{"id":145524,"date":"2018-07-12T06:30:06","date_gmt":"2018-07-11T22:30:06","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=145524"},"modified":"2018-07-09T18:36:47","modified_gmt":"2018-07-09T10:36:47","slug":"nat-commun-%ef%bc%9a%e5%87%9d%e8%83%b6%e7%94%b5%e8%a7%a3%e8%b4%a8%e8%87%aa%e4%b8%8b%e8%80%8c%e4%b8%8a%e5%a1%ab%e5%85%85%e6%96%b0%e6%96%b9%e6%b3%95%e8%8e%b7%e5%be%97%e9%ab%98%e6%80%a7%e8%83%bd","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=145524","title":{"rendered":"Nat. Commun.\uff1a\u51dd\u80f6\u7535\u89e3\u8d28\u81ea\u4e0b\u800c\u4e0a\u586b\u5145\u65b0\u65b9\u6cd5\u83b7\u5f97\u9ad8\u6027\u80fd\u5168\u56fa\u6001\u67d4\u6027\u8d85\u7ea7\u7535\u5bb9\u5668"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u67d4\u6027\u56fa\u4f53\u8d85\u7ea7\u7535\u5bb9\u5668\uff08FSSCs\uff09\u901a\u5e38\u901a\u8fc7\u5c06\u51dd\u80f6\u7535\u89e3\u8d28\u5939\u5728\u4e00\u5bf9\u591a\u5b54\u7535\u6781\u4e4b\u95f4\u7ec4\u6210\uff0c\u540c\u65f6\u9700\u8981\u51dd\u80f6\u7535\u89e3\u8d28\u4e0e\u591a\u5b54\u7535\u6781\u7684\u5185\u90e8\u5b54\u9699\u5145\u5206\u63a5\u89e6\uff0c\u4ee5\u5f62\u6210\u5145\u653e\u7535\u7684\u754c\u9762\u3002\u73b0\u5728\u5e38\u7528\u7684\u67d4\u6027\u7535\u6781\u90fd\u6bd4\u8f83\u8584\uff0c\u8fd9\u6837\u7535\u89e3\u8d28\u53ef\u4ee5\u4e0e\u7535\u6781\u6750\u6599\u5145\u5206\u63a5\u89e6\uff0c\u4f46\u662f\u5176\u539a\u5ea6\u4ec5\u4e3a\u51e0\u5341\u7eb3\u7c73\u5230\u5fae\u7c73\uff0c\u8fdc\u5c0f\u4e8e\u5546\u7528\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u7535\u6781\u539a\u5ea6\uff08100 \u03bcm \u2013 150 \u03bcm\uff09\uff0c\u5bfc\u81f4\u7535\u5bb9\u5668\u5177\u6709\u4f4e\u7684\u9762\u79ef\u7535\u5bb9\uff0c\u96be\u4ee5\u6ee1\u8db3\u5b9e\u7528\u9700\u6c42\u3002\u867d\u7136\u5236\u4f5c\u5927\u539a\u5ea6\u7684\u591a\u5b54\u7535\u6781\u5e76\u4e0d\u56f0\u96be\uff0c\u4f46\u662f\u4f7f\u51dd\u80f6\u7535\u89e3\u8d28\u5145\u5206\u63a5\u89e6\u5927\u539a\u5ea6\u591a\u5b54\u7535\u6781\u7684\u5185\u90e8\u5b54\u9699\u5374\u662f\u4e00\u9879\u6280\u672f\u6311\u6218\u3002\u672c\u6587\u63d0\u51fa\u4e86\u4e00\u79cd\u65b0\u7684\u56fa\u6001\u51dd\u80f6\u7535\u89e3\u8d28\u586b\u5145\u65b9\u6cd5\uff0c\u4f7f\u56fa\u6001\u51dd\u80f6\u7535\u89e3\u8d28\u7684\u6709\u6548\u586b\u5145\u6df1\u5ea6\u8fbe\u5230\u4e86500 \u03bcm\u4ee5\u4e0a\uff0c\u4f7f\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u5355\u4f4d\u9762\u79ef\u7535\u5bb9\u503c\u4e3a\u4ee5\u5f80\u5b66\u672f\u754c\u62a5\u9053\u7684\u6700\u5927\u503c\u76845\u500d\u4ee5\u4e0a\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u4e2d\u56fd<strong>\u897f\u5b89\u4ea4\u901a\u5927\u5b66<\/strong>\u7684<strong>\u90b5\u91d1\u53cb<\/strong>\u548c\u7f8e\u56fd<strong>\u4f0a\u5229\u8bfa\u4f0a\u5927\u5b66\u5384\u5df4\u7eb3<\/strong><strong>&#8211;<\/strong><strong>\u9999\u69df\u5206\u6821<\/strong>\u7684<strong>Paul