{"id":156058,"date":"2018-10-13T06:30:25","date_gmt":"2018-10-12T22:30:25","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=156058"},"modified":"2018-10-12T16:58:41","modified_gmt":"2018-10-12T08:58:41","slug":"acta-materialia%ef%bc%9a%e9%87%91%e5%b1%9e%e7%8e%bb%e7%92%83%e4%b8%ad%e7%bc%ba%e9%99%b7%e5%af%86%e5%ba%a6%e5%92%8c%e6%9c%ac%e5%be%81%e7%bb%93%e6%9e%84%e5%9c%a8%e5%8a%bf%e8%83%bd%e5%9b%be%e6%99%af","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=156058","title":{"rendered":"Acta Materialia\uff1a\u91d1\u5c5e\u73bb\u7483\u4e2d\u7f3a\u9677\u5bc6\u5ea6\u548c\u672c\u5f81\u7ed3\u6784\u5728\u52bf\u80fd\u56fe\u666f\u4e2d\u5206\u5e03\u7684\u5173\u8054"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u7406\u89e3\u6750\u6599\u7684\u7ed3\u6784\u53ca\u5176\u5bf9\u5916\u754c\u523a\u6fc0\u7684\u54cd\u5e94\u81f3\u5173\u91cd\u8981\uff0c\u5176\u5bf9\u4e8e\u5f3a\u5ea6\u3001\u97e7\u6027\u548c\u5931\u6548\u7b49\u4e34\u754c\u529b\u5b66\u6027\u80fd\u8d77\u7740\u51b3\u5b9a\u6027\u4f5c\u7528\u3002\u5728\u975e\u6676\u6001\u6750\u6599\u4e2d\uff0c\u7531\u4e8e\u5176\u65e0\u5e8f\u539f\u5b50\u672c\u8d28\u548c\u70b9\u9635\u5468\u671f\u6027\u6d88\u5931\uff0c\u7ed3\u6784-\u6027\u80fd\u5173\u7cfb\u5f88\u96be\u6e05\u6670\u5b9a\u4e49\uff0c\u7814\u7a76\u4eba\u5458\u666e\u904d\u8ba4\u4e3a\u5728\u975e\u6676\u6001\u6750\u6599\u4e2d\u5b58\u5728\u7740\u4e00\u4e9b\u666e\u9002\u7684\u5f62\u53d8\u5355\u5143\u3002\u8fd1\u671f\u5b9e\u9a8c\u548c\u6a21\u62df\u4e5f\u53d1\u73b0\u5355\u4e2a\u5f62\u53d8\u5355\u5143\u7684\u6027\u8d28\u662f\u4e0d\u53d8\u91cf\uff0c\u800c\u5f62\u53d8\u5355\u5143\u7684\u5bc6\u5ea6\u548c\u5206\u5e03\u4e0e\u5236\u5907\u5386\u53f2\u3001\u5f1b\u8c6b\u7a0b\u5ea6\u606f\u606f\u76f8\u5173\u3002\u7136\u800c\uff0c\u7531\u4e8e\u975e\u6676\u6001\u6750\u6599\u7684\u65e0\u5e8f\u539f\u5b50\u5806\u579b\u65b9\u5f0f\uff0c\u4f7f\u5f97\u5173\u4e8e\u5916\u754c\u73af\u5883\u5bf9\u7ed3\u6784\u53d8\u91cf\u5f71\u54cd\u7684\u5b9a\u91cf\u5316\u7814\u7a76\u53d8\u5f97\u5c24\u4e3a\u56f0\u96be\u3002\u539f\u5b50\u95f4\u7684\u76f8\u4e92\u4f5c\u7528\u52bf\u901a\u5e38\u662f\u539f\u5b50\u95f4\u76f8\u5bf9\u4f4d\u7f6e\u7684\u51fd\u6570\uff0c\u800c\u6574\u4e2a\u4f53\u7cfb\u7684\u52bf\u80fd\u4f1a\u5728\u9ad8\u7ef4\u6784\u578b\u7a7a\u95f4\u5f62\u6210\u4e00\u4e2a\u590d\u6742\u8868\u9762\uff0c\u8fd9\u5c31\u662f\u52bf\u80fd\u56fe\u666f\uff08potential energy landscape\uff09\u3002\u65e0\u5e8f\u6750\u6599\u7684\u52bf\u80fd\u56fe\u666f\u5177\u6709\u5f88\u591a\u7684\u5c40\u57df\u80fd\u91cf\u6781\u5c0f\u503c\uff0c\u5373\u672c\u5f81\u7ed3\u6784\uff08inherent