{"id":153651,"date":"2018-09-21T06:54:46","date_gmt":"2018-09-20T22:54:46","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=153651"},"modified":"2018-09-20T20:55:26","modified_gmt":"2018-09-20T12:55:26","slug":"materials-today%e7%bb%bc%e8%bf%b0%ef%bc%9a%e5%bd%a2%e7%8a%b6%e8%ae%b0%e5%bf%86%e5%90%88%e9%87%91%e7%9a%84%e7%9b%b8%e5%8f%98%e6%9d%a1%e4%bb%b6%e4%b8%8e%e8%b6%85%e7%9b%b8%e5%ae%b9%e6%80%a7","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=153651","title":{"rendered":"materials today\u7efc\u8ff0\uff1a\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u7684\u76f8\u53d8\u6761\u4ef6\u4e0e\u8d85\u76f8\u5bb9\u6027"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u5177\u6709\u5408\u9002\u6676\u7c92\u5c3a\u5bf8\u76f8\u7684\u8d85\u7ea7\u76f8\u5bb9\u6027\u548c\u6709\u5229\u7684\u6c89\u6dc0\u7269\u9635\u5217\u76f8\u7ed3\u5408\uff0c\u5b9e\u73b0\u4e86\u529f\u80fd\u548c\u7ed3\u6784\u6297\u75b2\u52b3\u6027\u548c\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u7684\u6ede\u540e\u6027\u7684\u964d\u4f4e\u3002\u672c\u6587\u5206\u6790\u548c\u6bd4\u8f83\u8fd9\u4e9b\u4f8b\u5b50\uff0c\u9610\u660e\u8fd9\u4e9b\u56e0\u7d20\u7684\u4f5c\u7528\uff0c\u53ca\u5728\u66f4\u82db\u523b\u7684\u5e94\u529b\u8bf1\u5bfc\u76f8\u53d8\u7684\u60c5\u51b5\u4e0b\uff0c\u4ecd\u5b58\u5728\u7684\u95ee\u9898\u3002\u8fd9\u4e9b\u56e0\u7d20\u7684\u63a7\u5236\u6709\u52a9\u4e8e\u5408\u91d1\u4f53\u7cfb\u7684\u5f00\u53d1\u3002\u672c\u6587\u5c55\u73b0\u4e86\u6539\u5584\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u7684\u91cd\u8981\u65b9\u6cd5\uff0c\u4ee5\u53ca\u65b0\u7684\u53ef\u9006\u8f6c\u5316\u591a\u94c1\u6027\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u7f8e\u56fd<strong>\u660e\u5c3c\u82cf\u8fbe\u5927\u5b66<\/strong>\u7684<strong>Richard D. James<\/strong>\u548c\u5fb7\u56fd<strong>\u57fa\u5c14\u5927\u5b66<\/strong><strong>Eckhard Quandt<\/strong><strong>\uff08\u5171\u540c\u901a\u8baf\uff09<\/strong>\u4f5c\u8005\u7b49\u4eba\uff0c\u5217\u51fa\u4e86\u63a7\u5236\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u76f8\u53d8\u53ef\u9006\u6027\u6761\u4ef6\uff1a\u6676\u4f53\u76f8\u5bb9\u6027\uff0c\u6676\u7c92\u5c3a\u5bf8\u548c\u6c89\u6dc0\u3002\u7814\u7a76\u8868\u660e\uff0c\u5982\u679c\u6ee1\u8db3\u8fd9\u4e09\u4e2a\u6761\u4ef6\uff0c\u5c31\u53ef\u80fd\u83b7\u5f97\u6781\u597d\u7684\u6297\u529f\u80fd\u75b2\u52b3\u6027\u548c\u4f4e\u6ede\u540e\u6027\u7684\u5408\u91d1\u3002\u7136\u800c\uff0c\u5176\u4e2d\u4e00\u4e2a\u6216\u591a\u4e2a\u6761\u4ef6\u7a0d\u5fae\u6b20\u7f3a\uff0c\u4ecd\u5177\u6709\u663e\u7740\u7684\u529f\u80fd\u75b2\u52b3\u3002\u76f8\u5173\u6210\u679c\u4ee5<strong>\u201c<\/strong><strong>Phase engineering and supercompatibility of shape memory alloys<\/strong>\u201d\u4e3a\u9898\u53d1\u8868\u5728<strong>materials today<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe<\/strong><strong> 1 i-Ni-X-Y<\/strong><strong>\u5408\u91d1\u7684\u6ede\u540e\u4e0e\u03bb<\/strong><strong><sub>2<\/sub><\/strong><strong>\u66f2\u7ebf\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153660\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/1-25.jpg\" alt=\"\" width=\"600\" height=\"215\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/1-25.