V. Braun<\/strong><strong>\uff08\u5171\u540c\u901a\u8baf\uff09<\/strong>\u7b49\u4eba\u62a5\u9053\u4e86\u4e00\u79cd\u56fa\u4f53\u51dd\u80f6\u7535\u89e3\u8d28\u586b\u5145\u65b9\u6cd5\uff0c\u89e3\u51b3\u4e86\u56fa\u6001\u51dd\u80f6\u7535\u89e3\u8d28\u4e0e\u5927\u539a\u5ea6\u591a\u5b54\u7535\u89e3\u7684\u754c\u9762\u63a5\u89e6\u95ee\u9898\u3002\u5982\u679c\u56fa\u6001\u7535\u89e3\u8d28\u4e0d\u5b8c\u5168\u586b\u5145\u591a\u5b54\u7535\u6781\u7684\u5185\u90e8\u5b54\u9699\uff0c\u5c06\u4f1a\u964d\u4f4e\u56fa\u6001\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u7535\u5b66\u6027\u80fd\u548c\u673a\u68b0\u67d4\u6027\uff0c\u4f46\u56fa\u4f53\u51dd\u80f6\u7535\u89e3\u8d28\u5bf9\u5927\u539a\u5ea6\u591a\u5b54\u7535\u6781\u7684\u586b\u5145\u4e00\u76f4\u662f\u4e2a\u96be\u9898\uff0c\u5bfc\u81f4\u5927\u539a\u5ea6\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7684\u56fa\u4f53\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u5236\u9020\u6781\u5177\u6311\u6218\u6027\uff0c\u4e3a\u6b64\uff0c\u7814\u7a76\u4eba\u5458\u62a5\u9053\u4e86\u4e00\u79cd\u201c\u81ea\u4e0b\u800c\u4e0a\u201d\u7684\u586b\u5145\u65b9\u6cd5\u514b\u670d\u4e86\u8fd9\u4e9b\u6311\u6218\u3002\u5229\u7528\u8be5\u65b9\u6cd5\u53ef\u5c06PVA\/H3PO4\u56fa\u6001\u51dd\u80f6\u7535\u89e3\u8d28\u586b\u6ee1\u539a\u5ea6\u8fbe500\u03bcm \u7684MWNCT\u7535\u6781\u4ee5\u53caMWCNT-PEDOT\/PSS\u590d\u5408\u7535\u6781\u3002\u8fd9\u79cd\u7535\u6781\u8868\u73b0\u51fa\u4e86\u4f18\u5f02\u7684\u673a\u68b0\u6027\u80fd\uff1a\u5377\u66f2\u81f30.5mm\u4f7f\u4ecd\u672a\u89c1\u88c2\u7eb9\u4ea7\u751f\uff0c5000\u6b21\u5faa\u73af\u5f2f\u66f2\u540e\u4fdd\u630195%\u7684\u7535\u5bb9\u503c\uff0c\u5176\u4e2d\u57fa\u4e8e500\u03bcm\u539a\u7684WMCNT-PEDOT\/PSS\u7684\u56fa\u6001\u8d85\u7ea7\u7535\u5bb9\u5668\uff0c\u5176\u9762\u7535\u5bb9\u503c\u8fbe\u52302662 mF cm<sup>-2<\/sup>@2 mV s<sup>-1<\/sup>\uff0c\u4e3a\u76ee\u524d\u6700\u5148\u8fdb\u7684\u56fa\u4f53\u8d85\u7ea7\u7535\u5bb9\u5668\u5bb9\u503c\u7ea65\u500d\u3002\u76f8\u5173\u6210\u679c\u4ee5<strong>\u201c<\/strong><strong>High energy flexible supercapacitors formed via bottom-up infilling of gel electrolytes into thick porous electrodes<\/strong>\u201d\u4e3a\u9898\u53d1\u8868\u5728<strong>Nature Communications<\/strong>\u4e0a\uff0c\u8bba\u6587\u7b2c\u4e00\u4f5c\u8005\u4e3a\u897f\u5b89\u4ea4\u901a\u5927\u5b66<strong>\u674e\u7965\u660e<\/strong>\u526f\u6559\u6388\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong> 