{"id":150996,"date":"2018-08-20T06:57:43","date_gmt":"2018-08-19T22:57:43","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=150996"},"modified":"2018-08-19T17:58:19","modified_gmt":"2018-08-19T09:58:19","slug":"%e9%a9%ac%e9%87%8c%e5%85%b0%e5%a4%a7%e5%ad%a6%e8%83%a1%e8%89%af%e5%85%b5adv-mater-%ef%bc%9a%e5%8f%97%e8%82%8c%e8%82%89%e5%90%af%e5%8f%91%e7%9a%84%e9%ab%98%e5%ba%a6%e5%90%84%e5%90%91%e5%bc%82%e6%80%a7","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=150996","title":{"rendered":"\u9a6c\u91cc\u5170\u5927\u5b66\u80e1\u826f\u5175Adv. Mater.\uff1a\u53d7\u808c\u8089\u542f\u53d1\u7684\u9ad8\u5ea6\u5404\u5411\u5f02\u6027\u3001\u9ad8\u5f3a\u4e14\u79bb\u5b50\u5bfc\u7535\u7684\u6c34\u51dd\u80f6"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u57fa\u4e8e3D\u7ed3\u6784\u3001\u826f\u597d\u7684\u67d4\u6027\u548c\u751f\u7269\u76f8\u5bb9\u6027\u4ee5\u53ca\u9ad8\u542b\u6c34\u91cf\u7b49\u7279\u70b9\uff0c\u6c34\u51dd\u80f6\u6750\u6599\u5df2\u7ecf\u5728\u8bf8\u5982\u836f\u7269\u9012\u9001\u3001\u8f6f\u6267\u884c\u5668\u3001\u7535\u5316\u5b66\u5668\u4ef6\u548c\u4eba\u5de5\u808c\u8089\u7b49\u751f\u7269\u533b\u5b66\u548c\u751f\u7269\u5de5\u7a0b\u9886\u57df\u53d1\u6325\u91cd\u8981\u4f5c\u7528\u3002\u7136\u800c\uff0c\u5927\u591a\u6570\u7684\u7ea4\u7ef4\u7d20\u57fa\u6c34\u51dd\u80f6\u6750\u6599\u5fae\u89c2\u7ed3\u6784\u6709\u5e8f\u5ea6\u548c\u5b8f\u89c2\u673a\u68b0\u6027\u80fd\u90fd\u6bd4\u8f83\u5dee\uff0c\u6781\u5927\u9650\u5236\u4e86\u5176\u5e94\u7528\u4ef7\u503c\u3002\u5b9a\u5411\u51b7\u51bb\u3001\u9759\u7535\u6392\u65a5\u3001\u62c9\u4f38\u6216\u538b\u7f29\u8bf1\u5bfc\u91cd\u65b0\u5b9a\u5411\u4ee5\u53ca\u81ea\u7ec4\u88c5\u7b49\u591a\u79cd\u65b9\u6cd5\u88ab\u8bc1\u5b9e\u80fd\u591f\u4e00\u5b9a\u7a0b\u5ea6\u4e0a\u63d0\u9ad8\u6c34\u51dd\u80f6\u7684\u673a\u68b0\u6027\u80fd\uff0c\u4f46\u662f\u6c34\u51dd\u80f6\u6750\u6599\u7684\u62c9\u4f38\u5f3a\u5ea6\u4ecd\u7136\u6ca1\u6709\u8fbe\u523010 MPa\uff08\u751f\u7269\u7ec4\u7ec7\u5f3a\u5ea6\uff09\u3002\u4ece\u4eff\u751f\u89d2\u5ea6\u6765\u8bf4\uff0c\u5728\u6c34\u51dd\u80f6\u7f51\u7edc\u7ed3\u6784\u4e2d\u5f15\u5165\u7c7b\u4f3c\u808c\u8089\u7ec4\u7ec7\u4e2d\u7684\u9ad8\u5ea6\u6709\u5e8f\u7eb3\u7c73\u7ed3\u6784\u4e3a\u83b7\u5f97\u9ad8\u5ea6\u5404\u5411\u5f02\u6027\u3001\u9ad8\u5f3a\u6c34\u51dd\u80f6\u63d0\u4f9b\u4e86\u673a\u4f1a\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u7f8e\u56fd\u9a6c\u91cc\u5170\u5927\u5b66\u80e1\u826f\u5175\u6559\u6388\u8bfe\u9898\u7ec4<\/strong>\u7ed3\u5408\u5929\u7136\u6728\u6750\u7684\u9ad8\u62c9\u4f38\u5f3a\u5ea6\u548c\u6c34\u51dd\u80f6\u7684\u67d4\u6027\u3001\u9ad8\u542b\u6c34\u91cf\u7b49\u7279\u70b9\uff0c\u5b9e\u73b0\u4e86\u9ad8\u5ea6\u5404\u5411\u5f02\u6027\u3001\u9ad8\u5f3a\u4e14\u79bb\u5b50\u5bfc\u7535\u7684\u6728\u6750\u6c34\u51dd\u80f6\u7684\u5236\u5907\u3002\u7814\u7a76\u8868\u660e\uff0c\u6709\u5e8f\u7ea4\u7ef4\u7d20\u7eb3\u7c73\u7ea4\u7ef4\u4e0e\u805a\u5408\u7269\u5206\u5b50\u94fe\u4e4b\u95f4\u5b58\u5728\u8f83\u5f3a\u7684\u6c22\u952e\u4f5c\u7528\u548c\u4ea4\u8054\u7ed3\u6784\uff0c\u4f7f\u5f97\u6728\u6750\u6c34\u51dd\u80f6\u7684\u62c9\u4f38\u5f3a\u5ea6\u9ad8\u8fbe36 