{"id":149726,"date":"2018-08-10T06:19:14","date_gmt":"2018-08-09T22:19:14","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=149726"},"modified":"2018-08-08T23:21:20","modified_gmt":"2018-08-08T15:21:20","slug":"%e5%a4%a7%e8%bf%9e%e7%90%86%e5%b7%a5-%e9%82%b1%e4%bb%8b%e5%b1%b1%e7%8e%8b%e6%b2%bb%e5%ae%87-acs-nano-%e5%9f%ba%e4%ba%8e%e8%81%9a%e5%90%88%e7%9a%843d-mxene%e6%9e%b6%e6%9e%84%e4%bd%9c%e4%b8%ba","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=149726","title":{"rendered":"\u5927\u8fde\u7406\u5de5 \u90b1\u4ecb\u5c71&#038;\u738b\u6cbb\u5b87 ACS Nano: \u57fa\u4e8e\u805a\u5408\u76843D MXene\u67b6\u6784\u4f5c\u4e3a\u5b8c\u5168\u5206\u89e3\u6c34\u7684\u9ad8\u6548\u53cc\u529f\u80fd\u7535\u50ac\u5316\u5242"},"content":{"rendered":"<div><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\u7531\u4e8e\u5177\u6709\u4e0d\u540c\u5bfb\u5e38\u7684\u7ed3\u6784\u548c\u6027\u80fd\uff0cMXene\u6210\u4e3a\u4e86\u4e00\u79cd\u975e\u5e38\u6709\u5438\u5f15\u529b\u7684\u4e8c\u7ef4\uff082D\uff09\u6750\u6599\u3002\u5b83\u4eec\u7684\u901a\u5f0f\u662fM<sub>n+1<\/sub>X<sub>n<\/sub>T<sub>x<\/sub>\uff08n = 1-3\uff09\uff0c\u5176\u4e2dM\u662f\u8fc7\u6e21\u91d1\u5c5e\uff08\u4f8b\u5982Ti\u3001V\u3001Nb\u3001Mo\u7b49\uff09\uff0cX\u662fC\u6216N\u5143\u7d20\uff0c\u800cT\u4ee3\u8868\u5316\u5b66\u57fa\u56e2\uff0c\u4f8b\u5982-OH\u3001-O\u3001-Cl\u548c-F\u3002\u5177\u6709\u5e7f\u6cdb\u7684\u5316\u5b66\u548c\u7ed3\u6784\u53d8\u5316\u6027\u80fd\u4f7f\u5f97\u5b83\u4eec\u6709\u826f\u597d\u7684\u5438\u5f15\u529b\u6027\u80fd\uff0c\u4f8b\u5982\u4e0e\u8d39\u7c73\u80fd\u7ea7\u9644\u8fd1\u7684\u9ad8\u7535\u5b50\u6001\u5bc6\u5ea6\u76f8\u5173\u7684\u9ad8\u5bfc\u7535\u6027\u3001\u4f18\u5f02\u7684\u4eb2\u6c34\u6027\u3001\u826f\u597d\u7684\u673a\u68b0\u7a33\u5b9a\u6027\u4ee5\u53ca\u901a\u8fc7\u63a5\u679d\u5316\u5b66\u57fa\u56e2\u4ee5\u5b9e\u73b0\u4e30\u5bcc\u7684\u8868\u9762\u5316\u5b66\u3002\u6700\u8fd1\u62a5\u9053\u7684Ti<sub>3<\/sub>C<sub>2<\/sub>\u548cNb<sub>2<\/sub>C MXenes\u7528\u4e8e\u4f53\u5185\u5149\u70ed\u7597\u6cd5\u8868\u73b0\u51fa\u826f\u597d\u7684\u751f\u7269\u76f8\u5bb9\u6027\u548c\u8fd1\u7ea2\u5916\u5438\u9644\u3002\u8fd9\u4e9b\u4f18\u70b9\u4f7f\u5f97MXene\u5728\u8bf8\u5982\u50a8\u80fd\u3001\u50ac\u5316\u3001\u900f\u660e\u7535\u5b50\u5668\u4ef6\u3001\u5206\u79bb\u819c\u3001\u4f20\u611f\u5668\u3001\u590d\u5408\u6750\u6599\u589e\u5f3a\u3001\u7535\u78c1\u5c4f\u853d\u548c\u751f\u7269\u533b\u5b66\u7b49\u5e7f\u6cdb\u9886\u57df\u4e2d\u975e\u5e38\u6709\u524d\u666f\u3002\u7136\u800c\uff0c\u901a\u8fc7\u8303\u5fb7\u534e\u529b\u7684\u7247\u72b6\u805a\u96c6\u9650\u5236\u4e86\u57fa\u4e8eMXene\u7684\u6750\u6599\/\u5668\u4ef6\u7684\u529f\u80fd\u6027\u3001\u53ef\u52a0\u5de5\u6027\u3002<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\u8fd1\u65e5\uff0c<strong>\u5927\u8fde\u7406\u5de5\u5927\u5b66\u7684\u90b1\u4ecb\u5c71\u6559\u6388\u548c\u738b\u6cbb\u5b87\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u7b49\u62a5\u9053\u4e86\u5229\u7528\u6bdb\u7ec6\u5f3a\u538b\u7ec4\u88c5\u7b56\u7565\u52a0\u5de5MXene\u4e3a\u5177\u6709\u51e0\u4f55\u5f62\u72b6\u7684\u9ad8\u6297\u805a\u96c6\u6027\u7684\u5206\u5c423D\u7ed3\u6784\u30023D MXene\u7684\u6297\u805a\u96c6\u6027\u80fd\u4e0d\u4ec5\u4f7f\u8868\u9762\u79ef\u52a0\u500d\uff0c\u800c\u4e14\u4e0d\u635f\u574fMXene\u7684\u56fa\u6709\u6027\u80fd\uff0c\u4f8b\u5982\u826f\u597d\u7684\u52a8\u529b\u5b66\u6846\u67b6\u3001\u9ad8\u7a33\u5b9a\u6027\u548c\u6eb6\u6db2-\u56fa\u6001\u7684\u4f18\u5f02\u52a0\u5de5\u6027\u7b49\u30023D MXene\u4e0e\u7535\u5316\u5b66\u6d3b\u6027\u7269\u8d28\u76f8\u534f\u540c\u8026\u5408\uff0c\u4f7f\u5f97\u6df7\u5408\u7269\u7cfb\u7edf\u5177\u6709\u975e\u5e38\u9ad8\u7684\u6d3b\u6027\u8868\u9762\u79ef\u3001\u7535\u8377\u8f6c\u79fb\u52a8\u529b\u5b66\u548c\u8d28\u91cf\u6269\u6563\u901f\u7387\u3002\u7279\u522b\u662fCoP-3D