1 <\/strong><strong>\u81ea\u4e0a\u800c\u4e0b\u548c\u81ea\u4e0b\u800c\u4e0a\u586b\u5145\u793a\u610f\u56fe\u53ca\u5176\u7ed3\u6784\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-145528\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig1_HTML.jpg\" alt=\"\" width=\"600\" height=\"632\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig1_HTML.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig1_HTML-285x300.jpg 285w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u81ea\u4e0a\u800c\u4e0b\u7684\u586b\u5145\u65b9\u6cd5\uff08\u4ece\u5de6\u5230\u53f3\uff1a\u6eb6\u80f6\u6d47\u94f8\u5728\u591a\u5b54\u7535\u6781\u4e0a\uff1b\u591a\u5b54\u7535\u6781\u4e0a\u65b9\u7684\u6eb6\u80f6\u51dd\u80f6\u5f62\u6210\u819c\uff1b\u6eb6\u80f6\u5728\u591a\u5b54\u7535\u6781\u51dd\u80f6\u4e2d\uff0c\u7559\u4e0b\u7a7a\u9699\uff1b\u5728\u4ece\u57fa\u5e95\u5206\u79bb\uff0c\u83b7\u5f97\u72ec\u7acb\u7684\u672a\u5b8c\u5168\u586b\u5145\u7684\u7535\u6781\uff09\uff1b<\/p>\n<p>\uff08b\uff09\u81ea\u4e0b\u800c\u4e0a\u7684\u586b\u5145\u65b9\u6cd5\uff1b\uff08\u4ece\u5de6\u5230\u53f3\uff1a\u6eb6\u80f6\u6d47\u94f8\u5728\u4f4d\u4e8e\u900f\u6c14\u57fa\u6750\u4e0a\u7684\u591a\u5b54\u7535\u6781\u4e0a\uff0c\u5e76\u8986\u76d6\u4e0d\u6e17\u900f\u7684\u8584\u819c\uff1b\u4ece\u5e95\u90e8\u5411\u4e0a\u5f62\u6210\u51dd\u80f6\uff0c\u76f4\u5230\u6574\u4e2a\u591a\u5b54\u7535\u6781\u5145\u6ee1\u51dd\u80f6\uff1b\u9664\u53bb\u57fa\u6750\u540e\u83b7\u5f97\u72ec\u7acb\u7684\u51dd\u80f6\u586b\u5145\u7535\u6781\uff09<\/p>\n<p>\uff08c\uff09\u81ea\u4e0a\u800c\u4e0b\uff08\u5de6\uff09\u548c\u81ea\u4e0b\u800c\u4e0a\uff08\u53f3\uff09\u65b9\u6cd5\u586b\u5145\u51dd\u80f6\u7535\u89e3\u8d28\u7684MWCNT\u7535\u6781\u9876\u90e8\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 2 <\/strong><strong>\u81ea\u4e0a\u800c\u4e0b\u548c\u81ea\u4e0b\u800c\u4e0a\u586b\u5145\u7684<\/strong><strong>FSSC<\/strong><strong>\u7684\u7535\u5316\u5b66\u6027\u80fd\u5bf9\u6bd4<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-145527\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig2_HTML.jpg\" alt=\"\" width=\"600\" height=\"470\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig2_HTML.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig2_HTML-300x235.