{"id":155704,"date":"2018-10-07T06:30:17","date_gmt":"2018-10-06T22:30:17","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=155704"},"modified":"2018-10-08T00:59:55","modified_gmt":"2018-10-07T16:59:55","slug":"%e7%a7%91%e7%a0%94%e5%b9%b2%e8%b4%a7-xps%e5%b3%b0%e5%bd%a2%e6%8b%9f%e5%90%88","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=155704","title":{"rendered":"\u79d1\u7814\u5e72\u8d27 | XPS\u5cf0\u5f62\u62df\u5408"},"content":{"rendered":"<p>\n X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31\u5206\u6790(X-ray photoelectron spectroscopy, XPS)\u662f\u7528X\u5c04\u7ebf\u53bb\u8f90\u5c04\u6837\u54c1\uff0c\u4f7f\u539f\u5b50\u6216\u5206\u5b50\u7684\u5185\u5c42\u7535\u5b50\u6216\u4ef7\u7535\u5b50\u53d7\u6fc0\u53d1\u8f90\u5c04\u51fa\u6765\u3002<\/p>\n<p>\n XPS\u53ef\u4ee5\u7528\u4e8e\u5143\u7d20\u7684\u5b9a\u6027\u3001\u5b9a\u91cf\u5206\u6790\uff0c\u56fa\u4f53\u8868\u9762\u7684\u5316\u5b66\u7ec4\u6210\u6216\u5143\u7d20\u7ec4\u6210\uff0c\u539f\u5b50\u4ef7\u6001\uff0c\u8868\u9762\u80fd\u6001\u5206\u5e03\uff0c\u6d4b\u5b9a\u8868\u9762\u7535\u5b50\u7684\u7535\u5b50\u4e91\u5206\u5e03\u548c\u80fd\u7ea7\u7ed3\u6784\u7b49\u3002<\/p>\n<p>\n \u5728\u65e0\u673a\u975e\u91d1\u5c5e\u9886\u57df\uff0cXPS\u6700\u5e38\u89c1\u7684\u7528\u9014\u662f\u4ef7\u6001\u7814\u7a76\u3002\u6839\u636e\u539f\u5b50\u5468\u56f4\u7684\u5316\u5b66\u73af\u5883\u5dee\u5f02\uff0c\u5149\u7535\u5b50\u5cf0\u4f4d\u7f6e\u5728\u5355\u8d28\u548c\u4e0d\u540c\u5316\u5408\u7269\u4e2d\u4f1a\u4e0d\u4e00\u6837\uff0c\u76f8\u4e92\u4e4b\u95f4\u7684\u80fd\u91cf\u5dee\u53ef\u4ee5\u4e3a\u96f6\u70b9\u51e0\u5230\u5341\u51e0\u7535\u5b50\u4f0f\u7279\uff0c\u8fd9\u6b63\u662f\u5149\u7535\u5b50\u80fd\u8c31\u7528\u4e8e\u7814\u7a76\u539f\u5b50\u4ef7\u6001\u7684\u4f9d\u636e\u3002<\/p>\n<p>\n \u53ef\u662f\u6211\u4eec\u7ecf\u5e38\u6d4b\u8bd5\u5b8c\u4e4b\u540e\uff0c\u5f97\u5230\u7684\u90fd\u662fexcel\u6570\u636e\uff0c\u81f3\u591a\u518d\u7ed9\u6211\u4eec\u4e00\u4e2a\u4e0d\u80fd\u7f16\u8f91\u7684\u7ed3\u5408\u80fd\u8c31\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155707 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72471-1.png\" alt=\"\" width=\"444\" height=\"389\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72471-1.png 444w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72471-1-300x263.png 300w\" sizes=\"(max-width: 444px) 100vw, 444px\" \/><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155706 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72472.png\" alt=\"\" width=\"444\" height=\"392\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72472.png 444w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72472-300x265.png 300w\" sizes=\"(max-width: 444px) 100vw, 444px\" \/><br \/>\n \u5168\u8c31\u4e00\u822c\u4e0d\u7528\u62df\u5408\uff0c\u76f4\u63a5\u62ff\u539f\u59cb\u6570\u636e\u5728origin\u4e2d\u7ed8\u56fe\u5373\u53ef\uff1b\u4f46\u5355\u5143\u7d20\u7684\u7279\u5f81\u80fd\u8c31\u76f4\u63a5\u7ed8\u5236\u56fe\u8c31\u5c31\u6709\u70b9\u7c97\u7cd9\uff0c\u5fc5\u987b\u8fdb\u884c\u62df\u5408\u624d\u80fd\u7528\u4e8ePPT\u548c\u53d1\u6587\u7ae0\u3002\u4e5f\u5c31\u9700\u8981\u6211\u4eec\u5bf9\u539f\u59cb\u7684excel\u6570\u636e\u8fdb\u884c\u62df\u5408\uff0c\u518d\u548c\u62df\u5408\u4e4b\u540e\u7684\u6570\u636e\u4e00\u8d77\u7ed8\u5236\u9700\u8981\u7684\u56fe\u8c31\u3002\u5f88\u591a\u521a\u63a5\u89e6XPS\u7684\u540c\u5b66\u90fd\u4e0d\u4f1aXPS\u5cf0\u5f62\u62df\u5408\uff0c\u4eca\u5929\u5c31\u6559\u5927\u5bb6\u62df\u5408\u7684\u57fa\u672c\u6d41\u7a0b\u548c\u5177\u4f53\u64cd\u4f5c\u3002<\/p>\n<p>\n \u4e00\u3001\u5fc5\u5907\u8f6f\u4ef6\uff1aXPSPEAK41<\/p>\n<p>\n \u4e8c\u3001\u51c6\u5907\u6570\u636e\uff1a.xls\u6216\u8005.txt\u6216.dat\u683c\u5f0f\u7684XPS\u6570\u636e<\/p>\n<p>\n \u4e09\u3001\u62df\u5408\u5f00\u59cb\uff1a<br \/>\n 1.