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/1-25-300x108.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Ti-Ni-X-Y\u5408\u91d1\u7684\u6ede\u540e\u4e0e\u03bb<sub>2<\/sub>\u66f2\u7ebf\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u662f\uff08a\uff09\u4e2d\u03bb<sub>2<\/sub>= 1\u9644\u8fd1\u7684\u56fe\u7684\u653e\u5927\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 2 <\/strong><strong>\u9a6c\u6c0f\u4f53\u6676\u4f53\u5b66\u7406\u8bba\u4e2d\u8f85\u52a9\u56e0\u5b50\u6761\u4ef6\u7684\u542b\u4e49<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153661\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/2-25.jpg\" alt=\"\" width=\"600\" height=\"464\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/2-25.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/2-25-300x232.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5bf9\u4e8e\u7ed9\u5b9a\u7684\u53cc\u7cfb\u7edf\uff0c\u6ca1\u6709\u6676\u4f53\u5b66\u7406\u8bba\u7684\u89e3\u51b3\u65b9\u6848\uff1b<\/p>\n<p>\uff08b\uff09\u53ef\u9006\u9a6c\u6c0f\u4f53\u6ee1\u8db3\u7684\u53cc\u7cfb\u7edf4\u79cd\u89e3\u51b3\u65b9\u6848\u7684\u4e00\u822c\u60c5\u51b5\uff1b<\/p>\n<p>\uff08c\uff09\u60c5\u51b5\u03bb<sub>2<\/sub>= 1\uff0c\uff08d\uff09\u6ee1\u8db3\u8f85\u52a9\u56e0\u5b50\u6761\u4ef6\u7684\u60c5\u51b5\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 3 <\/strong><strong>\u5408\u91d1\u7684\u7acb\u65b9<\/strong><strong>&#8211;<\/strong><strong>\u6b63\u4ea4\u7cfb\u7edf\u4e2d\u7684\u8f85\u52a9\u56e0\u5b50\u6761\u4ef6<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153658\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/3-22.jpg\" alt=\"\" width=\"600\" height=\"492\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/3-22.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/3-22-300x246.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u5408\u91d1\u5206\u522b\u4e3a\uff1aTi<sub>54.7<\/sub>Ni<sub>30.7<\/sub>Cu<sub>12.3<\/sub>Co<sub>2.3<\/sub>\uff08\u03bb<sub>2<\/sub>= 1.00083\uff09\uff0cTiNiCuPd\uff08\u03bb<sub>2<\/sub>= 1.00088\uff09\uff0cTi<sub>50<\/sub>Ni<sub>40.75<\/sub>Pd<sub>9.25<\/sub>\uff08\u03bb<sub>2<\/sub>= 1.0002\uff09\uff0cTi<sub>54<\/sub>Ni<sub>34<\/sub>Cu<sub>12<\/sub>\uff08\u03bb<sub>2<\/sub>= 0.9905\uff09\uff0cTi<sub>79<\/sub>Nb<sub>21<\/sub>\uff08\u03bb<sub>2<\/sub>= 1\uff09\u548cTi<sub>79<\/sub>Ta<sub>21<\/sub>\uff08\u03bb<sub>2<\/sub>= 1\uff09\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 4 <\/strong><strong>\u65bd\u5bc6\u5fb7\u5b9a\u5f8b\u7684\u6700\u5927\u5e94\u53d8\u7684\u6781\u5750\u6807\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153657\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/4-24.jpg\" alt=\"\" width=\"600\" height=\"208\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/4-24.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/4-24-300x104.