MPa\uff0c\u662f\u76ee\u524d\u62a5\u9053\u7684\u5f3a\u5ea6\u6700\u9ad8\u7684\u6c34\u51dd\u80f6\u6750\u6599\u4e4b\u4e00\u3002\u6b64\u5916\uff0c\u7531\u4e8e\u6709\u5e8f\u7ea4\u7ef4\u7d20\u7eb3\u7c73\u7ea4\u7ef4\u5e26\u6709\u8d1f\u7535\u8377\uff0c\u8be5\u79cd\u6728\u6750\u6c34\u51dd\u80f6\u8fd8\u53ef\u4ee5\u4f5c\u4e3a\u7eb3\u7c73\u6d41\u4f53\u5bfc\u7ba1\u5b9e\u73b0\u7c7b\u4f3c\u751f\u7269\u808c\u8089\u7ec4\u7ec7\u7684\u79bb\u5b50\u9009\u62e9\u6027\u4f20\u8f93\u529f\u80fd\u3002\u8be5\u6210\u679c\u4ee5\u9898\u4e3a&#8221;<strong>Muscle-Inspired Highly Anisotropic, Strong, Ion-Conductive Hydrogels&#8221;<\/strong>\u53d1\u8868\u5728<strong>Advanced Materials<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe1\u6728\u6750\u6c34\u51dd\u80f6\u7684\u7ed3\u6784\u548c\u5fae\u89c2\u7f51\u7edc\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-150997 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-1-2.jpg\" alt=\"\" width=\"600\" height=\"515\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-1-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-1-2-300x258.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u5e38\u89c1\u7684\u67d4\u6027\u6a2a\u7eb9\u808c\u8089\u7ec4\u7ec7\u793a\u610f\u56fe\uff1b<\/p>\n<p>(b) 7 cm\u957f\u7684\u6728\u6750\u6c34\u51dd\u80f6\u6837\u54c1\u626d\u66f2180\u5ea6\u7684\u7167\u7247\uff1b<\/p>\n<p>(c) \u6728\u6750\u6c34\u51dd\u80f6\u5185\u90e8PAM\u5206\u5b50\u94fe\u4e4b\u95f4\u6c22\u952e\u548c\u5171\u4ef7\u4ea4\u8054\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe2\u6728\u6750\u6c34\u51dd\u80f6\u548c\u767d\u6728\u7684\u5149\u5b66\u4ee5\u53caSEM\u56fe\u7247<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-150998 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-2-2.jpg\" alt=\"\" width=\"600\" height=\"581\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-2-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-2-2-300x291.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u53bb\u9664\u6728\u8d28\u7d20\u540e\u767d\u6728\u7684\u7167\u7247\uff1b<\/p>\n<p>(b) \u767d\u6728\u7684\u653e\u5927\u56fe\u50cf\u6e05\u6670\u5730\u5c55\u73b0\u51fa\u6709\u5e8f\u7684\u7ea4\u7ef4\u6392\u5217\uff1b<\/p>\n<p>(c) \u767d\u6728\u7684\u9ad8\u500dSEM\u56fe\u7247\u8bc1\u5b9e\u4e86\u6709\u5e8f\u7ea4\u7ef4\u7d20\u7eb3\u7c73\u7ea4\u7ef4\uff1b<\/p>\n<p>(d) \u6cbfL\u65b9\u5411\u5f2f\u66f2\u7684\u6c34\u51dd\u80f6\u7167\u7247\uff1b<\/p>\n<p>(e) \u6cbfR\u65b9\u5411\u5f2f\u66f20.01 M\u7684\u6c34\u51dd\u80f6\u7167\u7247\uff1b<\/p>\n<p>(f) \u6cbfL\u548cR\u65b9\u5411\u5f2f\u66f2\u7684\u6c34\u51dd\u80f6\u90fd\u53ef\u4ee5\u8fc5\u901f\u6062\u590d\u539f\u59cb\u67f1\u72b6\u7ed3\u6784\u800c\u6ca1\u6709\u65ad\u88c2\u6216\u8005\u5851\u6027\u5f62\u53d8\uff1b<\/p>\n<p>(g) \u53bb\u9664\u6728\u8d28\u7d20\u540e\u6728\u5757R\u65b9\u5411\u6a2a\u622a\u9762\u7684SEM\u56fe\u50cf\uff0c\u663e\u793a\u5176\u5185\u8868\u9762\u6709\u8bb8\u591a\u5b54\uff1b<\/p>\n<p>(h) \u4e0ePAM\u6c34\u51dd\u80f6\u5f62\u6210\u6728\u6750\u6c34\u51dd\u80