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09CV\u548c\uff08b\uff09GCD\u7684\u66f2\u7ebf\u5bf9\u6bd4\u56fe\uff1b<\/p>\n<p>\uff08c\uff09\u5728\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u81ea\u4e0a\u800c\u4e0b\u548c\u81ea\u4e0b\u800c\u4e0a\u586b\u5145\u7684FSSC\u7684\u9762\u79ef\u7535\u5bb9\u56fe\uff1b<\/p>\n<p>\uff08d\uff09\u57280.5\u548c5 mA cm<sup>-2<\/sup>\u65f6\uff0c\u81ea\u4e0a\u800c\u4e0b\u548c\u81ea\u4e0b\u800c\u4e0a\u586b\u5145FSSC\u5668\u4ef6\u7684\u9762\u79ef\u7535\u5bb9\u7684\u539a\u5ea6\u4f9d\u8d56\u6027\u5173\u7cfb\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 3 <\/strong><strong>\u51dd\u80f6\u586b\u5145\u65b9\u6cd5\u4e0e\u673a\u68b0\u7a33\u5b9a\u6027\u7684\u63a2\u7a76\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-145526\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig3_HTML.jpg\" alt=\"\" width=\"600\" height=\"345\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig3_HTML.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig3_HTML-300x173.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff0cb\uff09\u57280.5 mm\u534a\u5f84\u7684\u73bb\u7483\u7ba1\u4e0a\u5377\u8d77\u540e\uff0c\u4e24\u79cd\u65b9\u6cd5\u5236\u5907\u7684\u51dd\u80f6\u586b\u5145\u7684\u7ea6150 \u03bcm\u539aMWCNT\u7535\u6781\u7684\u5fae\u88c2\u7eb9\u5b9e\u7269\u56fe\uff1b<\/p>\n<p>\uff08c\uff0cd\uff09\u4e24\u79cd\u5f2f\u66f2FSSC\u5668\u4ef6\u7684\u7535\u5316\u5b66\u6027\u80fd\u56fe\uff1b<\/p>\n<p>\uff08e\uff09\u53cd\u590d\u5f2f\u66f2\u540e\uff0c\u5f2f\u66f2\u6b21\u6570\u4e0e\u7535\u5bb9\u4fdd\u6301\u7387\u7684\u5173\u7cfb\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 4 500 \u03bcm<\/strong><strong>\u539a<\/strong><strong>PEDOT\/PSS-WMCNT<\/strong><strong>\u7535\u6781\u7684<\/strong><strong>FSSC<\/strong><strong>\u6027\u80fd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-145525\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig4_HTML.jpg\" alt=\"\" width=\"600\" height=\"308\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig4_HTML.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/07\/41467_2018_4937_Fig4_HTML-300x154.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09CV\u66f2\u7ebf\u548c\uff08b\uff09GCD\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08c\uff09\u81ea\u4e0a\u800c\u4e0b\u548c\u81ea\u4e0b\u800c\u4e0a\u8bbe\u8ba1\u7684\u963b\u6297\u56fe\uff1b<\/p>\n<p>\uff08d\uff09\u5728\u4e0d\u540c\u7535\u4f4d\u7a97\u53e3\u4e0b\uff0c\u81ea\u4e0b\u800c\u4e0a\u586b\u5145\u7684500 \u03bcm\u539aPEDOT\/PSS- MWCNT\u7535\u6781\u7684FSSC\u7684CV\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08e\uff09\u5728\u4e0d\u540c\u7535\u4f4d\u7a97\u53e3\u4e0b\uff0c\u81ea\u4e0b\u800c\u4e0a\u586b\u5145\u7684500 \u03bcm\u539aPEDOT\/PSS- MWCNT\u7535\u6781\u7684FSSC\u7684GCD\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08f\uff09\u9762\u79efRagone\u56fe\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u6587\u9610\u8ff0\u4e86\u4e00\u79cd\u81ea\u4e0b\u800c\u4e0a\u586b\u5145\u65b9\u6cd5\uff0c\u53ef\u5c06\u56fa\u4f53\u51dd\u80f6\u7535\u89e3\u8d28\u586b\u5165\u5927\u539a\u5ea6\u7684\u591a\u5b54\u7535\u6781\uff0c\u4f7f\u7535\u89e3\u8d28\u79bb\u5b50\u5bf9\u5185\u90e8\u7535\u6781\u8868\u9762\u7684\u53ef\u83b7\u5f97\u6027\u6700\u5927\u5316\u3001\u79bb\u5b50\u6269\u6563\u8def\u5f84\u6700\u5c0f\u5316\uff0c\u4ece\u800c\u6539\u5584\u4e86\u5927\u539a\u5ea6FSSC\u7684\u7535\u5316\u5b66\u6027\u80fd\u3002\u5728\u673a\u68b0\u6027\u80fd\u65b9\u9762\uff0c\u7531\u4e8e\u6240\u586b\u5145\u7684\u56fa\u6001\u51dd\u80f6\u7535\u89e3\u8d28\u4e0e\u591a\u5b54\u7535\u6781\u6750\u6599\u5f62\u6210\u4e86\u673a\u68b0\u4e92\u9501\uff0c\u6240\u4ee5\u63d0\u9ad8\u4e86\u5668\u4ef6\u7684\u673a\u68b0\u7a33\u5b9a\u6027\uff0c\u53ef\u5728\u4e0d\u51cf\u5c0f\u7535\u5bb9\u7684\u60c5\u51b5\u4e0b\u5377\u8d77\u548c\u53cd\u590d\u5f2f\u66f2\u3002\u56e0\u4e3a\u51dd\u80f6\u7535\u89e3\u8d28\u5f62\u6210\u8fc7\u7a0b\u4e2d\u7684\u4f53\u79ef\u6536\u7f29\u51e0\u4e4e\u662f\u666e\u904d\u5b58\u5728\u7684\uff0c\u56e0\u6b64\u6211\u4eec\u76f8\u4fe1\uff0c\u8fd9\u79cd\u81ea\u4e0b\u800c\u4e0a\u7684\u586b\u5145\u7b56\u7565\u53ef\u5e7f\u6cdb\u7528\u4e8e\u4e0d\u540c\u591a\u5b54\u7535\u6781\u7684\u586b\u5145\uff0c\u56e0\u6b64\u53ea\u8981\u80fd\u591f\u5236\u5f97\u5927\u539a\u5ea6\u7684\u591a\u5b54\u7535\u6781\uff0c\u5982\u679c\u4f7f\u7528\u66f4\u4e3a\u5148\u8fdb\u7684\u591a\u5b54\u8d5d\u7535\u5bb9\u7535\u6781\uff0c\u5176\u7535\u5bb9\u503c\u751a\u81f3\u53ef\u80fd\u9ad8\u4e8e\u76ee\u524d\u7684\u6700\u4f73\u503c\uff082662 mF\/cm<sup>2<\/sup>\uff09<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"https:\/\/www.nature.com\/articles\/s41467-018-04937-8\" target=\"_blank\" rel=\"noopener\"><strong>High energy flexible supercapacitors formed via bottom-up infilling of gel electrolytes into thick porous electrodes<\/strong><\/a>\uff08Nat. Commun., 2018, DOI: 10.1038\/s41467-018-04937-8\uff09<\/p>\n<p><strong>\u3010\u56e2\u961f\u4ecb\u7ecd\u3011<\/strong><\/p>\n<p>\u897f\u5b89\u4ea4\u901a\u5927\u5b66<strong>\u90b5\u91d1\u53cb<\/strong>\u6559\u6388\u5fae\u7eb3\u5236\u9020\u7814\u7a76\u56e2\u961f\uff0c\u4f9d\u6258\u4e8e\u897f\u5b89\u4ea4\u901a\u5927\u5b66\u673a\u68b0\u5236\u9020\u7cfb\u7edf\u56fd\u5bb6\u91cd\u70b9\u5b9e\u9a8c\u5ba4\uff0c\u957f\u671f\u81f4\u529b\u4e8e\u5fae\u7eb3\u5236\u9020\u5de5\u827a\u3001\u88c5\u5907\u4e0e\u5668\u4ef6\u65b9\u9762\u7684\u7814\u7a76\u5de5\u4f5c\uff0c\u8bfe\u9898\u7ec4\u5728\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u201c\u7eb3\u7c73\u5236\u9020\u7684\u57fa\u7840\u7814\u7a76\u201d\u91cd\u5927\u7814\u7a76\u8ba1\u5212\