MXene\u6742\u5316\u7269\u5bf9\u78b1\u6027\u7535\u89e3\u8d28\u4e2d\u6c27\u548c\u6c22\u7684\u91ca\u653e\u8868\u73b0\u51fa\u9ad8\u7535\u50ac\u5316\u6d3b\u6027\u3002\u4f5c\u4e3a\u4e00\u79cd\u53cc\u529f\u80fd\u7535\u50ac\u5316\u5242\uff0c\u5b83\u4eec\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u7535\u6c60\u7535\u538b\u548c\u8010\u4e45\u6027\uff0c\u7ed3\u5408RuO<sub>2<\/sub>\/Pt\u50ac\u5316\u5242\u7528\u4e8e\u78b1\u6027\u6eb6\u6db2\u4e2d\u4f7f\u6c34\u5b8c\u5168\u5206\u89e3\uff0c\u7a81\u51fa\u4e86\u9ad8\u6297\u805a\u96c6\u60273D MXene\u4f5c\u4e3a\u4e00\u79cd\u9ad8\u6027\u80fd\u7535\u50ac\u5316\u5242\u7684\u5de8\u5927\u5e94\u7528\u6f5c\u529b\u3002\u7814\u7a76\u6210\u679c\u4ee5\u9898\u4e3a<strong>\u201cAggregation-Resistant 3D MXene-Based Architecture as Efficient Bifunctional Electrocatalyst for Overall Water Splitting\u201d<\/strong>\u53d1\u8868\u5728\u56fd\u9645\u8457\u540d\u671f\u520a<strong>ACS Nano<\/strong>\u4e0a\u3002<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/div>\n<div>\u00a0<\/div>\n<div><strong>\u56fe\u4e00\u30013D Mxene\u7684\u5236\u5907\u8fc7\u7a0b\u548c\u7ed3\u6784\u793a\u610f\u56fe<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-149727\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/1-22.jpg\" alt=\"\" width=\"600\" height=\"404\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/1-22.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/1-22-300x202.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\uff08a\uff09 \u6297\u805a\u96c63D MXene\u7ed3\u6784\u7684\u91cd\u8981\u4f18\u70b9\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08b\uff09 \u55b7\u96fe\u5e72\u71e5\u542bMXene\u80f6\u4f53\u7684\u6c14\u6eb6\u80f6\u6db2\u6ef4\uff0c\u5c06MXene\u6bdb\u7ec6\u72b6\u5f3a\u538b\u7ec4\u88c5\u62103D\u7ed3\u6784\u3002<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u56fe\u4e8c\u30013D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684\u7406\u5316\u8868\u5f81<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-149728\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/2-23.jpg\" alt=\"\" width=\"600\" height=\"602\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/2-23.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/2-23-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/2-23-300x300.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\uff08a\u3001b\uff093D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u56fe\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08c\uff093D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684TEM\u56fe\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08d\uff093D MXene \u7684TEM\u56fe\u663e\u793a\u57283D\u7ed3\u6784\u4e2d\u7684\u6291\u5236\u805a\u96c6\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08e\u3001f\uff09\u7403\u5f62\u72b63D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u56fe\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08g\uff09\u7403\u5f62\u72b63D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684TEM\u56fe\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08h\uff093D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684\u5c3a\u5bf8\u53d8\u5316\u3002<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u56fe\u4e09\u30013D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u548cTi<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684\u7406\u5316\u8868\u5f81<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-149729\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/3-21.jpg\" alt=\"\" width=\"600\" height=\"459\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/3-21.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/3-21-300x230.