{"id":150910,"date":"2018-08-21T06:30:12","date_gmt":"2018-08-20T22:30:12","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=150910"},"modified":"2018-08-19T21:19:30","modified_gmt":"2018-08-19T13:19:30","slug":"%e5%a4%a7%e8%bf%9e%e7%90%86%e5%b7%a5%e8%91%a3%e5%ba%94%e8%b6%85nano-lett-%ef%bc%9a%e7%a8%b3%e5%ae%9a%e7%9a%84%e8%b6%85%e7%96%8f%e6%b0%b4%e9%99%b6%e7%93%b7%e5%9f%ba%e7%a2%b3%e7%ba%b3%e7%b1%b3%e7%ae%a1","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=150910","title":{"rendered":"\u5927\u8fde\u7406\u5de5\u8463\u5e94\u8d85Nano Lett.\uff1a\u7a33\u5b9a\u7684\u8d85\u758f\u6c34\u9676\u74f7\u57fa\u78b3\u7eb3\u7c73\u7ba1\u590d\u5408\u8131\u76d0\u819c"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u6d77\u6c34\u6de1\u5316\u6b63\u6210\u4e3a\u7f13\u89e3\u6de1\u6c34\u8d44\u6e90\u5371\u673a\u7684\u4e00\u79cd\u5e7f\u6cdb\u5e94\u7528\u7684\u65b9\u6cd5\u3002\u7136\u800c\uff0c\u901a\u8fc7\u53cd\u6e17\u900f\u819c(RO)\u5de5\u827a\u8fdb\u884c\u5927\u89c4\u6a21\u6d77\u6c34\u6de1\u5316\u4f1a\u4ea7\u751f\u5927\u91cf\u9ad8\u76d0\u5ea6\u7684\u5e9f\u6c34\uff0c\u82e5\u76f4\u63a5\u6392\u6d77\u4f1a\u5bf9\u6d77\u6d0b\u73af\u5883\u9020\u6210\u4e25\u91cd\u7684\u7834\u574f\u3002\u6d77\u6c34\u6d53\u7f29\u6c34\u548c\u5de5\u4e1a\u9ad8\u76d0\u5e9f\u6c34\u96f6\u6392\u653e\u662f\u89e3\u51b3\u6c34\u6c61\u67d3\u548c\u6c34\u8d44\u6e90\u5371\u673a\uff0c\u5b9e\u73b0\u8d44\u6e90\u56de\u6536\u7684\u91cd\u8981\u9014\u5f84\uff0c\u662f\u4e9f\u5f85\u89e3\u51b3\u7684\u91cd\u8981\u73af\u5883\u95ee\u9898\u3002\u819c\u84b8\u998f\u6cd5 (MD)\u662f\u4e00\u79cd\u5f88\u6709\u524d\u9014\u7684\u9ad8\u76d0\u5e9f\u6c34\u5904\u7406\u5de5\u827a\uff0c\u5982\u679c\u80fd\u591f\u5145\u5206\u5229\u7528\u5de5\u4e1a\u4f59\u70ed\u6216\u5e9f\u70ed\u7b49\u4f4e\u54c1\u4f4d\u70ed\u6e90\uff0c\u819c\u84b8\u998f\uff08MD\uff09\u5c06\u6781\u5177\u7ade\u4e89\u529b\u3002MD\u7684\u5173\u952e\u7ec4\u6210\u662f\u4e00\u79cd\u7a33\u5b9a\u7684\u591a\u5b54\u758f\u6c34\u819c\uff0c\u5177\u6709\u5927\u7684\u6db2-\u6c14\u754c\u9762\uff0c\u53ef\u6709\u6548\u5730\u8f93\u9001\u6c34\u84b8\u6c14\uff0c\u5177\u6709\u70ed\u7a33\u5b9a\u6027\u548c\u758f\u6c34\u7a33\u5b9a\u6027\u3001\u6297\u6d78\u6da6\u6027\u548c\u6297\u819c\u6c61\u67d3\u6027\u3002\u7136\u800c\uff0c\u76ee\u524d\u805a\u5408\u7269\u6216\u758f\u6c34\u6539\u6027\u65e0\u673a\u819c\u7684\u4e00\u4e2a\u5173\u952e\u6311\u6218\u662f\u64cd\u4f5c\u7a33\u5b9a\u6027\u4e0d\u8db3\uff0c\u5bfc\u81f4\u4e00\u4e9b\u95ee\u9898\uff0c\u5982\u819c\u6d78\u6da6\u3001\u819c\u6c61\u67d3\u3001\u901a\u91cf\u548c\u8131\u76d0\u7387\u7684\u4e0b\u964d\u3002\u78b3\u7eb3\u7c73\u7ba1(CNTs)\u5177\u6709\u4f18\u5f02\u7684\u7269\u7406\u5316\u5b66\u6027\u80fd\uff0c\u5982\u9ad8\u758f\u6c34\u6027\u3001\u5927\u6bd4\u8868\u9762\u79ef\u3001\u826f\u597d\u7684\u70ed\u7a33\u5b9a\u6027\u3001\u673a\u68b0\u5316\u5b66\u7a33\u5b9a\u6027\u548c\u826f\u597d\u7684\u5bfc\u7535\u6027\u7b49\u3002\u56e0\u6b64\uff0cCNT\u53ef\u7528\u4f5c\u6539\u6027\u5242\u4ee5\u6539\u5584\u5305\u62ecMD\u5728\u5185\u7684\u5206\u79bb\u5e94\u7528\uff0c\u4f46\u