u96c6\u6210\u9879\u76ee\u3001\u91cd\u70b9\u7814\u53d1\u4e13\u9879\u9879\u76ee\u7b49\u91cd\u5927\u9879\u76ee\u7684\u652f\u6301\u4e0b\uff0c\u5728\u7535\u9a71\u52a8\u7eb3\u7c73\u538b\u5370\u6280\u672f\u3001\u67d4\u6027\u7535\u5b50\u5236\u9020\u6280\u672f\u3001\u667a\u80fd\u4f20\u611f\u4e0e\u5fae\u7eb3\u4eff\u751f\u5236\u9020\u6280\u672f\u7b49\u65b9\u9762\u5f62\u6210\u4e86\u9c9c\u660e\u7684\u7814\u7a76\u7279\u8272\u3002<\/p>\n<p><strong>\u56e2\u961f\u5728\u8be5\u9886\u57df\u4e2d\u7684\u5de5\u4f5c\u6c47\u603b<\/strong>\uff1a\u8be5\u56e2\u961f\u4ee5\u7eb3\u7c73\u5236\u9020\u6280\u672f\u7684\u7814\u7a76\u4e3a\u57fa\u7840\uff0c\u63a2\u7d22\u7eb3\u7c73\u5236\u9020\u6280\u672f\u5728\u67d4\u6027\u8d85\u7ea7\u7535\u5bb9\u3001\u67d4\u6027\u4f20\u611f\u7535\u5b50\u5668\u4ef6\u3001\u9ad8\u6027\u80fdLED\u82af\u7247\u5236\u9020\u3001\u538b\u7535\/\u6469\u64e6\u80fd\u91cf\u6536\u96c6\u3001\u67d4\u6027\u900f\u660e\u5bfc\u7535\u8584\u819c\u7b49\u9886\u57df\u7684\u5e94\u7528\u3002<\/p>\n<p><strong>\u3010\u76f8\u5173\u4f18\u8d28\u6587\u732e\u63a8\u8350\u3011<\/strong><\/p>\n<p>[1] Chunhui Wang, Jinyou Shao*, Hongmiao Tian, et al, Step-Controllable Electric-Field-Assisted Nanoimprint Lithography for Uneven Large-Area Substrates, ACS Nano, 2016, 10 (4), 4354\u20134363<\/p>\n<p>[2] Xiangming Li, Chuan Xu, Chao Wang, Jinyou Shao* et al. Improved triboelectrification effect by bendable and slidable fish-scale-like microstructures. Nano Energy, 2017, 40, 646-654.<\/p>\n<p>[3] Xiaoliang Chen Xiangming Li Jinyou Shao*, et al.\u00a0 High-Performance Piezoelectric Nanogenerators with Imprinted P(VDF-TrFE)\/BaTiO<sub>3<\/sub> Nanocomposite Micropillars for Self-Powered Flexible Sensors, Small, 2017, 13, 1604245.<\/p>\n<p>[4] Xiaoliang Chen, Jinyou Shao *, Ningli An, et al. Self-powered flexible pressure sensors with vertically well-aligned piezoelectric nanowire arrays for monitoring vital signs. J. Mater. Chem. C, 2015, 3, 11806-11814<\/p>\n<p>[5] Xiaoliang Chen, Hongmiao Tian, Xiangming Li, Jinyou Shao*, et al.\u00a0 A high performance P(VDF-TrFE) nanogenerator with self-connected and vertically integrated fibers by patterned EHD pulling. Nanoscale, 2015, 7, 11536-11544.<\/p>\n<p>[6] Bangbang Nie, Xiangming Li, Jinyou Shao, et al. Flexible and Transparent Strain Sensors with Embedded Multiwalled Carbon Nanotubes Meshes. ACS Appl. Mater. Interfaces, 2017, 9 (46), 40681\u201340689.<\/p>\n<p>[7] Xiangming Li Yucheng Ding Jinyou Shao, et al. Fabrication of Microlens Arrays with Well-controlled Curvature by Liquid Trapping and Electrohydrodynamic Deformation in Microholes. Advanced materials, 2012, 24, OP165-OP169.