u5b66\u9662\u5f20\u52c7\u7b49\u4eba\u7684\u300a\u6263\u5f0f\u9502\u79bb\u5b50\u7535\u6c60\u7684\u5236\u5907\u5de5\u827a\u7814\u7a76\u300b\u4ee5\u53ca\u4e00\u4e9b\u7f51\u53cb\u610f\u89c1\u548c\u4e00\u4e9b\u6e05\u534e\u7814\u53cb\u7684\u5de5\u4f5c\u7ecf\u9a8c\u3002<\/p>\n<p>\u9996\u5148\u8bf4\u660e\u4e00\u4e0b\uff0c\u5b9e\u9a8c\u5ba4\u6240\u8bf4\u7684\u6263\u5f0f\u7535\u6c60\u4e00\u822c\u90fd\u662f\u6307\u534a\u7535\u6c60\uff0c\u5373\u4ee5\u9502\u7247\u4e3a\u201c\u8d1f\u6781\u201d\uff0c\u6211\u4eec\u81ea\u5df1\u505a\u7684\u6781\u7247\u4e3a\u201c\u6b63\u6781\u201d\u3002\u6240\u4ee5\uff0c\u65e0\u8bba\u662f\u6b63\u6781\u8fd8\u662f\u8d1f\u6781\u6750\u6599\uff0c\u7ec4\u88c5\u6263\u5f0f\u7535\u6c60\u7684\u6d41\u7a0b\u90fd\u662f\u4e00\u6837\u7684<\/p>\n<ol>\n<li><strong>\u6263\u5f0f\u7535\u6c60\u57fa\u672c\u4ecb\u7ecd<\/strong><\/li>\n<\/ol>\n<p>\u9502\u79bb\u5b50\u6263\u5f0f\u7535\u6c60\u4e3b\u8981\u7531\u4ee5\u4e0b\u51e0\u90e8\u5206\u7ec4\u6210\uff1a\u6b63\u6781\u58f3\u3001\u8d1f\u6781\u58f3\u3001\uff08\u6b63\/\u8d1f\uff09\u6781\u7247\u3001\u9694\u819c\u3001\u57ab\u7247\u3001\u5f39\u7247\u3001\u7535\u89e3\u6db2\u3002<\/p>\n<p>\u5e38\u7528\u7684\u6263\u5f0f\u7535\u6c60\u7684\u7535\u6c60\u58f3\u4e3aCR2032\u3001CR2025\u3001CR2016\u7b49\uff0cC\u4ee3\u8868\u6263\u7535\u4f53\u7cfb\uff0cR\u4ee3\u8868\u7535\u6c60\u5916\u5f62\u4e3a\u5706\u5f62\u3002\u524d\u4e24\u4f4d\u6570\u5b57\u4e3a\u76f4\u5f84\uff08\u5355\u4f4d mm\uff09\uff0c\u540e\u4e24\u4f4d\u6570\u5b57\u4e3a\u539a\u5ea6\uff08\u5355\u4f4d 0.1 mm\uff09\uff0c\u53d6\u4e24\u8005\u7684\u63a5\u8fd1\u6570\u5b57\u3002\u4f8b\u5982 CR2032 \u7684\u5927\u7565\u5c3a\u5bf8\u4e3a\u76f4\u5f84 20 mm\uff0c\u539a\u5ea6 3.2 mm\u3002<\/p>\n<p><strong>1.1 \u00a0\u7535\u6c60\u58f3<\/strong><\/p>\n<p>\u4e0b\u56fe\u4e3aCR2032\u6263\u5f0f\u7535\u6c60\u7535\u6c60\u58f3\uff0c\u6b63\u6781\u58f3\u8f83\u5927\uff0c\u8d1f\u6781\u58f3\u4e3a\u8868\u9762\u6709\u7f51\u72b6\u7ed3\u6784\u4e14\u8f83\u5c0f\uff0c\u6240\u4ee5\u4e00\u822c\u7ec4\u88c5\u8fc7\u7a0b\u4ece\u8d1f\u6781\u58f3\u5f00\u59cb\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/\u6263\u75351.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-14100 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/\u6263\u75351.jpg\" alt=\"\u6263\u75351\" width=\"425\" height=\"220\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/\u6263\u75351.jpg 425w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/\u6263\u75351-300x155.jpg 300w\" sizes=\"(max-width: 425px) 100vw, 425px\" \/><\/a><\/p>\n<p style=\"text-align: center;\">\u56fe1\u00a0 CR2032\u6263\u5f0f\u7535\u6c60\u6b63\u6781\u58f3\uff08\u5de6\uff09\uff0c\u8d1f\u6781\u58f3\uff08\u53f3\uff09<\/p>\n<p style=\"text-align: left;\"><strong>1.2 \u00a0\u6781\u7247<\/strong><\/p>\n<p>\u6781\u7247\u7684\u5236\u5907\u5de5\u827a\u5bf9\u7535\u5316\u5b66\u6027\u80fd\u80fd\u5426\u5145\u5206\u53d1\u6325\u6709\u91cd\u8981\u5f71\u54cd\uff0c\u6211\u4eec\u4f1a\u57282.1\u4e2d\u91cd\u70b9\u8bb2\u89e3\uff0c\u6b64\u5904\u7b80\u8981\u4ecb\u7ecd\u3002\u4e0b\u56fe\u4e3a\u6b63\u6781\u6750\u6599\u6240\u5236\u5907\u7684\u6781\u7247\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/2-11.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-14096\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/2-11.png\" alt=\"2\" width=\"460\" height=\"209\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/2-11.png 460w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/2-11-300x136.png 300w\" sizes=\"(max-width: 460px) 100vw, 460px\" \/><\/a><\/p>\n<p style=\"text-align: center;\">\u56fe2\u00a0 \u6b63\u6781\u7247\uff08\u5de6\uff09\u4e0e\u94dd\u7b94\uff08\u53f3\uff09<\/p>\n<p>\u6b63\u8d1f\u6781\u6781\u7247\u7684\u5236\u5907\u6d41\u7a0b\u76f8\u540c\uff0c\u533a\u522b\u5728\u4e8e<strong>\u6b63\u6781\u6d82\u5e03\u5728\u94dd\u7b94\u4e0a\uff0c\u8d1f\u6781\u6d82\u5e03\u5728\u5728\u94dc\u7b94\u4e0a\uff0c\u8fd9\u662f\u4e3a\u4f55\u5462\uff1f<\/strong><\/p>\n<p>\u9996\u5148\uff0c\u4e24\u8005\u7684\u5bfc\u7535\u6027\u90fd\u76f8\u5bf9\u8f83\u597d\uff0c\u8d28\u5730\u6bd4\u8f83\u67d4\u8f6f\uff0c\u4ef7\u683c\u4e5f\u76f8\u5bf9\u8f83\u4f4e\u3002<\/p>\n<p>\u5176\u6b21\uff0c\u94dd\u672c\u8eab\u6bd4\u8f83\u6d3b\u6cfc\uff0c\u5728\u4f4e\u7535\u4f4d\u4e0b\uff0c\u94dd\u4f1a\u51fa\u73b0\u5d4c\u9502\uff0c\u751f\u6210\u9502\u94dd\u5408\u91d1\uff0c\u4e0d\u5b9c\u4f5c\u4e3a\u8d1f\u6781\u7684\u96c6\u6d41\u4f53\u3002\u5982\u679c\u4f7f\u7528\u94dd\u7b94\u4f5c\u4e3a\u8d1f\u6781\u7684\u96c6\u6d41\u4f53\uff0c\u94dd\u4f1a\u548c\u9502\u5f62\u6210\u5408\u91d1\uff0c\u7136\u540e\u7c89\u5316\uff0c\u4e25\u91cd\u5f71\u54cd\u7535\u6c60\u7684\u5bff\u547d\u548c\u6027\u80fd\u3002<\/p>\n<p>\u6700\u540e\uff0c\u94dc\u5728\u9ad8\u7535\u4f4d\u4e0b\u5bb9\u6613\u6c27\u5316\uff0c\u4e0d\u5b9c\u4f5c\u4e3a\u6b63\u