4e3b\u8981\u7528\u4e8e\u805a\u5408\u7269\u819c\u3002\u56fd\u9645\u4e0a\uff0c\u5982\u4f55\u5f00\u53d1\u65b0\u578b\u819c\u6750\u6599\uff0c\u540c\u65f6\u63d0\u9ad8\u64cd\u4f5c\u7a33\u5b9a\u6027\u548c\u819c\u6027\u80fd\uff0c\u662f\u79d1\u5b66\u5bb6\u4eec\u91cd\u70b9\u7814\u7a76\u7684\u6311\u6218\u6027\u5de5\u7a0b\u79d1\u5b66\u95ee\u9898\u4e4b\u4e00\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u5728<strong><b>\u5927\u8fde\u7406\u5de5\u5927\u5b66\u73af\u5883\u5b66\u9662\u73af\u5883\u6c61\u67d3\u63a7\u5236\u5de5\u7a0b\u7814\u7a76\u5ba4\u8463\u5e94\u8d85\u6559\u6388<\/b><\/strong><strong><b>\uff08\u901a\u8baf\u4f5c\u8005\uff09<\/b><\/strong>\u548c<strong><b>\u5408\u4f5c\u8005<\/b><\/strong><strong><b>Michael D. Guiver\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u7b49<\/b><\/strong>\u56e2\u961f\u5e26\u9886\u4e0b\uff0c\u4e0e<strong><b>\u9999\u6e2f\u5927\u5b66<\/b><\/strong><strong><b>\uff08\u6c64\u521d\u9633\u6559\u6388\uff0c\u5927\u8fde\u7406\u5de5\u5927\u5b66\u6d77\u5929\u5b66\u8005\uff09\u3001\u7f8e\u56fd\u548c\u7231\u5c14\u5170\u7684\u7814\u7a76\u5355\u4f4d<\/b><\/strong>\u5408\u4f5c\uff0c\u9488\u5bf9\u96be\u70b9\u95ee\u9898\uff0c\u521b\u65b0\u5730\u63d0\u51fa\u4e86\u4e00\u79cd\u8d85\u758f\u6c34\u9676\u74f7\u57fa\u78b3\u7eb3\u7c73\u7ba1(CNT)\u8131\u76d0\u819c\u7684\u603b\u4f53\u6982\u5ff5\u8bbe\u8ba1\u548c\u5e94\u7528\u7b56\u7565\uff0c\u8be5\u819c\u5177\u6709\u7279\u6b8a\u8bbe\u8ba1\u7684\u819c\u7ed3\u6784\uff0c\u5145\u5206\u5229\u7528\u78b3\u7eb3\u7c73\u7ba1\u7684\u758f\u6c34\u6027\u3001\u8010\u70ed\u7a33\u5b9a\u6027\u548c\u5bfc\u7535\u6027\uff0c\u5177\u6709\u524d\u6240\u672a\u6709\u7684\u8fd0\u884c\u7a33\u5b9a\u6027\u548c\u8d85\u758f\u6c34\u6027\u80fd\uff0c\u5176\u4e2d\u4e92\u8fde\u7684CNT\u7f51\u7edc\u662f\u901a\u8fc7\u5316\u5b66\u6c14\u76f8\u6dc0\u79ef\uff08CVD\uff09\u76f4\u63a5\u5728\u9676\u74f7\u8f7d\u4f53\u7684\u8868\u9762\u548c\u957f\u901a\u9053\u6307\u72b6\u5927\u5b54\u5185\u539f\u4f4d\u5f62\u6210\u3002\u901a\u8fc7\u5bf9\u539f\u4f4d\u751f\u957f\u7684CNT\u8fdb\u884c\u5b9a\u91cf\u8c03\u63a7\uff0c\u6784\u7b51\u4e86\u5177\u6709CNT\u7f51\u7edc\u7684\u8d85\u591a\u5b54\u8d85\u758f\u6c34\u8868\u9762\u7ed3\u6784\u3002\u5728\u52a0\u901f\u7a33\u5b9a\u6027\u8bd5\u9a8c\u4e0b\uff0c\u5b8c\u5168\u8986\u76d6\u7684CNT\u5c42(FC-CNT\u819c)\u5728\u70ed\u7a33\u5b9a\u6027\u548c\u8d85\u758f\u6c34\u7a33\u5b9a\u6027\u65b9\u9762\u8868\u73b0\u51fa\u663e\u8457\u7684\u6539\u5584\u3002\u7531\u4e8e\u8d85\u591a\u5b54\u8868\u9762\u7f51\u7edc\u7684\u72ec\u7279\u7ed3\u6784\uff0c\u63d0\u4f9b\u5927\u7684\u6db2-\u6c14\u8d85\u758f\u6c34\u754c\u9762\u548c\u5185\u90e8\u6307\u72b6\u5927\u5b54\uff0cFC-CNT\u819c\u8868\u73b0\u51fa\u7a33\u5b9a\u7684\u9ad8\u901a\u91cf\uff0cNa<sup>+<\/sup>\u7684\u53bb\u9664\u7387\u4e3a99.9\uff05\uff0c\u4f18\u4e8e\u73b0\u6709\u7684\u65e0\u673a\u819c\u4f53\u7cfb\u3002\u5728\u7b80\u5355\u3001\u65e0\u635f\u7535\u5316\u5b66\u8f85\u52a9\u76f4\u63a5\u63a5\u89e6\u819c\u84b8\u998f(e-DCMD)\u4e0b\uff0c\u53ef\u4ee5\u89c2\u5bdf\u5230\u63d0\u9ad8\u7684\u6297\u819c\u6c61\