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\u00a0<\/div>\n<div>\uff08a\uff09 3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u548cTi<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684XRD\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08b\uff09 3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u548cTi<sub>3<\/sub>C<sub>2<\/sub> MXene\u4e2dTi <sub>2<\/sub>P\u7684XPS\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08c\uff09 3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u548cTi<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684FT-IR\u8c31\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08d\uff0920 MPa\u6052\u5b9a\u538b\u529b\u4e0b\uff0c3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7ed3\u6784\u548c\u539f\u59cbTi<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684\u5bfc\u7535\u6027\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08e\uff093D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u9897\u7c92\uff08\u9876\u90e8\uff09\u624b\u6447\u52a8\u5206\u6563\u5728\u591a\u79cd\u6eb6\u5242\u4e2d\u5e76\u4fdd\u6301\u7a33\u5b9a4\u5c0f\u65f6\uff0c\u800c\u539f\u59cbTi<sub>3<\/sub>C<sub>2 <\/sub>MXene\u8d85\u58f0\u6ce2\u5904\u7406\u540e\u5728\u5927\u591a\u6570\u6eb6\u5242\u4e2d\u5feb\u901f\u805a\u96c6\uff08\u5e95\u90e8\uff09\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08f\uff09 3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7ed3\u6784\u3001\u539f\u59cbTi<sub>3<\/sub>C<sub>2<\/sub> MXene\u548c\u771f\u7a7a\u8fc7\u6ee4Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u8584\u819c\u7684N<sub>2<\/sub>\u5438\u9644\/\u89e3\u5438\u7b49\u6e29\u7ebf\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08g\u3001h\uff09 150 MPa\u4e0b\uff0c3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7ed3\u6784\u548c\u539f\u59cbTi<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u56fe\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08i\uff09\u771f\u7a7a\u8fc7\u6ee4Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u8584\u819c\u7684SEM\u56fe\u3002<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u56fe\u56db\u30013D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7ed3\u5408\u4e0d\u540c\u5143\u7d20\u6216\u6c27\u5316\u7269\u7684\u7406\u5316\u8868\u5f81<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-149730\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/4-22.jpg\" alt=\"\" width=\"600\" height=\"354\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/4-22.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/4-22-300x177.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\uff08a\u3001b\uff09Co<sub>3<\/sub>O<sub>4<\/sub>@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u3001TEM\u3001\u5143\u7d20\u5206\u6790\u548cXRD\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08c\u3001d\uff09SnO<sub>2<\/sub>@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u3001TEM\u3001\u5143\u7d20\u5206\u6790\u548cXRD\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08e\u3001f\uff09MnTiO<sub>3<\/sub>@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u3001TEM\u3001\u5143\u7d20\u5206\u6790\u548cXRD\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08g\u3001h\uff09Pt@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u3001TEM\u3001\u5143\u7d20\u5206\u6790\u548cXRD\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08i\u3001j\uff09Ag@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u3001TEM\u3001\u5143\u7d20\u5206\u6790\u548cXRD\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08k\u3001l\uff09S@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\u3001TEM\u3001\u5143\u7d20\u5206\u6790\u548cXRD\u3002<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u56fe\u4e94\u3001CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684\u7406\u5316\u8868\u5f81<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-149731\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/5-17.jpg\" alt=\"\" width=\"600\" height=\"519\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/5-17.