6781\u7684\u96c6\u6d41\u4f53\uff0c\u94dc\u8868\u9762\u7684\u6c27\u5316\u5c42\u5c5e\u4e8e\u534a\u5bfc\u4f53\uff0c\u7535\u5b50\u5bfc\u901a\uff0c\u6c27\u5316\u5c42\u592a\u539a\u65f6\uff0c\u963b\u6297\u4f1a\u589e\u52a0\u3002\u540c\u65f6\u9502\u4e0d\u4f1a\u4e0e\u540c\u5728\u5730\u70b9\u4e3a\u4e0b\u5f62\u6210\u5d4c\u9502\u5408\u91d1\u3002<\/p>\n<p><strong>\u4ec0\u4e48\u6837\u7684\u6781\u7247\u624d\u662f\u597d\u6781\u7247\uff1f<\/strong><\/p>\n<p>\u5e94\u8be5\u6ee1\u8db3\u8fd9\u51e0\u65b9\u9762\uff1a\uff081\uff09\u6d46\u6599\u6d82\u5e03\u5747\u5300\uff0c\u89c2\u5bdf\u4e0d\u5230\u660e\u663e\u7684\u539a\u5ea6\u4e0d\u5747\u5300\uff0c\u7279\u522b\u8584\u7684\u5730\u65b9\u751a\u81f3\u80fd\u89c2\u5bdf\u5230\u4eae\u8272\u7684\u94dd\u7b94\uff1b\uff082\uff09\u6781\u7247\u4fdd\u6301\u5b8c\u6574\u5706\u5f62\u672a\u53d7\u635f\u574f\uff0c\u5468\u56f4\u5c3d\u91cf\u6ca1\u6709\u6bdb\u523a\uff1b\uff083\uff09\u6781\u7247\u6d82\u5e03\u533a\u57df\u6ca1\u6709\u9897\u7c92\u7269\u5e76\u4e14\u6ca1\u6709\u660e\u663e\u7684\u6389\u7c89\u73b0\u8c61\u3002<\/p>\n<p><strong>1.3 \u00a0\u9694\u819c<\/strong><\/p>\n<p>\u5b9e\u9a8c\u5ba4\u6240\u7528\u9694\u819c\u4e00\u822c\u4e3aCelgard2400\u6216\u8005Celgard\u7cfb\u5217\u5176\u4ed6\u4ea7\u54c1\uff0c\u51b2\u538b\u6210\u5c0f\u5706\u7247\u540e\u4f7f\u7528\uff0c\u76f4\u5f84\u7565\u5927\u4e8e\u6b63\u8d1f\u6781\u6781\u7247\u3002\u53ef\u4ee5\u6839\u636e\u7535\u6c60\u6027\u80fd\u8981\u6c42\u4e0d\u540c\u9009\u62e9\u9694\u819c\uff0c\u5173\u4e8e\u9694\u819c\u7684\u9009\u62e9\u548c\u53c2\u6570\uff0c\u8bf7\u89c1\u540e\u671f\u5173\u4e8e\u9502\u7535\u6c60\u9694\u819c\u7684\u9009\u62e9\u4ee5\u53ca\u53c2\u6570\u610f\u4e49\u7684\u4ecb\u7ecd\u3002<\/p>\n<p><strong>\u9694\u819c\u7684\u4f5c\u7528\u662f\u4ec0\u4e48\u5462\uff1f<\/strong><\/p>\n<p>\u7b80\u5355\u7684\u8bf4\uff0c\u5982\u679c\u6ca1\u6709\u9694\u819c\uff0c\u6b63\u8d1f\u6781\u5c31\u76f4\u63a5\u63a5\u89e6\uff0c\u4e5f\u5c31\u662f\u4f1a\u53d1\u751f\u77ed\u8def\uff0c\u8fd9\u4e5f\u5c31\u662f\u4e3a\u4ec0\u4e48\u6709\u7684\u7535\u6c60\u4e2d\u8981\u6291\u5236\u9502\u679d\u6676\u7684\u4ea7\u751f\uff0c\u5c31\u662f\u9632\u6b62\u5176\u523a\u7834\u9694\u819c\uff0c\u5f15\u8d77\u5c40\u90e8\u77ed\u8def\uff0c\u800c\u9020\u6210\u5b89\u5168\u4e8b\u6545\u3002\u9694\u819c\u4e00\u822c\u91c7\u7528\u805a\u4e59\u70ef\u7b49\u9ad8\u5206\u5b50\u6750\u6599\uff0c\u4e0d\u5bfc\u7535\uff0c\u5176\u7ed3\u6784\u4e2d\u6709\u8bb8\u591a\u5fae\u5b54\uff0c\u5141\u8bb8\u9502\u79bb\u5b50\u901a\u8fc7,\u867d\u7136\u5b83\u662f\u7edd\u7f18\u4f53\uff0c\u4f46\u201c\u4e0d\u5141\u8bb8\u7535\u5b50\u901a\u8fc7\u7684\u8bf4\u6cd5\u5e76\u4e0d\u51c6\u786e\u201d\u3002<\/p>\n<p><strong>1.4 \u00a0\u9502\u7247\uff08\u5373\u8d1f\u6781\u7247\uff09<\/strong><\/p>\n<p>\u8d1f\u6781\u7247\u76f4\u5f84\u7565\u5c0f\u4e8e\u8d1f\u6781\u58f3\u76f4\u5f84\uff0cCR2032\u7684\u9502\u7247\u76f4\u5f84\u4e3a15.8mm\uff0c\u5bf9\u5e94\u7684\u6b63\u6781\u7247\u4e5f\u662f15.8mm\u3002<strong>\u503c\u5f97\u6ce8\u610f\u7684\u662f\uff1a<\/strong>\u9502\u7247\u6bd4\u8f83\u67d4\u8f6f\uff0c\u5bb9\u6613\u53d8\u5f62\uff0c\u6240\u4ee5\u5728\u88c5\u7535\u6c60\u524d\u53ef\u4ee5\u7528\u6b63\u6781\u58f3\uff08\u56e0\u4e3a\u5b83\u6bd4\u8f83\u5927\uff09\u5c06\u53d8\u5f62\u7684\u9502\u7247\u538b\u5e73\u6574\u3002\u800c\u4e14\u91d1\u5c5e\u9502\u5728\u7a7a\u6c14\u4e2d\u6781\u6613\u6c27\u5316\u53d8\u8d28\uff0c\u9047\u6c34\u5bb9\u6613\u7206\u70b8\uff0c\u6240\u4ee5\u8d2d\u4e70\u56de\u6765\u7684\u91d1\u5c5e\u9502\u7247\u9700\u8981\u5728\u624b\u5957\u7bb1\u4e2d\u6253\u5f00\uff0c\u6253\u5f00\u65f6\u6ce8\u610f\uff0c\u4e0d\u8981\u635f\u574f\u624b\u5957\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/3-9.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-14097\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/3-9.png\" alt=\"3\" width=\"387\" height=\"236\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/3-9.png 387w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/3-9-300x183.png 300w\" sizes=\"(max-width: 387px) 100vw, 387px\" \/><\/a><\/p>\n<p style=\"text-align: center;\">\u56fe3 \u00a0\u9002\u5408CR2032\u7535\u6c60\u4f7f\u7528\u7684\u91d1\u5c5e\u9502\u7247<\/p>\n<p style=\"text-align: left;\"><strong>1.5 \u00a0\u57ab\u7247<\/strong><\/p>\n<p>\u57ab\u7247\u4e3a\u5706\u5f62\u7684\u94dd\u7247\uff0c\u76f4\u5f84\u4e0e\u9502\u7247\u5927\u5c0f\u4e00\u6837\uff0c\u5b9e\u9a8c\u4e2d\uff0c\u53ef\u4ee5\u6839\u636e\u9700\u6c42\u8d2d\u4e70\u4e0d\u540c\u89c4\u683c\u548c\u539a\u5ea6\u7b49\u3002<\/p>\n<p><strong>\u6ce8\u610f\uff1a<\/strong>\u57ab\u7247\u3001\u6b63\u8d1f\u6781\u58f3\u7b49\u7ec4\u4ef6\uff0c\u5728\u4f7f\u7528\u524d\u8981\u7528\u9152\u7cbe\u53cd\u590d\u8d85\u58f0\u6e05\u6d17\uff0c\u7136\u540e\u9f13\u98ce\u5e72\u71e5\u7bb1\u70d8\u5e72<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/4-11.