u67d3\u6027\u80fd\u3002\u8be5\u5de5\u4f5c\u4e2d\u819c\u7ed3\u6784\u4e0e\u5e94\u7528\u7684\u8bbe\u8ba1\u7b56\u7565\u5177\u6709\u666e\u9002\u6027\uff0c\u819c\u5236\u5907\u4e5f\u53ef\u9002\u7528\u4e8e\u5176\u4ed6\u9676\u74f7\u6216\u65e0\u673a\u8f7d\u4f53\u4f53\u7cfb\uff0c\u901a\u8fc7\u5b9a\u91cf\u8c03\u63a7\u590d\u5408\u819c\u7684\u7535\u8d1f\u6027\uff0c\u9884\u671f\u4e5f\u53ef\u5b9e\u73b0\u51cf\u7f13\u4e0d\u540c\u8377\u7535\u7279\u6027\u7269\u8d28\u7684\u819c\u6c61\u67d3\uff0c\u819c\u5e94\u7528\u4e5f\u4e0d\u5c40\u9650\u4e8e\u6d77\u6c34\u6de1\u5316\u548c\u9ad8\u76d0\u5e9f\u6c34\u5904\u7406\uff0c\u9884\u671f\u4e5f\u9002\u7528\u4e8e\u542b\u6709\u975e\u6325\u53d1\u6027\u6eb6\u8d28\u5e9f\u6c34\u5982\u91cd\u91d1\u5c5e\u3001\u5927\u5206\u5b50\u548c\u80f6\u4f53\u7b49\u5404\u7c7b\u5e9f\u6c34\u4f53\u7cfb\uff0c\u4e43\u81f3\u6c14\u4f53\u51c0\u5316\u7b49\u9886\u57df\u3002\u76f8\u5173\u6210\u679c\u4ee5\u9898\u4e3a\u201c<strong><b>Stable Superhydrophobic Ceramic-based Carbon Nanotube Composite Desalination Membranes<\/b><\/strong>\u201d\u53d1\u8868\u5728\u56fd\u9645\u9876\u7ea7\u671f\u520a<strong><b>Nano Lett.<\/b><\/strong>\u4e0a\uff082018\uff09\uff08DOI: 10.1021\/acs.nanolett.8b01907\uff09\u3002\u5927\u8fde\u7406\u5de5\u5927\u5b66\u4e3a\u7b2c\u4e00\u4f5c\u8005\u5355\u4f4d\u548c\u7b2c\u4e00\u901a\u8baf\u5355\u4f4d\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe1.<\/b><\/strong><strong><b>\u00a0\u9676\u74f7\u57faCNT\u819c\u7684\u5236\u9020\u548cDCMD\u5de5\u827a<\/b><\/strong><strong><b>\u6d41\u7a0b\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-150913\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/1-33.jpg\" alt=\"\" width=\"600\" height=\"462\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/1-33.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/1-33-300x231.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u00a0<\/b><\/strong><strong><b>\u56fe2.<\/b><\/strong><strong><b>\u00a0PC-CNT\u819c\u548cFC-CNT\u819c\u7684\u5f62\u8c8c\u8868\u5f81<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-150914\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/2-34.jpg\" alt=\"\" width=\"600\" height=\"622\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/2-34.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/2-34-289x300.jpg 289w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5c16\u6676\u77f3\u57fa\u9676\u74f7\u57fa\u6750\uff081\uff09\u8868\u9762SEM\u56fe\u50cf\uff0c\uff082\uff09\u6a2a\u622a\u9762SEM\u56fe\u50cf\uff0c\uff083\uff09\u7b80\u5316\u7684\u7ed3\u6784\u6a21\u578b\uff08\u9ed1\u8272\uff1aCNT\uff1b\u6d45\u7eff\u8272\uff1a\u5c16\u6676\u77f3\u57fa\u5e95\uff09\u548c\uff084\uff09\u5728\u5ba4\u6e29\uff08~25\u2103\uff09\u4e0b\u6d4b\u91cf\u6c34\u5728\u819c\u8868\u9762\u4e0a\u7684\u63a5\u89e6\u89d2\uff1b<\/p>\n<p>\uff08b\uff09PC-CNT\u819c\uff081\uff09\u8868\u9762SEM\u56fe\u50cf\uff0c\uff082\uff09\u6a2a\u622a\u9762SEM\u56fe\u50cf\uff0c\uff083\uff09\u7b80\u5316\u7684\u7ed3\u6784\u6a21\u578b\uff08\u9ed1\u8272\uff1aCNT\uff1b\u6d45\u7eff\u8272\uff1a\