\u5c06\u9700\u8981\u7ed8\u56fe\u7684\u4e24\u5217\u6570\u636e\u590d\u5236\u51fa\u6765\uff0c\u4fdd\u5b58\u4e3a.dat\u683c\u5f0f\u7684\u6570\u636e\u3002<\/p>\n<p>\n 2.\u6253\u5f00XPSPEAK41\u8f6f\u4ef6\uff0c\u5de6\u51fb\u201cData\u201d\u2192\u201cImport(ASCII)\u201d\u2192\u9009\u62e9\u6539\u597d\u683c\u5f0f\u7684.dat\u6570\u636e\uff0c\u6253\u5f00\uff0c\u51fa\u73b0\u56fe\u8c31\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155708 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72473.png\" alt=\"\" width=\"650\" height=\"390\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72473.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72473-300x180.png 300w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/p>\n<p>&nbsp;<\/p>\n<p>3.\u70b9\u51fb\u201cBack ground\u201d\uff0c\u5f39\u51fa\u80cc\u666f\u9009\u62e9\u5bf9\u8bdd\u6846\uff0c\u6839\u636e\u5143\u7d20\u7ed3\u5408\u80fd\u7684\u5cf0\u4f4d\u7f6e\uff0c\u9009\u62e9 \u201cHigh BE\u201d\u201cLow BE\u201d\u7684\u6570\u503c\uff0c\u70b9\u51fb\u201cAccept\u201d\u3002\u53ef\u4ee5\u5bf9\u9ad8\u5e95\u201cBE\u201d\u8fdb\u884c\u5fae\u8c03\uff0c\u81f3\u80cc\u5e95\u5904\u4e8e\u5408\u9002\u7684\u4f4d\u7f6e\u3002<br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155709 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72474.png\" alt=\"\" width=\"650\" height=\"281\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72474.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72474-300x130.png 300w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/p>\n<p>4.\u70b9\u51fb\u201cAdd Peak\u201d\uff0c\u51fa\u73b0\u4e00\u4e2a\u5cf0\u4f4d\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155710 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72475.png\" alt=\"\" width=\"650\" height=\"381\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72475.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72475-300x176.png 300w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><br \/>\n 5.\u901a\u8fc7\u624b\u52a8\u8c03\u8282\u5cf0\u4f4d\u201dPosition\u201d\u3001\u534a\u5cf0\u5bbd\u201dFWHM\u201d\u3001\u5cf0\u9762\u79ef\u201dArea\u201d\uff0c\u6bcf\u4e2a\u540e\u9762\u90fd\u6709\u201dFix\u201d\uff0c\u53ef\u6839\u636e\u9700\u8981\u9009\u4e2d\u56fa\u5b9a\uff0c\u5148\u70b9\u51fb\u540e\u9762\u5bf9\u5e94\u7684\u201cOptimise\u201d\u8fdb\u884c\u62df\u5408\uff0c\u518d\u70b9\u51fb\u201cOptimise Peak\u201d\uff0c\u8fdb\u884c\u62df\u5408\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155711 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72476.png\" alt=\"\" width=\"352\" height=\"711\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72476.png 352w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72476-149x300.png 149w\" sizes=\"(max-width: 352px) 100vw, 352px\" \/><\/p>\n<p> 6.\u5982\u679c\u4e00\u4e2a\u5cf0\u62df\u5408\u7684\u5dee\u4e0d\u591a\u4e86\uff0c\u4f46\u8fd8\u6709\u90e8\u5206\u4e5f\u53ef\u80fd\u6709\u5cf0\u9700\u8981\u62df\u5408\uff0c\u518d\u70b9\u51fb\u201cAdd Peak\u201d\uff0c\u589e\u52a0\u4e00\u4e2a\u5cf0\uff0c\u6b64\u65f6\u201cXPS Peak Processing\u201d\u9762\u677f\u4f1a\u51fa\u73b0\u4e24\u4e2a\u5cf0\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155712 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72477.png\" alt=\"\" width=\"619\" height=\"425\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72477.png 619w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72477-300x206.png 300w\" sizes=\"(max-width: 619px) 100vw, 619px\" \/><\/p>\n<p> 7.\u5982\u679c\u62df\u5408\u8fc7\u7a0b\u4e2d\u591a\u52a0\u4e86\u4e00\u4e2a\u5cf0\uff0c\u5728\u201cXPS Peak Processing\u201d\u9762\u677f\u9009\u4e2d\u591a\u52a0\u7684\u5cf0\uff0c\u201cDelete\u201d\u5373\u53ef\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155713 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72478.png\" alt=\"\" width=\"346\" height=\"706\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72478.png 346w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72478-147x300.png 147w\" sizes=\"(max-width: 346px) 100vw, 346px\" \/><\/p>\n<p> 8.