<\/p>\n<p>[8] Xiangming Li, Hongmiao Tian, Jinyou shao* et al. Decreasing the Saturated Contact Angle in Electrowetting-on-Dielectrics by Controlling the Charge Trapping at Liquid\u2013Solid Interfaces. Advance Functional Materials, 2016, 26, 2994-3002.<\/p>\n<p>[9] Qiang Zhao, Wenjun Wang, Jinyou shao* et al. Nanoscale Electrodes for Flexible Electronics by Swelling Controlled Cracking, Advanced Materials, 2016, 28 (30): 6337-6344<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c<a href=\"mailto:\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\" target=\"_blank\" rel=\"noopener\"><strong>\u6295\u7a3f\u90ae\u7bb1<\/strong><strong>tougao@cailiaoren.com<\/strong><\/a>\u3002<\/p>\n<p>\u6750\u6599\u4eba\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1a<strong>cailiaokefu<\/strong>\u3002<\/p>\n<p>\u6750\u6599\u725b\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c\u70b9\u6211\u52a0\u5165<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\"><strong>\u6750\u6599\u4eba\u7f16\u8f91\u90e8<\/strong><\/a>\u3002<\/p>\n<p><strong>\u6750\u6599\u6d4b\u8bd5\uff0c\u6570\u636e\u5206\u6790\uff0c\u4e0a<\/strong><a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\"><strong>\u6d4b\u8bd5\u8c37<\/strong><\/a><strong>\uff01<\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u67d4\u6027\u56fa\u4f53\u8d85\u7ea7\u7535\u5bb9\u5668\uff08FSSCs\uff09\u901a\u5e38\u901a\u8fc7\u5c06\u51dd\u80f6\u7535\u89e3\u8d28\u5939\u5728\u4e00\u5bf9\u591a\u5b54\u7535\u6781\u4e4b\u95f4\u7ec4\u6210\uff0c\u540c\u65f6\u9700\u8981\u51dd\u80f6\u7535\u89e3\u8d28\u4e0e\u591a\u5b54\u7535\u6781\u7684\u5185\u90e8\u5b54\u9699\u5145\u5206\u63a5\u89e6\uff0c\u4ee5\u5f62\u6210\u5145\u653e\u7535\u7684\u754c\u9762\u3002\u73b0\u5728&#8230;<\/p>\n","protected":false},"author":7035,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[2613,2511,3403,3404],"class_list":["post-145524","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-2613","tag-2511","tag-3403","tag-3404"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/145524"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7035"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=145524"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/145524\/revisions"}],"predecessor-version":[{"id":145593,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/145524\/revisions\/145593"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=145524"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=145524"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=145524"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}