u5c16\u6676\u77f3\u57fa\u5e95\uff09\u548c\uff084\uff09\u5728\u5ba4\u6e29\uff08~25\u2103\uff09\u4e0b\u6d4b\u91cf\u6c34\u5728\u819c\u8868\u9762\u4e0a\u7684\u63a5\u89e6\u89d2\uff1b<\/p>\n<p>\uff08c\uff09FC-CNT\u819c\uff081\uff09\u8868\u9762SEM\u56fe\u50cf\uff0c\uff082\uff09\u6a2a\u622a\u9762SEM\u56fe\u50cf\uff0c\uff083\uff09\u7b80\u5316\u7684\u7ed3\u6784\u6a21\u578b\uff08\u9ed1\u8272\uff1aCNT\uff1b\u6d45\u7eff\u8272\uff1a\u5c16\u6676\u77f3\u57fa\u5e95\uff09\u548c\uff084\uff09\u5728\u5ba4\u6e29\uff08~25\u2103\uff09\u4e0b\u6d4b\u91cf\u6c34\u5728\u819c\u8868\u9762\u4e0a\u7684\u63a5\u89e6\u89d2\uff1b\u56fe2c2\u4e2d\u7684\u63d2\u56feSEM\u56fe\u50cf\u662fFC-CNT\u819c\u8868\u9762\u4e0a\u539a\u5ea6~4\u03bcm\u7684\u8d85\u758f\u6c34\u7f51\u7edc\u5c42\uff09\u3002<\/p>\n<p><strong><b>\u56fe3.\u00a0<\/b><\/strong><b><\/b><strong><b>PC-CNT<\/b><\/strong><strong><b>\u819c\u548c<\/b><\/strong><strong><b>FC-CNT\u819c\u7684DCMD\u6027\u80fd\u4e0e\u6027\u8d28<\/b><\/strong><strong><b>\u8868\u5f81<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-150915\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/3-32.jpg\" alt=\"\" width=\"600\" height=\"642\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/3-32.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/3-32-280x300.jpg 280w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff0cb\uff09\u5206\u522b\u4e3aPC-CNT\u548cFC-CNT\u819c\u7684DCMD\u6027\u80fd\uff08\u6c34\u901a\u91cf\uff0c\u8131\u76d0\u7387\u548c\u998f\u51fa\u7269\u7535\u5bfc\u7387\uff09\uff1b<\/p>\n<p>\uff08c\uff09FC-CNT\u819c\u5904\u7406\u4e0d\u540c\u65f6\u95f4\u7684\u6c34\u63a5\u89e6\u89d2\u53d8\u5316\uff08\u7ea2\u8272\u5b9e\u5fc3\u5706\uff09\uff0c\u52a0\u901f\u70ed\u7a33\u5b9a\u6027\u6d4b\u8bd5\u4e2d\u7684SiNCO-\uff08\u84dd\u8272\u5b9e\u5fc3\u5706\uff09\u548cFAS-\uff08\u9ed1\u8272\u5b9e\u5fc3\u5706\uff09\u6539\u6027\u9676\u74f7\u819c\uff08\u4e0a\u56fe\u4e2d\u7684\u63d2\u56fe\uff1aFC-CNT\u819c\u4e0a\u6c34\u6ef4\u7684\u5149\u5b66\u56fe\u548c\u6c34\u63a5\u89e6\u89d2\u503c\uff09\uff1b<\/p>\n<p>\uff08d\uff09\u5728\u52a0\u901f\u7a33\u5b9a\u6027\u8bd5\u9a8c24\u5c0f\u65f6\u540e\uff0cFC-CNT\u819c\uff0cSi<sub>3<\/sub>N<sub>4<\/sub>-SiNCO\u9676\u74f7\u819c\u548cSi<sub>3<\/sub>N<sub>4<\/sub>-FAS\u9676\u74f7\u819c\u7684\u758f\u6c34\u635f\u5931\u6bd4\u8f83\uff1b<\/p>\n<p>\uff08e\uff09\u5728\u4e09\u79cd\u4e0d\u540c\u7684MD\u5de5\u827a\u4e0b\uff1aDCMD\uff08\u5b9e\u5fc3\u5706\u6216\u661f\u5f62\uff09\uff0cVMD\uff08\u771f\u7a7a\u819c\u84b8\u998f\uff09\uff08\u7a7a\u5fc3\u5706\uff09\u548cSGMD\uff08\u5439\u626b\u6c14\u819c\u84b8\u998f\uff09\uff08\u7a7a\u5fc3\u5706\uff09\uff0c\u6587\u732e\u4e2d\u62a5\u9053\u7684\u73b0\u6709\u6700\u5148\u8fdb\u7684\u758f\u6c34\u6027\u65e0\u673aMD\u819c\uff08\u5982\u9676\u74f7\uff0c\u91d1\u5c5e\u548c\u78b3\u57fa\u819c\uff09\u4e0e\u9676\u74f7-CNT\u4e4b\u95f4\u7684\u6c34\u901a\u91cf\u548c\u6c34\u63a5\u89e6\u89d2\u7684\u6bd4\u8f83\uff08\u758f\u6c34\u6027\uff09\uff1b<\/p>\n<p>\uff08f\uff09\u5728\u4e09\u79cd\u4e0d\u540c\u7684MD\u5de5\u827a\u4e0b\uff1aDCMD\uff08\u5b9e\u5fc3\u5706\u6216\u661f\u5f62\uff09\uff0cVMD\uff08\u771f\u7a7a\u819c\u84b8\u998f\uff09\uff08\u7a7a\u5fc3\u5706\uff09\u548cSGMD\uff08\u5439\u626b\u6c14\u819c\u84b8\u998f\uff09\uff08\u7a7a\u5fc3\u5706\uff09\uff0c\u6587\u732e\u4e2d\u62a5\u9053\u7684\u73b0\u6709\u6700\u5148\u8fdb\u7684\u758f\u6c34\u6027\u65e0\u673aMD\u819c\uff08\u5982\u9676\u74f7\uff0c\u91d1\u5c5e\u548c\u78b3\u57fa\u819c\uff09\u4e0e\u672c\u6587\u4e2d\u5236\u5907\u7684FC-CNT\u590d\u5408\u819c\uff08\u7ea2\u8272\u5b9e\u5fc3\u661f\uff09\u4e4b\u95f4\u7684\u8131\u76d0\u7387\u548c\u6c34\u63a5\u89e6\u89d2\uff08\u758f\u6c34\u6027\uff09\u7684\u6bd4\u8f83\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4<\/b><\/strong><strong><b>.\u00a0<\/b><\/strong><b><\/b><strong><b>e-DCMD\u8fd0\u884c\u671f\u95f4FC-CNT\u819c\u6027\u80fd\u548c\u819c\u6c61\u67d3\u7ed3\u6784\u8868\u5f81\u4e0e\u6a21\u578b<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-150916\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/4-30.jpg\" alt=\"\" width=\"600\" height=\"833\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/4-30.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/4-30-216x300.jpg 216w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09FC-CNT\u819c\u7684\u521d\u59cbDCMD\u6027\u80fd\uff08\u6c34\u901a\u91cf\uff0c\u8131\u76d0\u7387\u548c\u998f\u51fa\u7269\u7535\u5bfc\u7387\uff09\u4e0e\u76d0\u6d53\u5ea6\u7684\u51fd\u6570\u5173\u7cfb\uff1b<\/p>\n<p>\uff08b\uff09MD\u64cd\u4f5c6h\u540e\u7528\u70ed\u53bb\u79bb\u5b50\u6c34\u53cd\u6d17\u5904\u7406\u9ad8\u77ff\u5316\u5ea6\u6c34(70 g\u00b7L<sup>-1<\/sup>\u00a0NaCl)\u7684\u901a\u91cf\uff0c\u8131\u76d0\u7387\u548c\u998f\u51fa\u7269\u7535\u5bfc\u7387\u968fMD\u5de5\u827a\u64cd\u4f5c\u65f6\u95f4\u7684\u53d8\u5316\u5173\u7cfb\uff1b<\/p>\n<p>\uff08c\uff0cd\uff09\u5bf9\u4e8e\u542b\u6709\u8150\u6b96\u9178\u6709\u673a\u6c61\u57a2(70 g\u00b7L<sup>-1<\/sup>\u00a0NaCl\u548c30 mg\u00b7L<sup>-1<\/sup>\u8150\u6b96\u9178)\u7684\u9ad8\u76d0\u5ea6\u6c34\u5728e-DCMD\u8fd0\u884c6 h\u540e\u7528\u70ed\u53bb\u79bb\u5b50\u6c34\u53cd\u51b2\u6d17\u6e05\u6d17\u9ad8\u77ff\u5316\u5ea6\u6c34\u65f6\u7684\u6c34\u901a\u91cf\u548c\u8131\u76d0\u7387\u53d8\u5316\uff1b<\/p>\n<p>\uff08e-g\uff09\u5f53FC-CNT\u819c\u5728e-DCMD\u8fd0\u884c6 h\u540e\uff0c\u5206\u522b\u4f5c\u4e3a\u4e0d\u540c\u7684\u7535\u6781\uff08e\uff09\u5f00\u8def\uff0c\uff08f\uff09\u9634\u6781\u548c\uff08g\uff09\u9633\u6781\u65f6\u819c\u8868\u9762SEM\u56fe\u50cf\u548c\u6c34\u63a5\u89e6\u89d2\u503c\uff08\u63d2\u56fe\uff09\uff1b<\/p>\n<p>\uff08h-j\uff09\u5728\u4e0d\u540c\u7684\u7535\u5316\u5b66\u8f85\u52a9\u4e0b\uff0ce-DCMD\u8fd0\u884c\u671f\u95f4FC-CNT\u819c\u8868\u9762\u4e0a\u7684\u8868\u5f81\u548c\u9759\u7535\u76f8\u4e92\u4f5c\u7528\u7b80\u5316\u4e86\u6a21\u578b\uff1a\uff08h\uff09\u65e0\u6781\u5316\uff08\u5f00\u8def\uff09\uff0c\uff08i\uff09\u8d1f\u6781\u5316\uff08FC-CNT\u819c\u4f5c\u4e3a\u9634\u6781\uff09\u548c\uff08j\uff09\u6b63\u6781\u5316\uff08FC-CNT\u819c\u4f5c\u4e3a\u9633\u6781\uff09\u3002<\/p>\n<p>\u3010<strong><b>\u5c0f\u7ed3