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/5-17-300x260.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\uff08a\u3001b\uff09CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684SEM\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08c\u3001d\uff09CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684TEM\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08e\uff09TEM\u56fe\u663e\u793a\u8d85\u7ec6CoP\u7eb3\u7c73\u7c92\u5b50\u57283D MXene\u8868\u9762\u7684\u5747\u5300\u5206\u6563\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08f\uff09CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684HRTEM\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08g\uff09CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u4e2dC\u3001Co\u3001Ti\u548c P\u7684\u5143\u7d20\u5206\u6790\u3002<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u56fe\u516d\u3001CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684\u7535\u5316\u5b66\u6027\u80fd\u548c\u50ac\u5316\u6548\u679c<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-149732\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/6-10.jpg\" alt=\"\" width=\"600\" height=\"647\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/6-10.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/6-10-278x300.jpg 278w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\uff08a\uff09 \u4e0d\u540cCoP\u542b\u91cf\u3001\u4e0d\u542bMXene\u7684CoP\u548c3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u7684CoP @ 3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u50ac\u5316\u5242\u7684iR\u6821\u6b63LSV\u66f2\u7ebf\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08b\uff09 \u7528\u4e8eOER\u7684CoP@3D Ti3C2 MXene\u3001CoP @ Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u3001CoP @3D rGO\u3001CoP\u30013D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u548cRuO2\u50ac\u5316\u5242\u7684iR\u6821\u6b63LSV\u66f2\u7ebf\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08c\uff09 \u50ac\u5316\u5242\u5728\u8d77\u59cb\u8fc7\u7535\u4f4d\u548c\u03b7<sub>j<\/sub>= 10\u7684\u6bd4\u8f83\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08d\uff09 \u7535\u6d41\u5bc6\u5ea6\u4e3a10.0 mA\/cm<sup>-2<\/sup>\u7684CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u3001CoP@Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u3001CoP@3D rGO\u3001CoP\u548cRuO<sub>2<\/sub>\u50ac\u5316\u5242\u7684Tafel\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08e\uff09 \u7535\u6d41\u5bc6\u5ea6\u4e3a10.0 mA\/cm<sup>-2<\/sup>\u7684CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u3001CoP@Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u3001CoP@3D rGO\u3001CoP\u548cRuO<sub>2<\/sub>\u50ac\u5316\u5242\u7684\u8ba1\u65f6\u7535\u4f4d\u54cd\u5e94\uff1b<\/div>\n<div>\u00a0<\/div>\n<div>\uff08f\uff09 CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u3001CoP@Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u3001CoP@3D rGO\u3001MXene free CoP\u548cRuO<sub>2<\/sub>\u50ac\u5316\u5242\u7684\u50ac\u5316\u6d3b\u6027\u548c\u7a33\u5b9a\u6027\u7684\u7efc\u5408\u56fe\u3002<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\u7814\u7a76\u62a5\u9053\u4e86\u901a\u8fc7\u5c06MXene\u7ec4\u88c5\u6210\u5177\u6709\u5206\u5c42\u7ed3\u6784\u548c\u805a\u96c6\u6297\u6027\u76843D\u7ed3\u6784\u6765\u6709\u6548\u5730\u51cf\u8f7b\u5176\u7eb3\u7c73\u7247\u7684\u805a\u5408\u30023D