f6\u7684R\u65b9\u5411\u6a2a\u622a\u9762\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>(i) \u6728\u6750\u6c34\u51dd\u80f6\u7684\u653e\u5927SEM\u56fe\u50cf\uff0c\u663e\u793a\u51fa\u8be6\u7ec6\u7684\u5fae\u89c2\u7ed3\u6784\uff1b<\/p>\n<p>(j) \u767d\u6728\u7684L\u65b9\u5411\u6a2a\u622a\u9762SEM\u56fe\u50cf\uff1b<\/p>\n<p>(k) \u6728\u6750\u6c34\u51dd\u80f6\u7684L\u65b9\u5411\u6a2a\u622a\u9762SEM\u56fe\u50cf\uff1b<\/p>\n<p>(l) \u6728\u6750\u6c34\u51dd\u80f6\u7684\u653e\u5927SEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe3 \u6728\u6750\u6c34\u51dd\u80f6\u7684\u529b\u5b66\u6027\u8d28<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-150999 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-3-2.jpg\" alt=\"\" width=\"600\" height=\"438\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-3-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-3-2-300x219.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) PAM\u6c34\u51dd\u80f6\u548c\u6728\u6750\u6c34\u51dd\u80f6R\u65b9\u5411\u4e0a\u7684\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\uff1b<\/p>\n<p>(b) \u6728\u6750\u6c34\u51dd\u80f6L\u65b9\u5411\u4e0a\u7684\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\uff1b<\/p>\n<p>(c) \u4e0e\u5176\u4ed6\u6c34\u51dd\u80f6\u76f8\u6bd4\u7684\u6781\u9650\u62c9\u4f38\u5f3a\u5ea6\uff1b<\/p>\n<p>(d) \u6728\u6750\u6c34\u51dd\u80f6\u7684SEM\u4fa7\u89c6\u56fe\u56fe\u50cf\uff0c\u663e\u793aPAM\u7f51\u7edc\u548c\u767d\u6728\u5b54\u9053\u7684\u8be6\u7ec6\u5fae\u89c2\u7ed3\u6784\uff1b<\/p>\n<p>(e, f) \u6728\u6750\u6c34\u51dd\u80f6\u7684\u653e\u5927SEM\u56fe\u50cf\uff0c\u663e\u793a\u6709\u5e8f\u7ea4\u7ef4\u7d20\u7eb3\u7c73\u7ea4\u7ef4\u4e5f\u901a\u8fc7\u6c22\u952e\u4e0ePAM\u5206\u5b50\u94fe\u4ea4\u8054\uff1b<\/p>\n<p>(g) PAM\u9ad8\u5206\u5b50\u94fe\u4e0e\u6709\u5e8f\u7ea4\u7ef4\u7d20\u7eb3\u7c73\u7ea4\u7ef4\u95f4\u6c22\u952e\u7ed3\u5408\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe4 \u6728\u6750\u6c34\u51dd\u80f6\u4e2d\u7684\u79bb\u5b50\u4f20\u8f93<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-151000 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-4-2.jpg\" alt=\"\" width=\"600\" height=\"495\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-4-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/08\/\u672a\u6807\u9898-4-2-300x248.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u6728\u6750\u6c34\u51dd\u80f6\u4e2d\u79bb\u5b50\u4f20\u8f93\u7684\u673a\u5236\u793a\u610f\u56fe\uff1b<\/p>\n<p>(b) \u6d4b\u8bd5\u7535\u8def\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>(c) 10<sup>-5<\/sup> M KCl\u6eb6\u6db2\u4e2d\u6728\u6750\u6c34\u51dd\u80f6\u7684Zeta\u7535\u4f4d\uff1b<\/p>\n<p>(d) \u6728\u6750\u6c34\u51dd\u80f6\u548cKCl\u6eb6\u6db2\u5728pH 