<\/b><\/strong>\u3011<\/p>\n<p>\u9488\u5bf9\u9ad8\u76d0\u5ea6\u5e9f\u6c34\u7684DCMD\u5904\u7406\uff0c\u56e2\u961f\u63d0\u51fa\u4e86\u5177\u6709\u70ed\u548c\u8d85\u758f\u6c34\u64cd\u4f5c\u7a33\u5b9a\u6027\u7684\u9ad8\u6027\u80fd\u65e0\u673a\u9676\u74f7-CNT\u7ed3\u6784\u819c\u7684\u6982\u5ff5\u8bbe\u8ba1\u4e0e\u5e94\u7528\u7b56\u7565\u3002\u4ee5\u4e2d\u7a7a\u7ea4\u7ef4\u7279\u6b8a\u7ed3\u6784\u7684\u591a\u5b54\u9676\u74f7\u819c\u4e3a\u8f7d\u4f53\uff0c\u901a\u8fc7\u539f\u4f4dCVD\u751f\u957f\u6784\u5efa\u8d85\u758f\u6c34\u548c\u8d85\u591a\u5b54CNT\u8868\u9762\u7f51\u7edc\u7ed3\u6784\u3002\u4e0e\u73b0\u6709\u7684\u65e0\u673a\u758f\u6c34\u819c\u76f8\u6bd4\uff0cFC-CNT\u819c\u5177\u6709\u4f18\u5f02\u7684\u8d85\u758f\u6c34\u6027\u548c\u70ed\u7a33\u5b9a\u6027\u3002\u7531\u4e8e\u5176\u51fa\u8272\u7684\u6297\u6d78\u6da6\u7279\u6027\u548c\u819c\u7ed3\u6784\uff0cFC-CNT\u819c\u5177\u6709\u9ad8\u800c\u7a33\u5b9a\u7684\u6c34\u901a\u91cf\u548c\u8131\u76d0\u7387\u3002\u6b64\u5916\uff0c\u5728\u7b80\u5355\u4e14\u65e0\u635f\u7684e-DCMD\u64cd\u4f5c\u4e0b\uff0cFC-CNT\u819c\u8868\u73b0\u51fa\u7a33\u5b9a\u7684\u9ad8\u901a\u91cf\uff0c\u9ad8\u8131\u76d0\u7387\uff0c\u5c24\u5176\u662f\u5bf9\u8150\u6b96\u9178\u5177\u6709\u4f18\u5f02\u7684\u6297\u6c61\u67d3\u6027\u3002\u672c\u7814\u7a76\u7684\u7ed3\u679c\u5c06\u4e3a\u5176\u4ed6\u5148\u8fdb\u65e0\u673a\u819c\u7684\u8bbe\u8ba1\u548c\u5236\u9020\u63d0\u4f9b\u4e86\u65b0\u601d\u8def\u548c\u6280\u672f\u53c2\u8003\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5<\/b><\/strong><strong><b>\uff1a<\/b><\/strong><a href=\"https:\/\/pubs.acs.org\/doi\/10.1021\/acs.nanolett.8b01907\" target=\"_blank\" rel=\"noopener\"><u>Stable Superhydrophobic Ceramic-based Carbon Nanotube Composite Desalination Membranes<\/u><\/a>\uff08Nano Lett., 2018, DOI\uff1a10.1021\/acs.nanolett.8b01907\uff09<\/p>\n<p>\u3010<b>\u56e2\u961f\u4ecb\u7ecd<\/b>\u3011<\/p>\n<p><strong><b>\u901a\u8baf\u4f5c\u8005<\/b><\/strong><strong><b>\u4ecb\u7ecd\uff1a<\/b><\/strong>\u8463\u5e94\u8d85\uff0c\u7537\uff0c\u5de5\u5b66\u535a\u58eb\uff0c\u5927\u8fde\u7406\u5de5\u5927\u5b66\u73af\u5883\u5b66\u9662\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\u30022008\u5e74\u83b7\u5f97\u4e2d\u56fd\u79d1\u5b66\u6280\u672f\u5927\u5b66\u5de5\u5b66\u535a\u58eb\u5b66\u4f4d\u30022007-2016\u5e74\u5148\u540e\u5728\u4e09\u4e00\u7535\u6c14\u4e0a\u6d77\u7814\u7a76\u9662\u3001\u56fd\u5bb6\u9676\u74f7\u5de5\u7a0b\u4e2d\u5fc3\/\u4e2d\u56fd\u79d1\u6280\u5927\u5b66\u3001\u7231\u5c14\u5170Limerick\u5927\u5b66\uff08Irish Research Council for Science Engineering and Technology Research Fellow\uff09\u3001\u65e5\u672c\u4e1c\u4eac\u5de5\u4e1a\u5927\u5b66\uff08PD