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-14098\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/4-11.png\" alt=\"4\" width=\"327\" height=\"263\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/4-11.png 327w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/4-11-300x241.png 300w\" sizes=\"(max-width: 327px) 100vw, 327px\" \/><\/a><\/p>\n<p style=\"text-align: center;\">\u56fe4 \u00a0\u57ab\u7247<\/p>\n<p><strong>1.6 \u00a0\u5f39\u7247\uff08\u652f\u6491\u7247\uff09<\/strong><\/p>\n<p>\u5f39\u7247\u4e3b\u8981\u662f\u8d77\u5230\u652f\u6491\u7535\u6c60\u7684\u4f5c\u7528\uff0c\u5982\u679c\u6ca1\u6709\u5f39\u7247\uff0c\u5728\u538b\u7535\u6c60\u7684\u6b65\u9aa4\u4e2d\u4f1a\u628a\u7535\u6c60\u538b\u7684\u5f88\u6241\uff0c\u5185\u90e8\u7ec4\u4ef6\u53ef\u80fd\u88ab\u538b\u574f\u3002\u5f39\u7247\u53ea\u5728\u8d1f\u6781\u4fa7\u52a0\uff0c\u4f46\u662f\u82e5\u6b63\u8d1f\u6781\u90fd\u52a0\u4e86\u5f39\u7247\uff0c\u538b\u7535\u6c60\u6b65\u9aa4\u4e2d\u4e0d\u80fd\u5c06\u6263\u7535\u5c01\u95ed\uff0c\u5bfc\u81f4\u7535\u89e3\u6db2\u4e0e\u7a7a\u6c14\u63a5\u89e6\uff0c\u800c\u5b9e\u9a8c\u5931\u8d25\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/5-11.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-14099\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/05\/5-11.png\" alt=\"5\" width=\"217\" height=\"207\" \/><\/a><\/p>\n<p style=\"text-align: center;\">\u56fe5\u00a0 \u5f39\u7247\uff08\u652f\u6491\u7247\uff09<\/p>\n<p><strong>1.7 \u00a0\u7535\u89e3\u6db2<\/strong><\/p>\n<p>\u4e0d\u540c\u7684\u6750\u6599\u4e00\u822c\u5bf9\u5e94\u4e0d\u540c\u7684\u7535\u89e3\u6db2\uff0c\u5728\u8fdb\u884c\u65f6\u5b9e\u9a8c\u65f6\u5343\u4e07\u4e0d\u8981\u56fe\u7701\u4e8b\u5c06\u5c31\uff0c\u5c0f\u6279\u91cf\u7684\u7535\u89e3\u6db2\u53ef\u4ee5\u627e\u516c\u53f8\u7d22\u8981\uff0c\u4e00\u822c\u90fd\u4f1a\u7ed9\u3002\u4e2a\u522b\u7279\u6b8a\u7684\u7535\u89e3\u6db2\uff0c\u5982\u4f4e\u6e29\u7535\u89e3\u6db2\u7b49\uff0c\u53ef\u80fd\u9700\u8981\u8d2d\u4e70\uff0c\u4ef7\u683c\u8fd8\u4e0d\u4f4e\u3002<\/p>\n<p><strong>2\u00a0 \u6263\u5f0f\u7535\u6c60\u7684\u7ec4\u88c5<\/strong><\/p>\n<p><strong>2.1\u00a0 \u6b63\u6781\u7247\u7684\u5236\u5907<\/strong><\/p>\n<p>\u6781\u7247\u7684\u5236\u5907\u4e3b\u8981\u5206\u4e3a\u4e24\u4e2a\u6b65\u9aa4\uff1a\uff081\uff09\u6d46\u6599\u7684\u5236\u5907\uff1b\uff082\uff09\u6d82\u5e03\u3001\u5e72\u71e5\u3001\u538b\u7247\u7b49\u6b65\u9aa4\u3002<\/p>\n<p><strong>2.1.1 \u00a0\u6d46\u6599\u7684\u5236\u5907\uff08\u4ee5\u78f7\u9178\u94c1\u9502\u4e3a\u4f8b\uff09<\/strong><\/p>\n<table width=\"100%\">\n<tbody>\n<tr>\n<td width=\"158\">\u6eb6\u5242<\/td>\n<td width=\"113\">\u6b63\u6781\u6750\u6599<\/td>\n<td width=\"123\">\u5bfc\u7535\u5242<\/td>\n<td width=\"173\">\u7c98\u7ed3\u5242<\/td>\n<\/tr>\n<tr>\n<td width=\"158\">N-\u7532\u57fa\u5421\u54af\u70f7\u916e\uff08NMP\uff09<\/td>\n<td width=\"113\">\u78f7\u9178\u94c1\u9502<\/td>\n<td width=\"123\">Super P<\/td>\n<td width=\"173\">\u805a\u504f\u4e8c\u6c1f\u4e59\u70ef\uff08PVDF\uff09<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u6d46\u6599\u7531\u6eb6\u5242\u3001\u6b63\u6781\u6750\u6599\u3001\u5bfc\u7535\u5242\u548c\u7c98\u7ed3\u5242\u7ec4\u6210\uff0c\u6211\u4eec\u4f1a\u5728\u4ee5\u540e\u7684\u51e0\u671f\u4e2d\u6bcf\u79cd\u7c7b\u522b\u4e2d\u5305\u542b\u7684\u4e0d\u540c\u7684\u6750\u6599\u5206\u522b\u4ecb\u7ecd\u3002<\/p>\n<p>\u5b9e\u9a8c\u5ba4\u4e00\u822c\u91c7\u7528\u6b63\u6781\u6750\u6599\uff1a\u5bfc\u7535\u5242\uff1a\u7c98\u7ed3\u5242\u7684\u8d28\u91cf\u6bd4\u4e3a80\uff1a10\uff1a10\u3002\u5f53\u7136\uff0c\u8fd9\u4e2a\u6bd4\u4f8b\u53ef\u4ee5\u81ea\u7531\u8c03\u8282\uff0c\u4f46\u8c03\u6574\u8fc7\u7a0b\u9700\u8981\u5927\u91cf\u7684\u8bd5\u9519\u3002\u4f46\u4e00\u822c\u6765\u8bf4\uff0c\u6b63\u6781\u6750\u6599\u4e0d\u4f4e\u4e8e75\uff0c\u5bfc\u7535\u5242\u548c\u7c98\u7ed3\u5242\u4e0d\u4f4e\u4e8e5\u3002\u6709\u65f6\u5019\u4e3a\u4e86\u8fbe\u5230\u9ad8\u500d\u7387\u6027\u80fd\uff0c\u6709\u62a5\u9053\u4e2d\u5bfc\u7535\u5242\u6bd4\u4f8b\u6709\u8fbe\u523040\u7684\u60c5\u51b5\u3002<\/p>\n<p>\u82e5\u5236\u5907\u7684\u6b63\u6781\u6750\u6599\u8f83\u5c11\uff0c\u53ef\u4ee5\u5c06\u4e09\u79cd\u7269\u8d28\u6309\u6bd4\u4f8b\u6df7\u5408\uff0c\u7528\u5438\u7ba1\u5047\u5982\u9010\u6ef4\u5047\u5982NMP\uff0c\u7136\u540e\u5c0f\u7814\u94b5\u4e2d\u7814\u78e8\uff0c\u8fd9\u4e2a\u8fc7\u7a0b\u4e2d\u8981\u6ce8\u610f\u6eb6\u5242NMP\u7684\u91cf\uff0c\u82e5NMP\u52a0\u5165\u7684\u8fc7\u591a\uff0c\u53ef\u4ee5\u5728\u7ea2\u5916\u7ea2\u706f\u4e0b\u9002\u5f53\u70d8\u5e72\u3002<\/p>\n<p>\u6d3b\u6027\u7269\u8d28\u8f83\u591a\u65f6\uff0c\u53d60.4g\u6d3b\u6027\u7269\u8d28\uff0c\u76f8\u5e94\u7684\u5bfc\u7535\u5242\u548c\u7c98\u7ed3\u5242\u7684\u91cf\u4e3a0.05g\uff0c\u4f7f\u752820*20\u6216\u800520*40\u89c4\u683c\u7684\u79f0\u91cf\u74f6\uff0c\u5148\u540e\u52a0\u5165NMP\u3001\u6d3b\u6027\u7269\u8d28\u3001\u5bfc\u7535\u5242\u548c\u7c98\u7ed3\u5242\uff0c\u52a0\u5165\u6b21\u5e8f\u5f71\u54cd\u6700\u7ec8\u6781\u7247\u7684\u5236\u5907\u8d28\u91cf\u3002\u6839\u636e\u300a\u6263\u5f0f\u9502\u79bb\u5b50\u7535\u6c60\u7684\u5236\u5907\u5de5\u827a\u7814\u7a76\u300b\u4ee5\u53ca\u4e00\u4e9b\u7814\u53cb\u7684\u5b9e\u9a8c\u7ecf\u9a8c\uff0c\u6309\u4ee5\u4e0b\u6b21\u5e8f\u6dfb\u52a0\u5404\u7269\u8d28\uff0c\u6548\u679c\u6700\u597d\u3002<\/p>\n<p><strong>NMP<\/strong><strong>\u548c<\/strong><strong>PVDF<\/strong><strong>\u6eb6\u6db2\u7684\u914d\u5236<\/strong><\/p>\n<p>\u9996\u5148\uff0c\u914d\u5236NMP\u548cPVDF\u7684\u6eb6\u6db2\uff0c\u8fd9\u6837\u5728\u6bcf\u6b21\u914d\u5236\u6d46\u6599\u65f6\u80fd\u8282\u7701\u5f88\u591a\u65f6\u95f4\uff0c\u53ef\u4ee5\u914d\u52360.02g\/ml\u30010.025g\/ml\u548c0.03g\/ml\u7684\u4e09\u79cd\uff0c\u9009\u62e9\u5408\u9002\u81ea\u5df1\u6750\u6599\u7684\u6d53\u5ea6\u4f7f\u7528\u3002\u914d\u5236\u65b9\u6cd5\u5f88\u7b80\u5355\uff0c\u53ea\u9700\u8981\u5c06\u4e24\u79cd\u7269\u8d28\u5728\u5e7f\u53e3\u74f6\u4e2d\u6df7\u5408\u5c31\u884c\uff0c\u901a\u8fc7\u78c1\u529b\u6405\u62cc\uff0c\u6eb6\u6db2\u4e2d\u6ca1\u6709\u767d\u8272\u7269\u8d28\u5c31\u884c\u3002<strong>\u9700\u8981\u6ce8\u610f\u7684\u662f\uff1a<\/strong>\u914d\u5236\u7ed3\u675f\u540e\uff0c\u5e7f\u53e3\u74f6\u8981\u901a\u8fc7\u5c01\u53e3\u80f6\u5bc6\u5c01\uff0c\u56e0\u4e3aNMP\u5bb9\u6613\u5438\u6c34\u6216\u8005\u53d8\u8d28\u3002<\/p>\n<p><strong>\u6d46\u6599\u7684\u914d\u7f6e\u6b65\u9aa4\uff1a<\/strong><\/p>\n<p>\u7b2c\u4e00\u6b65\uff1a\u7528\u79fb\u6db2\u67aa\u91cf\u53d62ml\u76840.025g\/ml \u7684NMP\/PVDF\u6eb6\u6db2\uff0c\u653e\u5165D15\u6405\u62cc\u5b50\u8fdb\u884c\u78c1\u529b\u6405\u62cc\uff1b<\/p>\n<p>\u7b2c\u4e8c\u6b65\uff1a\u79f0\u53d60.05g\u5bfc\u7535\u5242Super P\u7f13\u6162\u52a0\u5165\u79f0\u91cf\u74f6\u4e2d\uff0c\u6405\u62cc20min\u3002\u52a0\u5165\u8fc7\u7a0b\u4e2d\u5c3d\u91cf\u4e0d\u8981\u4f7f\u5bfc\u7535\u5242\u78b0\u5230\u4e0a\u4fa7\u74f6\u58c1\uff0c\u66f4\u4e0d\u8981\u56e0\u4e3a\u52a0\u5165\u7684\u592a\u5feb\u800c\u4f7f\u5bfc\u7535\u5242\u6563\u51fa\u79f0\u91cf\u74f6\u3002<\/p>\n<p>\u7b2c\u4e09\u6b65\uff1a\u79f0\u53d60.4g\u6d3b\u6027\u7269\u8d28\uff0c\u52a0\u5165\u79f0\u91cf\u74f6\u4e2d\u3002\u6ce8\u610f\u4e8b\u9879\u540c\u4e0a\uff0c\u52a0\u5165\u540e\u6405\u62cc4-5\u5c0f\u65f6\uff0c\u6405\u62cc\u65f6\u95f4\u4e0d\u56fa\u5b9a\uff0c\u4ee5\u6d46\u6599\u7c98\u7a20\u72b6\u6001\u4e3a\u51c6\u3002<\/p>\n<p>\u53e6\u6709\u62a5\u9053\uff0c\u5728\u78c1\u529b\u6405\u62cc\u540e\uff0c\u8fdb\u884c15min\u7684\u8d85\u58f0\u6405\u62cc\uff0c\u6027\u80fd\u66f4\u597d\u3002<\/p>\n<p><strong>\u4f55\u79cd\u6d46\u6599\u72b6\u6001\u4e3a\u6700\u597d\uff1f<\/strong><\/p>\n<p>\u4e00\u822c\u6765\u8bf4\uff0c\u8f7b\u8f7b\u6643\u52a8\u79f0\u91cf\u74f6\uff0c\u6df7\u5408\u7269\u65e2\u4e0d\u662f\u7c98\u5ea6\u5f88\u9ad8\u65e0\u6cd5\u6d41\u52a8\uff0c\u53c8\u4e0d\u662f\u50cf\u6c34\u4e00\u6837\u6613\u52a8\u800c\u4e0d\u6302\u58c1\u5373\u53ef\u3002\u592a\u7a20\u53ef\u4ee5\u52a0\u5165\u4e00\u6ef4NMP\u7ee7\u7eed\u6405\u62cc\u4e00\u4f1a\u513f\uff0c\u4e00\u822c\u4e00\u6ef4\u5c31\u8db3\u591f\u4e86\u3002\u592a\u7a00\u53ef\u4ee5\u5c06\u79f0\u91cf\u74f6\u653e\u5165\u9f13\u98ce\u5e72\u71e5\u7bb1\u70d8\u5e72\u4e00\u4f1a\u513f\u3002<\/p>\n<p>\u4e5f\u53ef\u4f7f\u7528\u738b\u7426\u5e08\u5144\u7684\u914d\u6599\u65b9\u5f0f\uff0c\u4e0d\u8fc7\u8fd9\u79cd\u65b9\u5f0f\u8017\u65f6\u8f83\u957f\u3002<\/p>\n<p><strong>\u6ce8\u610f\uff1a\u7b2c\u4e8c\u4e09\u6b65\u7684\u987a\u5e8f\u5c3d\u91cf\u4e0d\u8981\u98a0\u5012\u3002<\/strong><\/p>\n<p><strong>2.1.2\u00a0 \u6781\u7247\u7684\u6d82\u5e03<\/strong><\/p>\n<p>\u4e00\u822c\u4f7f\u7528\u522e\u5200\u548c\u6d41\u5ef6\u6d82\u8986\u673a\uff0c\u8fdb\u884c\u6d82\u5e03\uff0c\u6b63\u6781\u6750\u6599\u6d82\u5e03\u5728\u94dd\u7b94\u4e0a\uff0c\u8d1f\u6781\u6d82\u5e03\u5728\u94dc\u7b94\u4e0a\u3002\u6ca1\u6709\u6d82\u8986\u673a\u7684\u540c\u5b66\u53ef\u4ee5\u4f7f\u7528\u73bb\u7483\u677f\u548c\u522e\u5200\u8fdb\u884c\u6d82\u5e03\u3002\u6d82\u5e03\u8fc7\u7a0b\u6bd4\u8f83\u7b80\u5355\uff0c\u4f46\u662f\u9700\u8981\u6ce8\u610f\u4ee5\u4e0b\u51e0\u70b9<\/p>\n<p>\uff081\uff09\u94dd\u7b94\u9700\u8981\u5e73\u6574\uff0c\u8981\u5c3d\u53ef\u80fd\u7684\u51cf\u5c11\u8936\u76b1\uff1b\uff082\uff09\u6d82\u5e03\u524d\u8981\u7528\u9152\u7cbe\u548c\u8131\u8102\u68c9\u4ed4\u7ec6\u6e05\u6d01\u94dd\u7b94\u548c\u6d82\u8986\u673a\u5e73\u53f0\uff1b\uff083\uff09\u8131\u8102\u68c9\u6e05\u6d01\u540e\u8981\u7528\u536b\u751f\u7eb8\u5c0f\u5fc3\u6e05\u6d01\u4e00\u6b21\uff0c\u4e00\u6765\u53bb\u6389\u53ef\u80fd\u5b58\u5728\u7684\u68c9\u7d6e\u4e8c\u6765\u4e0d\u8981\u5212\u4f24\u94dd\u7b94\u3002<\/p>\n<p><strong>2.1.3\u00a0 \u6781\u7247\u7684\u5e72\u71e5\u548c\u538b\u7247<\/strong><\/p>\n<p>\u4e4b\u6240\u4ee5\u8981\u5355\u5217\u4e00\u8282\uff0c\u662f\u56e0\u4e3a\u8fd9\u662f\u4e2a\u9700\u8981\u4e25\u683c\u6267\u884c\u7684\u8fc7\u7a0b\uff0c\u4f46\u662f\u5e72\u71e5\u6e29\u5ea6\u53ef\u4ee5\u6709\u53d8\u5316\u3002\u53e6\u5916,\u6781\u7247\u8d28\u91cf\u7684\u597d\u574f\u53ef\u4ee5\u7528\u6389\u7c89\u7a0b\u5ea6\u6765\u8861\u91cf,\u82e5\u6389\u7c89\u5bb9\u6613,\u7535\u6c60\u5728\u5faa\u73af\u8fc7\u7a0b\u4e2d,\u6d3b\u6027\u7269\u8d28\u4f1a\u4ece\u94dd\u7b94\u4e0a\u8131\u843d,\u6eb6\u89e3\u5728\u7535\u89e3\u6db2\u91cc,\u9694\u819c\u4f1a\u88ab\u67d3\u9ed1\u3002<\/p>\n<p>\u5e72\u71e5\u7684\u76ee\u7684\u5728\u4e8e\u53bb\u9664\u6d46\u6599\u4e2d\u5927\u91cf\u7684\u6eb6\u5242NMP\u4ee5\u53ca\u5176\u4e2d\u7684\u6c34\u5206\uff0c\u6240\u4ee5\u8981\u7ecf\u8fc7\u9f13\u98ce\u5e72\u71e5\u548c\u771f\u7a7a\u5e72\u71e5\u4e24\u4e2a\u6b65\u9aa4\u3002\u6bcf\u4e2a\u6b65\u9aa4\u7684\u5177\u4f53\u6e29\u5ea6\u548c\u65f6\u95f4\uff0c\u4e0d\u540c\u5de5\u4f5c\u4e2d\u6709\u4e0d\u540c\u7684\u62a5\u9053\uff0c\u4f46\u9700\u8981\u6ce8\u610f\uff1a<\/p>\n<p>\uff081\uff09\u5e72\u71e5NMP\u7684\u6e29\u5ea6\u4e0d\u9700\u8981\u592a\u9ad8\uff0c\u4f46\u7531\u4e8e\u6eb6\u5242\u592a\u591a\uff0c\u9700\u8981\u8f83\u591a\u7684\u70ed\u91cf\uff0c\u6240\u4ee5\u5e72\u71e5\u65f6\u95f4\u8f83\u957f\uff1b<\/p>\n<p>\uff082\uff09\u7531\u4e8e\u6c34\u7684\u6cb8\u70b9\u662f100\u2103\uff0c\u6240\u4ee5\u9f13\u98ce\u5e72\u71e5\u7684\u6e29\u5ea6\u9700\u8981\u8f83\u9ad8\uff0c\u4f46\u7531\u4e8e\u6c34\u5206\u542b\u91cf\u8f83\u5c11\uff0c\u5e72\u71e5\u65f6\u95f4\u53ef\u4ee5\u7f29\u77ed\uff0c\u5728\u9f13\u98ce\u5e72\u71e5\u65f6\uff0c\u53ef\u4ee5\u8bbe\u7f6e\u4e24\u4e2a\u6e29\u5ea6\u6bb5\uff0c\u6bcf\u4e2a\u6e29\u5ea6\u65f6\u95f4\u4e0d\u540c\uff0c\u6700\u9ad8\u6e29\u5ea6\u53ef\u4ee5\u8bbe\u7f6e\u4e3a100\u2103\u3002\u53e6\u5916\u8d1f\u6781\u7684\u5e72\u71e5\u6e29\u5ea6\u5e94\u4f4e\u4e8e\u6b63\u6781\uff0c\u6709\u65f6\u5019\u51fa\u73b0\u94dc\u7b94\u6c27\u5316\u7684\u73b0\u8c61\uff1b<\/p>\n<p><strong>\u6ce8\u610f\uff1a<\/strong>\u5e72\u71e5\u6e29\u5ea6\u8fc7\u9ad8\u548c\u65f6\u95f4\u8fc7\u957f\uff0c\u4f1a\u51fa\u73b0\u4e25\u91cd\u7684\u6389\u7c89\u884c\u4e3a\uff0c\u5173\u4e8e\u9f13\u98ce\u5e72\u71e5\u7684\u6e29\u5ea6\uff0c\u6b63\u6781\u4e0d\u5e94\u8d85\u8fc7120\u2103\uff0c\u8d1f\u6781\u4e0d\u8d85\u8fc790\u2103\u3002<\/p>\n<p>\uff083\uff09\u9f13\u98ce\u5e72\u71e5\u540e\uff0c\u8981\u7ecf\u8fc7\u771f\u7a7a\u5e72\u71e5\uff0c\u6e29\u5ea6\u4e00\u822c\u8bbe\u5b9a\u4e3a120\u2103\uff0c\u65f6\u95f410\u5c0f\u65f6\u5de6\u53f3\u3002\u4f46\u4e0d\u53ef\u4ee5\u4e0d\u7ecf\u8fc7\u9f13\u98ce\u5e72\u71e5\u76f4\u63a5\u8fdb\u884c\u771f\u7a7a\u5e72\u71e5\uff0c\u8fd9\u6837\u64cd\u4f5c\u4f1a\u5bfc\u81f4NMP\u5145\u6ee1\u4e8e\u771f\u7a7a\u5e72\u71e5\u7bb1\u5185\uff0c\u800c\u4f7f\u5e72\u71e5\u6548\u679c\u4e0d\u597d\u3002\u4e0d\u7ecf\u8fc7\u771f\u7a7a\u5e72\u71e5\u4e5f\u662f\u53ef\u4ee5\u7684\uff0c\u4f46\u662f\u6709\u6761\u4ef6\u7684\u6700\u597d\u4e0d\u8981\u7701\u7565\u8fd9\u4e2a\u6b65\u9aa4\u3002<\/p>\n<p><strong>2.1.4\u00a0 \u538b\u7247<\/strong><\/p>\n<p>\u6d82\u5e03\u540e\uff0c\u5e72\u71e5\u51fa\u7684\u590d\u5408\u6750\u6599\u6d82\u5c42\u6bd4\u8f83\u758f\u677e\u3002\u82e5\u76f4\u63a5\u4f7f\u7528\uff0c\u88ab\u7535\u89e3\u6db2\u6d78\u6da6\u540e\u5bb9\u6613\u8131\u843d\u635f\u574f\u3002\u53ef\u91c7\u7528\u5bf9\u8f8a\u673a\u6216\u8005\u538b\u7247\u673a\u7b49\u8fdb\u884c\u538b\u7247\u5904\u7406\uff0c\u5bf9\u8f8a\u673a\u4e00\u822c\u53ef\u5c06\u6b63\u6781\u7247\u6d82\u5c42\u538b\u5236\u523015-60\u03bcm\u3002\u538b\u7247\u673a\u53ef\u4ee5\u91c7\u7528\u5927\u7ea680-120kg\/cm<sup>2<\/sup>\u538b\u5f3a\u8fdb\u884c\u538b\u5236\u3002\u538b\u7247\u540e\u7684\u7535\u6781\uff0c\u7a33\u5b9a\u6027\u3001\u7262\u56fa\u6027\u4ee5\u53ca\u7535\u5316\u5b66\u6027\u80fd\u90fd\u83b7\u5f97\u4e86\u6539\u5584\uff0c\u6d4b\u8bd5\u8868\u73b0\u8981\u597d\u4e8e\u4e0d\u538b\u7247\u7684\u6837\u672c\u3002\u538b\u7247\u4e3b\u8981\u76ee\u7684\u6709\u4e24\u4e2a\uff1a\u4e00\u662f\u4e3a\u4e86\u6d88\u9664\u6bdb\u523a\uff0c\u4f7f\u8868\u9762\u5149\u6ed1\u3001\u5e73\u6574\uff0c\u9632\u6b62\u88c5\u7535\u6c60\u65f6\u6bdb\u523a\u523a\u7834\u9694\u819c\u5f15\u8d77\u77ed\u8def\uff1b\u4e8c\u662f\u589e\u5f3a\u6781\u7247\u7684\u5f3a\u5ea6\uff0c\u51cf\u5c0f\u6b27\u59c6\u963b\u6297\u3002\u538b\u529b\u8fc7\u5927\u4f1a\u5f15\u8d77\u6781\u7247\u7684\u5377\u66f2\uff0c\u4e0d\u5229\u4e8e\u7535\u6c60\u88c5\u914d\uff0c\u538b\u529b\u8fc7\u5c0f\u53c8\u8d77\u4e0d\u5230\u538b\u7247\u7684\u4f5c\u7528\u3002<\/p>\n<p>\u88c1\u526a\u9694\u819c\u3001\u6781\u7247\u4ee5\u53ca\u6d3b\u6027\u7269\u8d28\u542b\u91cf\u8ba1\u7b97\u7684\u6b65\u9aa4\u5728\u6b64\u5ffd\u7565\uff0c\u8f83\u4e3a\u7b80\u5355\uff0c\u6709\u95ee\u9898\u8bf7\u5728\u6750\u6599\u4eba\u5fae\u4fe1\u6216\u8005\u6750\u6599\u725b\u539f\u7f51\u9875\u7559\u8a00\u3002<\/p>\n<p><strong>2.1\u00a0 \u6263\u5f0f\u7535\u6c60\u7684\u7ec4\u88c5<\/strong><\/p>\n<p><strong>2.1.1\u00a0 \u5fc5\u5907\u7269\u54c1\uff1a<\/strong><\/p>\n<p>\u624b\u5957\u7bb1\u5185\uff1a\u538b\u7247\u673a(\u6700\u597d\u5e26\u6570\u663e)\u3001\u954a\u5b502\u628a\uff08\u81f3\u5c11\u6709\u4e00\u628a\u662f\u5851\u6599\u954a\u5b50\uff09\u3001\u836f\u53191\u628a\u3001\u7535\u89e3\u6db2\u3001\u9502\u7247\u3001\u78e8\u53e3\u73bb\u7483\u74f6(\u914d\u80f6\u5934\u6ef4\u7ba1)\u3001\u6ce8\u5c04\u5668\u3001\u5e72\u71e5\u7eb8\u5dfe\u7b49\u6e05\u6d01\u7528\u54c1\uff1b<\/p>\n<p>\u624b\u5957\u7bb1\u5916\uff1a\u6263\u5f0f\u7535\u6c60\u58f3\u3001\u96c6\u7535\u5668\u3001\u5f39\u7c27\u7247\uff08\u6216\u6ce1\u6cab\u954d\uff09\u3001\u6b63\u6781\u7247\u3001\u9694\u819c\u7247\uff1b<\/p>\n<p><strong>\u6ce8\u610f\uff1a<\/strong>\u7535\u6c60\u7ec4\u88c5\u90e8\u4ef6\u5728\u653e\u5165\u624b\u5957\u7bb1\u4e2d\u4e4b\u524d\uff0c\u8981\u8fdb\u884c4\u5c0f\u65f6\u5de6\u53f3\u7684\u771f\u7a7a\u5e72\u71e5\u5904\u7406\uff0c\u6e29\u5ea6\u4e0d\u5b9c\u592a\u9ad8\uff0c\u53ef\u4ee5\u8bbe\u7f6e\u572860-80\u2103\u6e29\u5ea6\u3002\u5bb9\u91cf\u8f83\u5927\u7684\u624b\u5957\u7bb1\u53ef\u4e8b\u5148\u8fd9\u4e9b\u5b58\u50a8\u7535\u6c60\u90e8\u4ef6\uff0c\u66f4\u6e05\u6d01\u3002\u539f\u6599\u5165\u8fdb\u7bb1\u8231\u95e8\u540e\uff0c\u4e25\u683c\u6309\u7167\u64cd\u4f5c\u89c4\u7a0b\u8fdb\u884c\u6392\u6c14-\u8fdb\u6c14\u64cd\u4f5c\uff0c\u81f3\u5c11\u4e09\u6b21\u3002\u5efa\u8bae\u5728\u624b\u5957\u7bb1\u5185\u4e13\u95e8\u653e\u4e00\u4e2a\u5c0f\u578b\u64cd\u4f5c\u53f0\uff0c\u4ee5\u9632\u8bd5\u5242\u8150\u8680\u624b\u5957\u7bb1\u3002\u7535\u89e3\u6db2\u5bf9\u4e8e\u624b\u5957\u548c\u624b\u5957\u7bb1\u5185\u58c1\u7684\u8150\u8680\u6bd4\u8f83\u4e25\u91cd\uff0c\u5e94\u8be5\u5c3d\u91cf\u907f\u514d\u64cd\u4f5c\u5931\u8bef\u3002<\/p>\n<p><strong>2.1.2\u00a0 \u786e\u5b9a\u6c34\u6c27\u542b\u91cf<\/strong><\/p>\n<p>\u4e00\u822c\u7684\u624b\u5957\u7bb1\u90fd\u6709\u6c34\u6c27\u542b\u91cf\u7684\u6570\u663e\u68c0\u6d4b\u4eea\uff0c\u5e03\u83b1\u6069\u7684\u624b\u5957\u7bb1\u6c34\u6c27\u542b\u91cf\u53ef\u4ee5\u63a7\u5236\u5728\u4f4e\u4e8e0.05PPM\uff0c\u4f46\u4e0d\u540c\u624b\u5957\u7bb1\u7684\u6807\u51c6\u4e0d\u5c3d\u76f8\u540c\u3002\u7ec4\u88c5\u7535\u6c60\u7684\u8fc7\u7a0b\uff0c\u90fd\u5728\u5df2\u7ecf\u4e25\u683c\u8fdb\u884c\u4e86\u6392\u6c14-\u8fdb\u6c14\u64cd\u4f5c\u7684\u624b\u5957\u7bb1\u4e2d\uff0c\u4e25\u683c\u9694\u7edd\u4efb\u4f55\u53ef\u80fd\u7684\u6c27\u5316\u3001\u6f6e\u6e7f\u7b49\u5e72\u6270\u3002\u82e5\u624b\u5957\u7bb1\u7684\u6c34\u6c27\u542b\u91cf\u4e00\u76f4\u8f83\u9ad8\uff0c\u5e94\u8be5\u68c0\u67e5\u624b\u5957\u662f\u5426\u7834\u635f\u6216\u8005\u5bf9\u624b\u5957\u7bb1\u8fdb\u884c\u518d\u751f\u3002<\/p>\n<p><strong>2.1.3\u00a0 \u7ec4\u88c5\u8fc7\u7a0b<\/strong><\/p>\n<p>\u6263\u5f0f\u7535\u6c60\u7ec4\u88c5\u6b21\u5e8f\u4e3b\u8981\u6709\u4e24\u79cd\uff0c\u6211\u4eec\u5b9e\u9a8c\u5ba4\u4e00\u822c\u4e60\u60ef\u4ece\u8d1f\u6781\u58f3\u5f00\u59cb\uff0c\u4f46\u4e5f\u53ef\u4ee5\u4ece\u6b63\u6781\u58f3\u5f00\u59cb\uff0c\u8fd9\u4e2a\u6ca1\u6709\u5bf9\u9519\u4e4b\u5206\uff0c\u5168\u770b\u4e2a\u4eba\u4e60\u60ef\u3002<\/p>\n<p><strong>|<\/strong><strong>\u8d1f\u6781\u58f3|\u5f39\u7247|\u57ab\u7247\u4e28\u9502\u7247\u4e28\u7535\u89e3\u6db2|\u9694\u819c|\u7535\u89e3\u6db2|\u6b63\u6781\u7247|\u57ab\u7247\u4e28\u6b63\u6781\u58f3|<\/strong><\/p>\n<table width=\"100%\">\n<tbody>\n<tr>\n<td width=\"26\"><strong>\u00a0<\/strong><\/td>\n<td width=\"170\">\u6b65\u9aa4\u63cf\u8ff0<\/td>\n<td width=\"372\">\u6b65\u9aa4\u8bf4\u660e<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>1<\/strong><\/td>\n<td width=\"170\">\u6b63\u6781\u58f3\u5f00\u53e3\u9762\u5411\u4e0a\uff0c\u5e73<\/p>\n<p>\u653e\u4e8e\u73bb\u7483\u677f\u4e0a<\/td>\n<td width=\"372\">\u65e0\u9700\u8bf4\u660e<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>2<\/strong><\/td>\n<td width=\"170\">\u7528\u954a\u5b50\u5c06\u57ab\u7247\u548c\u6b63\u6781\u7247\u4f9d\u6b21\u7f6e\u5165\u6b63\u6781\u58f3\uff0c\u6b63\u6781\u7247\u4f4d\u4e8e\u6b63\u4e2d<\/td>\n<td width=\"372\">\u7528\u954a\u5b50\u5c06\u57ab\u7247\u7f6e\u5165\u6b63\u6781\u58f3\uff0c\u6709\u6bdb\u523a\u7684\u4e00\u9762\u671d\u4e0b\uff0c\u7136\u540e\u5c0f\u5fc3\u5939\u53d6\u6b63\u6781\u7247\uff0c\u5c06\u6d82\u5e03\u5c42\u5411\u4e0a\uff0c\u653e\u4e8e\u6b63\u6781\u58f3\u7684\u6b63\u4e2d\u95f4\u3002\u8fd9\u4e00\u6b65\u9aa4\u5e94\u8be5\u53cd\u590d\u7ec3\u4e60\uff0c\u786e\u4fdd\u954a\u5b50\u5939\u53d6\u7684\u529b\u5ea6\u5408\u9002\uff0c\u4e0d\u4f1a\u635f\u4f24\u6b63\u6781\u7247\uff0c\u4e25\u9632\u5f2f\u6298\u6216\u8005\u626d\u66f2\u6b63\u6781\u7247\uff0c\u4fdd\u6301\u5e73\u6574\u7684\u653e\u5728\u6b63\u6781\u58f3\u4e2d<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>3<\/strong><\/td>\n<td