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u9a6c\u6c0f\u4f53\u6676\u4f53\u5b66\u7406\u8bba\u7684\u7ecf\u5178\u89e3\u91ca\uff1b<\/p>\n<p>\uff08b\uff09\u8f85\u56e0\u5b50\u6761\u4ef6\u4e0b\u53ef\u80fd\u7684\u7194\u6db2\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 5 <\/strong><strong>\u5728<\/strong><strong>1000<\/strong><strong>\u4e07\u6b21\u62c9\u4f38\u5faa\u73af\u5185\uff0c<\/strong><strong>Ti<sub>54.7<\/sub>Ni<sub>30.7<\/sub>Cu<sub>12.3<\/sub>Co<sub>2.3<\/sub><\/strong><strong>\u8584\u819c\u7684\u9ad8\u5468\u75b2\u52b3\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153656\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/5-19.jpg\" alt=\"\" width=\"600\" height=\"461\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/5-19.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/5-19-300x231.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong> 6 <\/strong><strong>\u76f4\u5f84\u4e3a<\/strong><strong>2 \u03bcm<\/strong><strong>\u7684<\/strong><strong>Zn<sub>45<\/sub>Au<sub>30<\/sub>Cu<sub>25<\/sub><\/strong><strong>\u5408\u91d1\u7684\u5faa\u73af\u538b\u7f29\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153655\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/6-15.jpg\" alt=\"\" width=\"600\" height=\"337\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/6-15.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/6-15-300x169.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong> 7 <\/strong><strong>\u4e0d\u540c\u7ed3\u6676\u6761\u4ef6\u4e0b\uff0c<\/strong><strong>Ti<sub>50.8<\/sub>Ni<sub>34.2<\/sub>Cu<sub>12.5<\/sub>Co<sub>2.5<\/sub><\/strong><strong>\u8584\u819c\u7684\u75b2\u52b3\u66f2\u7ebf\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153654\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/7-9.jpg\" alt=\"\" width=\"600\" height=\"238\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/7-9.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/7-9-300x119.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5728700\u2103\u4e0b\uff0c\u7ed3\u667615 min\u7684\u6676\u7c92\u5c3a\u5bf85 \u03bcm\u75b2\u52b3\u66f2\u7ebf\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u5728600\u2103\u4e0b\uff0c\u7ed3\u667615 min\u7684\u6676\u7c92\u5c3a\u5bf8300 nm\u75b2\u52b3\u66f2\u7ebf\u56fe\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong> 8 <\/strong><strong>\u5bcc<\/strong><strong>Ti<\/strong><strong>\u7684<\/strong><strong>TiNiCu<\/strong><strong>\u5408\u91d1\u7684\u7b2c<\/strong><strong>1<\/strong><strong>\u3001<\/strong><strong>200<\/strong><strong>\u548c<\/strong><strong>107<\/strong><strong>\u6b21\u7684\u8d85\u4f4e\u75b2\u52b3\u66f2\u7ebf\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153653\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/8-10.jpg\" alt=\"\" width=\"600\" height=\"452\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/8-10.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/8-10-300x226.