Researcher\u548cJPSP\u5916\u56fd\u4eba\u7279\u522b\u7814\u7a76\u5458\uff09\u3001\u4e2d\u79d1\u9662\u57ce\u5e02\u73af\u5883\u7814\u7a76\u6240\uff08\u7814\u7a76\u5458\u3001\u535a\u5bfc\uff09\u7b49\u56fd\u5185\u5916\u673a\u6784\u4ece\u4e8b\u79d1\u5b66\u7814\u7a76\u548c\u6280\u672f\u5f00\u53d1\u5de5\u4f5c\u3002\u4e3b\u8981\u4ece\u4e8b\u819c\u6280\u672f\u53ca\u73af\u5883\u80fd\u6e90\u5e94\u7528\u3001\u65e0\u673a\u9676\u74f7\u819c\u53ca\u9676\u74f7\u57fa\u590d\u5408\u819c\u3001\u6c34\u5904\u7406\u4e0e\u6c14\u4f53\u5206\u79bb\u3001\u65e0\u673a\u56fa\u4f53\u5e9f\u5f03\u7269\/\u77ff\u7269\u8d44\u6e90\u5316\u548c\u73af\u5883\u53cb\u597d\u6750\u6599\u7b49\u65b9\u9762\u7814\u7a76\u5de5\u4f5c\uff0c\u81f4\u529b\u4e8e\u201c\u73af\u5883\u819c\u6280\u672f\u4e0e\u6c61\u67d3\u63a7\u5236\u5de5\u7a0b\u201d\u7684\u6280\u672f\u5f00\u53d1\u53ca\u4ea7\u4e1a\u5316\u5de5\u4f5c\u3002\u81f3\u4eca\uff0c\u5728\u56fd\u9645\u5b66\u672f\u671f\u520a\uff08\u5982Nano Lett., Water Res. J. Membr. Sci., ACS Sustain. Chem. Eng., J. Am. Ceram. Soc., J. Eur. Ceram. Soc.,J. Power Sources\u7b49\uff09\u3001\u5b66\u672f\u4f1a\u8bae\u4e0a\u7b49\u53d1\u8868\u8bba\u658790\u4f59\u7bc7\uff0c\u5176\u4e2dSCI \u8bba\u6587~70\u7bc7\uff0cJCR\u4e00\u533a\u8bba\u6587~40\u7bc7\u3002\u8bba\u6587\u5f15\u7528~1500\u6b21\uff08H-index=25\uff09\u3002\u7533\u8bf7\u4e13\u52298\u9879\u3002\u83b7\u5f97\u7231\u5c14\u5170\u79d1\u6280\u5de5\u7a0b\u57fa\u91d1\u4f1a\u3001\u65e5\u672c\u5b66\u672f\u632f\u5174\u4f1aJSPS\u3001\u798f\u5efa\u7701\u6770\u9752\u548c\u5b81\u6ce2\u5e02\u9886\u519b\u548c\u62d4\u5c16\u4eba\u624d\u5de5\u7a0b\u7b49\u8d44\u52a9\u3002\u5148\u540e\u4e3b\u6301\u7231\u5c14\u5170Irish Research Council for Science Engineering and Technology\u9879\u76ee\u3001\u65e5\u672cJSPS\u9879\u76ee\u3001\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u59d4\u548c\u591a\u9879\u7701\u5e02\u7ea7\u8bfe\u9898\uff0c\u53c2\u4e0e\u56fd\u5bb6973\u9879\u76ee\u3001\u7231\u5c14\u5170SFI\u9879\u76ee\u3001\u65e5\u672cJST\u5143\u7d20\u6218\u7565\u9879\u76ee\u548c\u65e5\u672cMEXT\u9879\u76ee\u7b49\u3002\u517c\u4efb\u300a\u819c\u79d1\u5b66\u4e0e\u6280\u672f\u300b\uff08\u4e2d\u6587\u6838\u5fc3\uff09\u548c\u201cMembranes\u201d(ESCI\/EI, MDPI),\u201cJournal of Chemistry\u201d(SCI),\u201cEnvironments\u201d(ESCI, MDPI), Heliyon\u201d(ESCI, Elsevier)\u7b49\u591a\u4e2a\u56fd\u9645\u5b66\u672f\u671f\u520a\u7684\u7f16\u59d4\uff08Editorial Board\uff09\u3002<\/p>\n<p>\u4f5c\u8005\u94fe\u63a5\uff1a<a href=\"http:\/\/faculty.dlut.edu.cn\/2016011051\/zh_CN\/index.htm\" target=\"_blank\" rel=\"noopener\">http:\/\/faculty.dlut.edu.cn\/2016011051\/zh_CN\/index.htm<\/a><\/p>\n<p>\u3010<strong><b>\u6210\u679c\u6c47\u603b<\/b><\/strong>\u3011<\/p>\n<p><strong><b>\u56e2\u961f\u8fd1\u671f\u5de5\u4f5c\u6c47\u603b\u53ca\u4f18\u8d28\u6587\u732e<\/b><\/strong><strong><b>\u63a8\u8350\uff1a<\/b><\/strong><\/p>\n<ol>\n<li>Li Zhu, Mingliang Chen, <strong><u><b>Yingchao Dong*<\/b><\/u><\/strong>, Chuyang Y. Tang, Aisheng Huang, Lingling Li,A low-cost mullite-titania composite ceramic hollow fiber microfiltration membrane for highly efficient separation of oil-in-water emulsion,\u00a0<strong><em><b><i>Water Research<\/i><\/b><\/em><\/strong>, 90 (2016) 277-285. (SCI\u4e00\u533a\uff0cIF(2017)=7.051)<\/li>\n<li>Li Zhu, <strong><u><b>Yingchao Dong<\/b><\/u><\/strong><strong><b>*<\/b><\/strong>, Stuart Hampshire, Sophie Cerneaux, Louis Winnubst, Waste-to-resource preparation of a porous ceramic membrane support featuring elongated mullite whiskers with enhanced porosity and permeance, <strong><em><b><i>Journal of the European Ceramic Society<\/i><\/b><\/em><\/strong>, 35 (2015) 711-721.