width=\"170\">\u91c7\u7528\u80f6\u5934\u6ef4\u7ba1\u6216\u6ce8\u5c04\u5668\u5438\u53d6\u7535\u89e3\u6db2\uff0c\u6d78\u6da6\u6b63\u6781\u7247\u8868\u9762<\/td>\n<td width=\"372\">\u7528\u6781\u7ec6\u7684\u73bb\u7483\u6ef4\u7ba1\u914c\u91cf\u5438\u53d6\u7535\u89e3\u6db2\uff0c\u6b64\u8fc7\u7a0b\u4ee5\u5b8c\u6574\u5747\u5300\u7684\u6da6\u6e7f\u7535\u6781\u7247\u8868\u9762\u4e3a\u76ee\u6807\u3002\u6ce8\u610f\u5728\u6da6\u6e7f\u7684\u8fc7\u7a0b\u4e2d\uff0c\u6ef4\u7ba1\/\u9488\u5934\u548c\u7535\u6781\u7247\u4e00\u5b9a\u4e0d\u80fd\u78b0\u89e6<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>4<\/strong><\/td>\n<td width=\"170\">\u5939\u53d6\u9694\u819c\uff0c\u8986\u76d6\u6b63\u6781\u7247<\/td>\n<td width=\"372\">\u7528\u954a\u5b50\u5939\u53d6\u9694\u819c\uff0c\u7531\u4e8e\u88c1\u526a\u7684\u9694\u819c\u548c\u7535\u6c60\u58f3\u5185\u90e8\u76f4\u5f84\u4e00\u81f4\uff0c\u6070\u597d\u53ef\u4ee5\u88c5\u8fdb\u7535\u6c60\u6b63\u6781\u58f3\u4e2d\u3002\u8fd9\u4e00\u6b65\u5c24\u5176\u8981\u5c0f\u5fc3\uff0c\u4e0d\u8981\u4f7f\u9694\u819c\u63d0\u524d\u63a5\u89e6\u5230\u7535\u89e3\u6db2\uff0c\u5e94\u8be5\u5c06\u9694\u819c\u5148\u5bf9\u51c6\u7535\u6c60\u58f3\u8fb9\u7f18\uff0c\u7f13\u7f13\u9000\u51fa\u954a\u5b50\uff0c\u5747\u5300\u8986\u76d6<\/p>\n<p>\u4e0b<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>5<\/strong><\/td>\n<td width=\"170\">\u518d\u6b21\u4f7f\u7528\u80f6\u5934\u6ef4\u7ba1\/\u6ce8\u5c04\u5668\u5438\u53d6\u7535\u89e3\u6db2\uff0c\u6da6\u6e7f\u9694\u819c\u8868\u9762\u3002<\/td>\n<td width=\"372\">\u7531\u4e8e\u9694\u819c\u662f\u60f0\u6027\u4e14\u6d01\u51c0\u7684\u7269\u8d28\uff0c\u8fd9\u65f6\u53ef\u4ee5\u4f7f\u7528\u6ef4\u7ba1\u524d\u7aef\u8f7b\u8f7b\u78b0\u89e6\u9694\u819c\uff0c\u4f7f\u4e4b\u66f4\u52a0\u5e73\u6574\uff0c\u5747\u5300\uff0c\u8fb9\u7f18\u4e0e\u7535\u6c60\u58f3\u63a5\u89e6\u66f4\u4e3a\u4e25\u5bc6\u3002\u5c3d\u91cf\u907f\u514d\u9694\u819c\u7684\u8936\u76b1<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>6<\/strong><\/td>\n<td width=\"170\">\u5939\u53d6\u9502\u7247\u653e\u7f6e\u4e8e\u9694\u819c<\/p>\n<p>\u6b63\u4e2d<\/td>\n<td width=\"372\">\u9502\u7247\u534a\u5f84\u4e3a15.8mm\uff0c\u5e94\u5f53\u6070\u597d\u653e\u4e8e\u7535\u6c60\u58f3\u4e2d\u95f4\uff0c\u8fd9\u662f\u6700\u96be\u7684\u4e00\u6b65\uff0c\u5fc5\u987b\u4e00\u6b21\u6210\u529f\u3002\u56e0\u4e3a\u9502\u7247\u548c\u7535\u89e3\u6db2\u3001\u9694\u819c\u4f1a\u4ea7\u751f\u7c98\u9644\uff0c\u5982\u679c\u653e\u4e0d\u51c6\uff0c\u8c03\u6574\u975e\u5e38\u56f0\u96be\u3002\u4e5f\u5c31\u610f\u5473\u7740\u6b64\u6b21\u6a21\u62df\u7535\u6c60\u7ec4\u88c5\u7684\u5931\u8d25\uff08\u5176\u5b9e\u4e5f\u4e0d\u4e00\u5b9a\uff0c\u591a\u6ef4\u52a0\u4e00\u70b9\u7535\u89e3\u6db2\uff0c\u5c31\u53ef\u4ee5\u8fdb\u884c\u5fae\u8c03\uff09<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>7<\/strong><\/td>\n<td width=\"170\">\u5939\u53d6\u57ab\u7247\u7f6e\u4e8e\u9502\u7247\u4e0a\uff0c\u4e25\u683c\u5bf9\u9f50<\/td>\n<td width=\"372\">\u8fd9\u4e00\u6b65\u7684\u57ab\u7247\u5982\u679c\u7565\u5fae\u653e\u504f\uff0c\u53ef\u4ee5\u8fdb\u884c\u5c0f\u5fc3\u7684\u8c03\u6574<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>8<\/strong><\/td>\n<td width=\"170\">\u5939\u53d6\u5f39\u7247\u7f6e\u4e8e\u57ab\u7247\u4e0a\uff0c\u4e25\u683c\u5bf9\u9f50<\/td>\n<td width=\"372\">\u6240\u6709\u6b65\u9aa4\u90fd\u5c3d\u91cf\u7528\u954a\u5b50\u64cd\u4f5c\u3002\u5982\u4e0d\u614e\u653e\u504f\uff0c\u8fd9\u4e00\u6b65\u4e5f\u53ef\u4ee5\u8fdb\u884c\u5fae\u8c03\u3002\u6b64\u524d\u7684\u6b65\u9aa4\u4e2d\uff0c\u5982\u679c\u90e8\u4ef6\u7684\u653e\u7f6e\u4f4d\u7f6e\u51fa\u73b0\u504f\u5dee\uff0c\u90fd\u53ef\u4ee5\u7528\u53cc\u624b\u5404\u62ff\u4e00\u628a\u954a\u5b50\uff0c\u914d\u5408\u8fdb\u884c\u8f7b\u5fae\u7684\u8c03\u6574\uff0c\u954a\u5b50\u4e0d\u65b9\u4fbf\u4f7f\u7528\u65f6\uff0c\u53ef\u4f7f\u7528\u836f\u5319<\/td>\n<\/tr>\n<tr>\n<td width=\"26\"><strong>9<\/strong><\/td>\n<td width=\"170\">\u954a\u5b50\u5939\u53d6\u8d1f\u6781\u58f3\u8986\u76d6<\/td>\n<td width=\"372\">\u65e0\u9700\u8bf4\u660e<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><strong>3\u00a0 \u4e00\u4e9b\u95ee\u9898\u51fa\u73b0\u7684\u539f\u56e0<\/strong><\/p>\n<p>\u7535\u6c60\u7ec4\u88c5\u540e\uff0c\u5728\u6d4b\u8bd5\u65f6\u4f1a\u51fa\u73b0\u4e00\u4e9b\u95ee\u9898\uff0c\u4ee5\u4e0b\u662f\u53ef\u80fd\u9047\u5230\u7684\u95ee\u9898\u4ee5\u53ca\u90e8\u5206\u89e3\u91ca<\/p>\n<p><strong>3.1\u00a0 \u5f00\u8def\u7535\u538b\u4f4e\u7684\u539f\u56e0<\/strong><\/p>\n<p>\uff081\uff09\u6781\u7247\u7684\u6bdb\u523a\u7a7f\u7834\u9694\u819c\uff0c\u9020\u6210\u7535\u6c60\u77ed\u8def\uff1b<\/p>\n<p>\uff082\uff09\u7535\u6c60\u88c5\u914d\u8fc7\u7a0b\u4e2d\uff0c\u6b63\u8d1f\u6781\u504f\u79fb\uff0c\u5bfc\u81f4\u77ed\u8def\uff1b<\/p>\n<p>\uff083\uff09\u538b\u7535\u6c60\u6b65\u9aa4\u51fa\u9519\uff0c\u5bfc\u81f4\u7535\u6c60\u88c5\u914d\u4e0d\u7d27\u5bc6\uff0c\u7535\u6c60\u6b63\u8d1f\u6781\u5916\u58f3\u4e0e\u6b63\u8d1f\u6781\u7247\u865a\u63a5\uff0c\u9020\u6210\u77ed\u8def\u3002<\/p>\n<p><strong>3.2\u00a0 \u7535\u5316\u5b66\u963b\u6297\u5927<\/strong><\/p>\n<p>\uff081\uff09\u5bfc\u7535\u5242\u6dfb\u52a0\u91cf\u4e0d\u591f\uff1b<\/p>\n<p>\uff082\uff09\u9694\u819c\u7684\u5b54\u9699\u7387\u5c0f\uff0c\u4f7f\u5f97\u7535\u89e3\u6db2\u4e2d\u7684\u9502\u79bb\u5b50\u4e0d\u80fd\u80fd\u591f\u987a\u5229\u901a\u8fc7\uff1b<\/p>\n<p>\uff083\uff09\u7535\u89e3\u6db2\u5206\u89e3\uff0c\u5176\u4e2d\u7684\u9502\u76d0\u51cf\u5c11\u3002<\/p>\n<p>\u7535\u6c60\u7684\u7ec4\u88c5\u662f\u4e00\u4e2a\u719f\u80fd\u751f\u5de7\u7684\u8fc7\u7a0b\uff0c\u524d\u4e00\u4e24\u6b21\u88c5\u574f\u51e0\u4e2a\u7535\u6c60\u662f\u4e00\u4ef6\u5f88\u6b63\u5e38\u7684\u4e8b\uff0c\u4e0d\u8981\u7070\u5fc3\u3002\u6280\u672f\u6027\u7684\u5de5\u4f5c\u9700\u8981\u7684\u662f\u591a\u7ec3\u4e60\u548c\u89c2\u5bdf\u6539\u8fdb\u3002\u5bf9\u4e8e\u5b9e\u9a8c\u5ba4\u6765\u8bf4\uff0c\u66f4\u91cd\u8981\u7684\u662f\u4f20\u627f\uff0c\u50cf\u6b64\u7c7b\u7b80\u5355\u5de5\u4f5c\uff0c\u6bcf\u5e74\u65b0\u6765\u7684\u5e08\u5f1f\u5e08\u59b9\u90fd\u5f97\u91cd\u65b0\u6478\u7d22\uff0c\u662f\u4e00\u4ef6\u975e\u5e38\u6d6a\u8d39\u65f6\u95f4\u7684\u4e8b\uff0c\u8fd9\u4e5f\u662f\u5e08\u5144\u5e08\u59d0\u7684\u5931\u804c\u3002\u4e00\u4e2a\u6ca1\u6709\u4f20\u627f\u7684\u5b9e\u9a8c\u5ba4\uff0c\u5f88\u96be\u6709\u6df1\u539a\u7684\u79ef\u7d2f\u3002\u6240\u4ee5\uff0c\u5e0c\u671b\u5404\u4f4d\u7855\u535a\u7279\u522b\u662f\u5373\u5c06\u6bd5\u4e1a\u7684\u540c\u5b66\u4eec\u80fd\u591f\u6574\u7406\u81ea\u5df1\u7684\u5b9e\u9a8c\u7b14\u8bb0\uff0c\u5c06\u51e0\u5e74\u7684\u5b66\u672f\u79ef\u7d2f\u7559\u4e0b\u6765\uff0c\u6b22\u8fce\u52a0\u5165\u6750\u6599\u4eba\u5b66\u672f\u5e72\u8d27\u7ec4\uff08\u6750\u6599\u4eba\u79d1\u7814\u5e72\u8d27\u5c0f\u7ec4\u7fa4 563614587\uff09\uff0c\u6211\u4eec\u4e13\u6ce8\u5b9e\u9a8c\u6280\u5de7\u7684\u6536\u96c6\u4e0e\u4f20\u627f\u3002<\/p>\n<p><strong>4\u00a0 \u5b9e\u9a8c\u8bbe\u5907\u4e0e\u8017\u6750\u7684\u8d2d\u4e70<\/strong><\/p>\n<p>\u5bf9\u4e8e\u9502\u7535\u6c60\u4ee5\u53ca\u5176\u4ed6\u65b0\u80fd\u6e90\u7535\u6c60\u6240\u9700\u7684\u8bbe\u5907\u548c\u8017\u6750\u8bd5\u5242\u7b49\uff0c\u53ef\u4ee5\u627e\u6750\u6599\u4eba\u5546\u57ce\u8d2d\u4e70\uff0c\u6211\u4eec\u6709\u5145\u8db3\u7684\u5b9e\u9a8c\u7ecf\u9a8c\u548c\u53ef\u9760\u7684\u8d27\u6e90\uff0c\u5bf9\u4e8e\u5e76\u6709\u5168\u7a0b\u53c2\u4e0e\u65b0\u80fd\u6e90\u5b9e\u9a8c\u5ba4\u7684\u642d\u5efa\u7684\u7ecf\u9a8c\uff0c\u5bf9\u4e8e\u5176\u4e2d\u6240\u9700\u5b9e\u9a8c\u8bbe\u5907\u7684\u8d2d\u4e70\u3001\u5b89\u88c5\u7b49\u5177\u6709\u4e30\u5bcc\u7ecf\u9a8c\uff0c\u6b22\u8fce\u7167\u987e\u6211\u4eec\u751f\u610f\u54e6\uff01<\/p>\n<p>\u8054\u7cfb\u65b9\u5f0f\uff1a<\/p>\n<p>QQ\uff1a\u5b9e\u9a8c\u5ba4\u670d\u52a1\uff1a\u5c0f\u6750\u00a0 3176391711\u00a0\u00a0\u00a0 \u6750\u6599\u4eba\u5ba2\u670d\uff1a\u5927\u6750\u00a0 3130883937<\/p>\n<p>\u7535\u8bdd\uff1a15810216532\uff08\u4f55\u6218\u519b\uff09<\/p>\n<p><strong>\u5173\u4e8e\u7535\u6c60\u7684\u5404\u79cd\u7535\u6d4b\u624b\u6bb5\uff0c\u6211\u4eec\u4ee5\u540e\u4f1a\u9646\u7eed\u4ecb\u7ecd\uff0c\u89c9\u5f97\u6709\u7528\u5c31\u8f6c\u51fa\u53bb\u5427\uff01<\/strong><\/p>\n<p><strong>\u00a0<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u672c\u6587\u4e3b\u8981\u5bf9\u5b9e\u9a8c\u5ba4\u7ec4\u88c5\u6263\u5f0f\u7535\u6c60\u7684\u6d41\u7a0b\u8fdb\u884c\u4ecb\u7ecd\uff0c\u4e3b\u8981\u53c2\u8003\u5317\u5de5\u4e1a\u738b\u7426\u5e08\u5144\u7684\u300a\u9502\u79bb\u5b50\u6a21\u62df\u7535\u6c60\u7ec4\u88c5\u624b\u518c\u300b\u3001\u90d1\u5dde\u8f7b\u5de5\u5b66\u9662\u5f20\u52c7\u7b49\u4eba\u7684\u300a\u6263\u5f0f\u9502\u79bb\u5b50\u7535\u6c60\u7684\u5236\u5907\u5de5\u827a\u7814\u7a76\u300b\u4ee5\u53ca\u4e00\u4e9b\u7f51&#8230;<\/p>\n","protected":false},"author":51,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[18],"class_list":["post-14095","post","type-post","status-publish","format-standard","hentry","category-ganhuo","tag-xinnengyuan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/14095"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/51"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=14095"}],"version-history":[{"count":6,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/14095\/revisions"}],"predecessor-version":[{"id":103491,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/14095\/revisions\/103491"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=14095"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=14095"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=14095"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}