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe<\/strong><strong> 9 Ti<sub>53.7<\/sub>Ni<sub>24.6<\/sub>Cu<sub>21.7<\/sub><\/strong><strong>\u8584\u819c\u7684\u5fae\u89c2\u7ed3\u6784\u4e0e\u529f\u80fd\u75b2\u52b3\u7684\u5173\u7cfb\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-153652\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/9-6.jpg\" alt=\"\" width=\"600\" height=\"525\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/9-6.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/09\/9-6-300x263.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5728700\u2103\u4e0b\uff0c\u9000\u706b\u6837\u54c1\u7684TEM\u56fe\u50cf(\u63d2\u56fe\uff1aB19\u76f8\u548c\u6c89\u6dc0\u7269\u7684\u653e\u5927\u56fe)\uff1b<\/p>\n<p>\uff08b\uff09\u5728550\u2103\u4e0b\uff0c\u9000\u706b\u6837\u54c1\u7684TEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08c\uff09\u5728700\u2103\u9000\u706b\u6837\u54c1\u7684200\u6b21\u8d85\u5f39\u6027\u5faa\u73af\u7684\u529f\u80fd\u75b2\u52b3\u56fe\uff1b<\/p>\n<p>\uff08d\uff09\u5728550\u2103\u9000\u706b\u7684\u6837\u54c1\u7684200\u6b21\u8d85\u5f39\u6027\u5faa\u73af\u7684\u529f\u80fd\u75b2\u52b3\u56fe\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u6587\u5217\u51fa\u4e86\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u76f8\u53d8\u53ef\u9006\u6027\u6761\u4ef6\uff1a\u6676\u4f53\u76f8\u5bb9\u6027\uff0c\u6676\u7c92\u5c3a\u5bf8\u548c\u6c89\u6dc0\u3002\u7814\u7a76\u8868\u660e\uff0c\u5982\u679c\u6ee1\u8db3\u8fd9\u4e09\u4e2a\u6761\u4ef6\uff0c\u5c31\u53ef\u80fd\u83b7\u5f97\u6781\u597d\u7684\u6297\u529f\u80fd\u75b2\u52b3\u548c\u4f4e\u6ede\u540e\u6027\u7684\u5408\u91d1\u3002\u7136\u800c\uff0c\u5176\u4e2d\u4e00\u4e2a\u6216\u591a\u4e2a\u6761\u4ef6\u7a0d\u5fae\u6b20\u7f3a\uff0c\u4ecd\u5177\u6709\u663e\u7740\u7684\u529f\u80fd\u75b2\u52b3\u3002\u4f46\u662f\u70ed\u5904\u7406\u5bf9\u8fd9\u51e0\u4e2a\u6761\u4ef6\u6709\u5f88\u5927\u5f71\u54cd\u3002\u867d\u7136\u8fd9\u4e9b\u89c4\u5f8b\u7b26\u5408\u5728\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\uff0c\u4f46\u662f\u8fd9\u4e9b\u6761\u4ef6\u4e3b\u8981\u662f\u51e0\u4f55\u6216\u5f39\u6027\u652f\u914d\uff08\u76f8\u5bb9\u6027\u6761\u4ef6\uff0c\u6676\u7c92\u5c3a\u5bf8\uff0c\u6790\u51fa\u7269\u7684\u76f8\u5e72\u6027\uff09\uff0c\u56e0\u6b64\u9884\u671f\u5b83\u4eec\u5e94\u9002\u7528\u4e8e\u5e7f\u6cdb\u7684\u76f8\u53d8\u3002\u4f46\u662f\u5728\u94c1\u7535\u6216\u94c1\u78c1\u76f8\u53d8\u4e2d\uff0c\u5b58\u5728\u94c1\u7535\/\u94c1\u78c1\u7574\u4ecd\u9700\u8981\u8fdb\u4e00\u6b65\u7814\u7a76\u3002\u672c\u6587\u63d0\u51fa\u4e86\u4e00\u4e9b\u7279\u6b8a\u95ee\u9898\u3002\u5728\u03bb<sub>2<\/sub>= 1\u4e0e\u5b8c\u5168\u8f85\u56e0\u5b50\u6761\u4ef6\u5728\u786e\u5b9a\u6ede\u540e\u548c\u53ef\u9006\u6027\u65b9\u9762\u7684\u76f8\u5bf9\u4f5c\u7528\u3002\u5177\u6709\u76f8\u540c\u5904\u7406\u7684\u7c7b\u4f3c\u5408\u91d1\u7684\u6bd4\u8f83\u7814\u7a76\uff0c\u4e00\u4e2a\u6ee1\u8db3\u9ad8\u7cbe\u5ea6\u03bb<sub>2<\/sub>= 1\u4f46\u8fdc\u4e0d\u6ee1\u8db3CCI = 0\u6216CCII = 