MXene\u7ed3\u6784\u7684\u62d3\u6251\u7ed3\u6784\u4e0d\u4ec5\u53ef\u4ee5\u9632\u6b62\u7eb3\u7c73\u7247\u4e4b\u95f4\u7684\u805a\u96c6\uff0c\u800c\u4e14\u4e5f\u53ef\u4ee5\u5728\u56fa\u6001\u548c\u5177\u6709\u4e0d\u540c\u7279\u6027\u7684\u6eb6\u5242\u4e2d\u5b9e\u73b0\u51e0\u4f55\u5f62\u72b6\u7684\u805a\u96c6\u963b\u529b\u3002\u6b64\u5916\uff0c3D MXene\u7ed3\u6784\u8fd8\u5177\u6709\u5927\u7684\u8868\u9762\u79ef\u3001\u9ad8\u575a\u56fa\u6027\u30013D\u5bfc\u7535\u6846\u67b6\u4ee5\u53ca\u76f8\u5bf9\u4e8e\u6241\u5e73MXene\u677f\u6750\u66f4\u597d\u7684\u53ef\u52a0\u5de5\u6027\u3002\u901a\u8fc7\u4e0e\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269\u548c\u4e3b\u65cf\u91d1\u5c5e\u6c27\u5316\u7269\u3001\u9499\u949b\u77ff\u578b\u91d1\u5c5e\u6c27\u5316\u7269\u3001\u91d1\u5c5e\u78f7\u5316\u7269\u3001\u8d35\u91d1\u5c5e\u548c\u786b\u7b49\u7684\u7eb3\u7c73\u7ed3\u6784\u76f8\u7ed3\u5408\uff0c\u4f7f\u5b83\u4eec\u6210\u4e3a\u5177\u6709\u5e7f\u6cdb\u529f\u80fd\u7684\u5de5\u7a0b\u5206\u7ea7\u6df7\u5408\u7cfb\u7edf\u7684\u901a\u7528\u4e3b\u4f53\u3002CoP@3D Ti<sub>3<\/sub>C<sub>2<\/sub> MXene\u50ac\u5316\u5242\u7684\u53cc\u529f\u80fd\u7535\u50ac\u5316\u6d3b\u6027\u4f7f\u5b83\u4eec\u53ef\u4ee5\u5b8c\u5168\u7684\u5206\u89e3\u6c34\uff0c\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u6d3b\u6027\u548c\u5bf9\u8d35\u91d1\u5c5ePt\u548cRuO<sub>2<\/sub>\u50ac\u5316\u5242\u7684\u7ec4\u5408\u7684\u8010\u4e45\u6027\u3002\u6b64\u9879\u7814\u7a76\u4e0d\u4ec5\u8868\u660e\u57fa\u4e8e3D MXene\u7684\u7535\u50ac\u5316\u5242\u80fd\u591f\u5b9e\u73b0\u826f\u597d\u7684\u7535\u5316\u5b66\u7279\u6027\uff0c\u800c\u4e14\u8fd8\u662f\u89e3\u51b3MXene\u7cfb\u5217\u52a0\u5de5\u548c\u5e94\u7528\u4e2d\u7684\u57fa\u672c\u96be\u9898\u7684\u6709\u6548\u65b9\u6cd5\u3002<\/div>\n<div>\u00a0<\/div>\n<div>\u6587\u732e\u94fe\u63a5\uff1a<strong><a href=\"https:\/\/pubs.acs.org\/doi\/10.1021\/acsnano.8b02849\" target=\"_blank\" rel=\"noopener\">Aggregation-Resistant 3D MXene-Based Architecture as Efficient Bifunctional Electrocatalyst for Overall Water Splitting<\/a><\/strong>\uff08ACS Nano, <strong>2018<\/strong>, DOI: 10.1021\/acsnano.8b02849\uff09<\/div>\n<div>\u00a0<\/div>\n<div><strong>\u672c\u6587\u7531\u6750\u6599\u4eba\u751f\u7269\u6750\u6599\u7ec4\u5c0f\u80d6\u7eb8\u7f16\u8bd1\u3002<\/strong><\/div>\n<div>\u00a0<\/div>\n<div>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com.<\/div>\n<div>\u00a0<\/div>\n<div>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaokefu.<\/div>\n<div>\u00a0<\/div>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u00a0 \u7531\u4e8e\u5177\u6709\u4e0d\u540c\u5bfb\u5e38\u7684\u7ed3\u6784\u548c\u6027\u80fd\uff0cMXene\u6210\u4e3a\u4e86\u4e00\u79cd\u975e\u5e38\u6709\u5438\u5f15\u529b\u7684\u4e8c\u7ef4\uff082D\uff09\u6750\u6599\u3002\u5b83\u4eec\u7684\u901a\u5f0f\u662fMn+1XnTx\uff08n = 1-3\uff09\uff0c\u5176\u4e2dM\u662f\u8fc7\u6e21\u91d1\u5c5e&#8230;<\/p>\n","protected":false},"author":7770,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[3500,3501],"class_list":["post-149726","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-3d-mxene","tag-cop3d-ti3c2-mxenen"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/149726"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7770"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=149726"}],"version-history":[{"count":7,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/149726\/revisions"}],"predecessor-version":[{"id":150061,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/149726\/revisions\/150061"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=149726"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=149726"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=149726"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}