\u62df\u5408\u54ea\u4e2a\u5cf0\u5c31\u70b9\u51fb\u90a3\u4e2a\uff0c\u91cd\u590d\u6b65\u9aa45\u30016\u8fdb\u884c\u62df\u5408\u3002\u8fbe\u5230\u81ea\u5df1\u7684\u9884\u671f\u5cf0\u5f62\u4e4b\u540e\uff0c\u70b9\u51fb\u201cOptimise All\u201d\uff0c\u51e0\u4e2a\u5cf0\u4e00\u8d77\u62df\u5408\uff0c\u81f3\u03c72\u51cf\u5c0f\u4e0d\u53d8\u3002\u62df\u5408\u5b8c\u6bd5\uff08\u62df\u5408\u5b8c\u6bd5\u4e4b\u540e\uff0c\u8bb0\u4e0b\u62df\u5408\u7684\u5cf0\u4f4d\u7f6e\uff0c\u4fbf\u4e8e\u5728Origin\u4e2d\u7ed8\u56fe\u65f6\u6807\u6ce8\uff09\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155714 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72479.png\" alt=\"\" width=\"607\" height=\"419\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72479.png 607w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u72479-300x207.png 300w\" sizes=\"(max-width: 607px) 100vw, 607px\" \/><\/p>\n<p> 9.\u4e3a\u4e86\u65b9\u4fbf\u540e\u9762\u76f4\u63a5\u4fee\u6539\u62df\u5408\u7684\u56fe\u8c31\uff0c\u53ef\u4ee5\u5728XPS Peak Processing\u201d\u9762\u677f\u4e2d\u201cSave XPS\u201d\uff0c\u8fdb\u884c\u4fdd\u5b58\uff0c\u540e\u9762\u9700\u8981\u4fee\u6539\u53ef\u76f4\u63a5\u6253\u5f00\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-155715 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u724710.png\" alt=\"\" width=\"438\" height=\"301\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u724710.png 438w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/\u56fe\u724710-300x206.png 300w\" sizes=\"(max-width: 438px) 100vw, 438px\" \/><\/p>\n<p> \u56db\u3001\u6570\u636e\u5bfc\u51fa\u53ca\u7ed8\u56fe\uff1a<\/p>\n<p>\n \u62df\u5408\u5b8c\u6bd5\u540e\uff0c\u56de\u5230\u201cRegion\u201d\u9762\u677f\uff0c\u70b9\u51fb\u201cData\u201d\u2192\u201cExport Spectrum\u201d \u2192\u4fdd\u5b58.dat\u6570\u636e\u6587\u4ef6\u3002<\/p>\n<p>\n \u6253\u5f00\u8f93\u51fa\u7684.dat\u6570\u636e\uff0c\u6309\u9700\u8981\u9009\u62e9\u9700\u8981\u7684\u5217\u6570\uff0c\u590d\u5236\u540e\u5728Origin\u4e2d\u7ed8\u56fe\uff0c\u6807\u6ce8\u7279\u5f81\u5cf0\u5bf9\u5e94\u7684\u7ed3\u5408\u80fd\u3002<\/p>\n<p>\n \u62df\u5408\u5230\u6b64\u5c31\u5927\u529f\u544a\u6210\u5566\uff01\u5b70\u80fd\u751f\u5de7\uff0c\u5feb\u5feb\u8ddf\u7740\u6559\u7a0b\u8fde\u8d77\u6765\u5427\uff01<\/p>\n<p>&nbsp;<\/p>\n<p>\u672c\u6587\u7531\u5317\u4eac\u79d1\u6280\u5927\u5b66\u96e8\u7530\u4f9b\u7a3f\uff0c\u7f16\u8f91\u90e8\u6574\u7406\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1\uff1a<strong>tougao@cailiaoren.com<\/strong>\u3002<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1a<strong>cailiaokefu<\/strong>\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31\u5206\u6790(X-ray photoelectron spectroscopy, XPS)\u662f\u7528X\u5c04\u7ebf\u53bb\u8f90\u5c04\u6837\u54c1\uff0c\u4f7f\u539f\u5b50\u6216\u5206\u5b50\u7684\u5185\u5c42\u7535\u5b50\u6216\u4ef7\u7535\u5b50\u53d7\u6fc0\u53d1\u8f90\u5c04&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[],"class_list":["post-155704","post","type-post","status-publish","format-standard","hentry","category-ganhuo"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/155704"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=155704"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/155704\/revisions"}],"predecessor-version":[{"id":155720,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/155704\/revisions\/155720"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=155704"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=155704"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=155704"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}