0\uff0c\u53e6\u4e00\u4e2a\u6ee1\u8db3\u5b8c\u6574\u8f85\u56e0\u5b50\u6761\u4ef6\uff0c\u5c06\u662f\u6709\u542f\u53d1\u6027\u7684\u3002\u7c7b\u4f3c\u7684\u6bd4\u8f83\u7814\u7a76\u4e5f\u6d89\u53ca\u7c92\u5ea6\u548c\u6c89\u6dc0\u7269\u3002\u867d\u7136\u03bb<sub>2<\/sub>\u5bf9\u70ed\u6ede\u540e\u7684\u5f71\u54cd\u975e\u5e38\u660e\u663e\uff0c\u4f46\u662f\u5e94\u529b\u6ede\u540e\u7684\u56e0\u7d20\u5c1a\u4e0d\u6e05\u695a\u3002\u8fd9\u4e9b\u660e\u663e\u5c0f\u7684\u6ede\u540e\u73b0\u8c61\u4ecd\u5b58\u5728\u5f88\u5927\u5dee\u5f02\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u7ecf\u5178Cu-Al-Ni\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u4e2d\uff0c\u03b21\u2192\u03b21&#8217;\u8f6c\u53d8\u5177\u6709\u975e\u5e38\u5927\u7684\u5e94\u53d8\uff0c\u7ea6\u4e3a10\uff05\uff0c\u5e94\u529b\u6ede\u540e\u7ea6\u4e3a5 MPa\uff0c\u8010\u75b2\u52b3\u6027\u8f83\u5dee\u3002\u5728\u6297\u529f\u80fd\u75b2\u52b3\u6027\u7684\u5408\u91d1\u4e2d\uff0c\u662f\u5426\u4ea7\u751f\u5982\u6b64\u5c0f\u7684\u5e94\u529b\u6ede\u540e\u6548\u5e94\u4ecd\u9700\u8981\u8fdb\u4e00\u6b65\u7814\u7a76\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"https:\/\/www.sciencedirect.com\/science\/article\/pii\/S1369702117305497\" target=\"_blank\" rel=\"noopener\"><strong>Phase engineering and supercompatibility of shape memory alloys<\/strong><\/a>\uff08materials today, 2018, DOI: 10.1016\/j.mattod. 2017.10.002\uff09\u3002<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u91d1\u5c5e\u7f16\u8f91\u90e8\u5f20\u91d1\u6d0b\u7f16\u8bd1\u6574\u7406\u3002<\/p>\n<p><strong>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1a<\/strong><strong>cailiaokefu<\/strong><strong>\u3002<\/strong><\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u8fd1\u5e74\u6765\uff0c\u5177\u6709\u5408\u9002\u6676\u7c92\u5c3a\u5bf8\u76f8\u7684\u8d85\u7ea7\u76f8\u5bb9\u6027\u548c\u6709\u5229\u7684\u6c89\u6dc0\u7269\u9635\u5217\u76f8\u7ed3\u5408\uff0c\u5b9e\u73b0\u4e86\u529f\u80fd\u548c\u7ed3\u6784\u6297\u75b2\u52b3\u6027\u548c\u5f62\u72b6\u8bb0\u5fc6\u5408\u91d1\u7684\u6ede\u540e\u6027\u7684\u964d\u4f4e\u3002\u672c\u6587\u5206\u6790\u548c\u6bd4\u8f83\u8fd9\u4e9b\u4f8b\u5b50\uff0c\u9610\u660e\u8fd9\u4e9b&#8230;<\/p>\n","protected":false},"author":7035,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[533],"tags":[3567,2534,3566],"class_list":["post-153651","post","type-post","status-publish","format-standard","hentry","category-zongshu","tag-3567","tag-2534","tag-3566"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/153651"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7035"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=153651"}],"version-history":[{"count":7,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/153651\/revisions"}],"predecessor-version":[{"id":154154,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/153651\/revisions\/154154"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=153651"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=153651"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=153651"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}