7\u5de6\u53f3\u65f6\uff0c\u79bb\u5b50\u7535\u5bfc\u7387\u4e0eKCl\u6d53\u5ea6\u7684\u5173\u7cfb\u56fe\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u6587\u53d7\u808c\u8089\u7ec4\u7ec7\u7ed3\u6784\u7684\u542f\u53d1\u5236\u5907\u4e86\u4e00\u79cd\u9ad8\u5ea6\u5404\u5411\u5f02\u6027\u3001\u9ad8\u5f3a\u4e14\u79bb\u5b50\u5bfc\u7535\u7684\u6728\u6750\u6c34\u51dd\u80f6\u6750\u6599\uff0c\u5176\u4e2d\u5929\u7136\u6728\u6750\u63d0\u4f9b\u521a\u6027\u9aa8\u67b6\u7ed3\u6784\u800c\u805a\u5408\u7269\u94fe\u4f5c\u4e3a\u4ea4\u8054\u7f51\u7edc\u3002\u8be5\u79cd\u6728\u6750\u6c34\u51dd\u80f6\u6cbfL\u65b9\u5411\u7684\u62c9\u4f38\u5f3a\u5ea6\u8fbe\u523036 MPa\uff0c\u800c\u4e14\u79bb\u5b50\u7535\u5bfc\u7387\u4e3a5 \u00d7 10<sup>-4<\/sup> S cm<sup>-1<\/sup>\u3002\u56e0\u6b64\uff0c\u6709\u5e8f\u5fae\u7ed3\u6784\u7684\u4eff\u751f\u8bbe\u8ba1\u80fd\u591f\u8f83\u597d\u5730\u5e73\u8861\u673a\u68b0\u6027\u80fd\u3001\u79bb\u5b50\u5bfc\u7535\u7387\u4ee5\u53ca\u89c4\u6a21\u5316\u5236\u5907\u7b49\u56e0\u7d20\uff0c\u63d0\u4f9b\u4e86\u5148\u8fdb\u6c34\u51dd\u80f6\u6750\u6599\u8bbe\u8ba1\u7684\u65b0\u65b9\u5411\u3002\u540c\u65f6\uff0c\u6728\u6750\u6c34\u51dd\u80f6\u7684\u8fd9\u4e9b\u4f18\u70b9\u4f7f\u5f97\u5b83\u4eec\u6709\u671b\u5728\u8f6f\u7ec4\u7ec7\u3001\u667a\u80fd\u4f20\u611f\u5668\u8bbe\u5907\u4ee5\u53ca\u7eb3\u7c73\u6d41\u4f53\u5668\u4ef6\u7b49\u9886\u57df\u5f97\u5230\u5e94\u7528\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.201801934\" target=\"_blank\" rel=\"noopener\">Muscle-Inspired Highly Anisotropic, Strong, Ion-Conductive Hydrogels<\/a>\u00a0<\/strong>\u00a0(Adv. Mater. 2018, DOI: 10.1002\/adma.201801934)<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u751f\u7269\u5b66\u672f\u7ec4biotech\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u5ba1\u6838\u6574\u7406\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6295\u7a3f\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaokefu\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u8fd1\u5e74\u6765\uff0c\u57fa\u4e8e3D\u7ed3\u6784\u3001\u826f\u597d\u7684\u67d4\u6027\u548c\u751f\u7269\u76f8\u5bb9\u6027\u4ee5\u53ca\u9ad8\u542b\u6c34\u91cf\u7b49\u7279\u70b9\uff0c\u6c34\u51dd\u80f6\u6750\u6599\u5df2\u7ecf\u5728\u8bf8\u5982\u836f\u7269\u9012\u9001\u3001\u8f6f\u6267\u884c\u5668\u3001\u7535\u5316\u5b66\u5668\u4ef6\u548c\u4eba\u5de5\u808c\u8089\u7b49\u751f\u7269\u533b\u5b66\u548c\u751f\u7269\u5de5\u7a0b\u9886\u57df\u53d1&#8230;<\/p>\n","protected":false},"author":7746,"featured_media":150997,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[2600,3521],"class_list":["post-150996","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-2600","tag-3521"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/150996"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7746"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=150996"}],"version-history":[{"count":6,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/150996\/revisions"}],"predecessor-version":[{"id":151415,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/150996\/revisions\/151415"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/150997"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=150996"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=150996"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=150996"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}