(SCI\u4e00\u533a\uff0cIF(2017)=3.794)<\/li>\n<li>Mingliang Chen, Li Zhu, <strong><u><b>Yingchao Dong*<\/b><\/u><\/strong>, Lingling Li, Jing Liu, Waste-to-resource strategy to fabricate highly porous whisker-structured mullite ceramic membrane for simulated oil-in-water emulsion wastewater treatment,<strong><em><b><i>ACS Sustainable Chemistry &amp; Engineering<\/i><\/b><\/em><\/strong>, 4 (2016) 2098-2106. (SCI\u4e8c\u533a\uff0cIF(2017)=6.14)<\/li>\n<\/ol>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u5b66\u672f\u7ec4<strong><b>\u6728\u6587\u97ec<\/b><\/strong>\u7ffb\u8bd1\uff0c<strong><b>\u5927\u8fde\u7406\u5de5\u5927\u5b66<\/b><\/strong><strong><b>\u8463\u5e94\u8d85\u6559\u6388<\/b><\/strong><strong><b>\u56e2\u961f<\/b><\/strong>\u4fee\u6b63\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c<a href=\"http:\/\/www.cailiaoniu.com\/25127.html\" target=\"_blank\" rel=\"noopener\"><strong><u><b>\u70b9\u6211\u52a0\u5165\u7f16\u8f91\u90e8<\/b><\/u><\/strong><\/a>\u3002\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u4eea\u5668\u8bbe\u5907\u3001\u8bd5\u5242\u8017\u6750\u3001\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u627e\u6750\u6599\u4eba\u3001\u4e0a<a href=\"http:\/\/www.ceshigu.com\/\" target=\"_blank\" rel=\"noopener\"><strong><u><b>\u6d4b\u8bd5\u8c37<\/b><\/u><\/strong><\/a><strong><b>\uff01<\/b><\/strong><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u6d77\u6c34\u6de1\u5316\u6b63\u6210\u4e3a\u7f13\u89e3\u6de1\u6c34\u8d44\u6e90\u5371\u673a\u7684\u4e00\u79cd\u5e7f\u6cdb\u5e94\u7528\u7684\u65b9\u6cd5\u3002\u7136\u800c\uff0c\u901a\u8fc7\u53cd\u6e17\u900f\u819c(RO)\u5de5\u827a\u8fdb\u884c\u5927\u89c4\u6a21\u6d77\u6c34\u6de1\u5316\u4f1a\u4ea7\u751f\u5927\u91cf\u9ad8\u76d0\u5ea6\u7684\u5e9f\u6c34\uff0c\u82e5\u76f4\u63a5\u6392\u6d77\u4f1a\u5bf9\u6d77\u6d0b\u73af\u5883\u9020\u6210&#8230;<\/p>\n","protected":false},"author":2109,"featured_media":150917,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[2527],"class_list":["post-150910","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-2527"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/150910"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2109"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=150910"}],"version-history":[{"count":21,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/150910\/revisions"}],"predecessor-version":[{"id":151446,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/150910\/revisions\/151446"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/150917"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=150910"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=150910"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=150910"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}