structure\uff09\uff0c\u4ee3\u8868\u7cfb\u7edf\u4e2d\u4e00\u4e9b\u4e9a\u7a33\u6001\u3002\u4ece\u52bf\u80fd\u56fe\u666f\u7684\u89d2\u5ea6\u6765\u770b\uff0c\u975e\u6676\u56fa\u4f53\u4e2d\u7684\u5f62\u53d8\u5355\u5143\u5bf9\u5e94\u7740\u76f8\u90bb\u7684\u672c\u5f81\u7ed3\u6784\u4e4b\u95f4\u7684\u8df3\u8dc3(hopping)\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u7f8e\u56fd\u5bc6\u6b47\u6839\u5927\u5b66<\/strong>\u7684<strong>\u8303\u60a6\u6559\u6388<\/strong>\uff08<strong>\u901a\u8baf\u4f5c\u8005<\/strong>\uff09\u548c<strong>\u5317\u4eac\u8ba1\u7b97\u79d1\u5b66\u7814\u7a76\u4e2d\u5fc3<\/strong>\u7684<strong>\u7ba1\u9e4f\u98de\u7814\u7a76\u5458<\/strong>\u5408\u4f5c\uff0c\u5c31\u52bf\u80fd\u56fe\u666f\u4e2d\u672c\u5f81\u7ed3\u6784\u7684\u5b9a\u91cf\u5316\u8fd9\u4e00\u95ee\u9898\uff0c\u5728Acta Materialia\u4e0a\u53d1\u8868\u4e86\u9898\u4e3a\u201cCorrelating defects density in metallic glasses with the distribution of inherent structures in potential energy landscape\u201d\u7684\u6587\u7ae0\u3002\u5bf9\u975e\u6676\u5408\u91d1\u6a21\u578b\u4f53\u7cfb\u8fdb\u884c\u76f8\u5dee\u4e94\u4e2a\u6570\u91cf\u7ea7\u7684\u4e0d\u540c\u51b7\u5374\u5904\u7406\uff0c\u7814\u7a76\u52bf\u80fd\u56fe\u666f\u7684\u7ed3\u6784\u6f14\u5316\u3002\u52bf\u80fd\u56fe\u666f\u4e2d\u7684\u5c40\u57df\u6781\u5c0f\u503c\u5728\u8f83\u4f4e\u7684\u865a\u62df\u6e29\u5ea6\uff08fictive temperature\uff09T<sub>fic<\/sub>\u4e0b\uff0c\u5206\u5e03\u66f4\u4e3a\u7a00\u758f\uff1b\u5c40\u57df\u6781\u5c0f\u503c\u5bc6\u5ea6\u548c\u865a\u62df\u6e29\u5ea6\u4e4b\u95f4\u5b58\u5728Arrhenuis\u5173\u7cfb\u3002\u8fd9\u6837\u5c31\u5c06\u52bf\u80fd\u56fe\u666f\u4e2d\u672c\u5f81\u7ed3\u6784\u5206\u5e03\u548c\u975e\u6676\u6001\u56fa\u4f53\u7684\u526a\u5207\u8f6c\u53d8\u533a\u7684\u5bc6\u5ea6\u8054\u7cfb\u8d77\u6765\u3002\u6b64\u5916\uff0cArrhenius\u5173\u7cfb\u57281.3-1.4T<sub>g<\/sub>\u65f6\u5931\u6548\uff1a\u5728\u66f4\u9ad8\u6e29\u5ea6\u4e0b\uff0c\u5c40\u57df\u6781\u5c0f\u503c\u5bc6\u5ea6\u8fbe\u5230\u9971\u548c\u3002\u8be5\u4e34\u754c\u6e29\u5ea6\u4e0e\u5b9e\u9a8c\u89c2\u5bdf\u5230\u7684\u52a8\u529b\u5b66\u8f6c\u6298\u6e29\u5ea6\u76f8\u7b26\u5408\uff0c\u8868\u660e\u52bf\u80fd\u56fe\u666f\u7ed3\u6784\u548c\u975e\u6676\u6001\u4f53\u7cfb\u7684\u52a8\u529b\u5b66\u5b58\u5728\u5bc6\u5207\u5173\u8054\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u56fe1\uff1a\u65e0\u5e8f\u4f53\u7cfb\u7684\u52bf\u80fd\u56fe\u666f\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-156059\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/1-4.png\" alt=\"\" width=\"600\" height=\"277\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/1-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/1-4-300x139.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u542b\u6709N\u4e2a\u539f\u5b50\u7684\u65e0\u5e8f\u7cfb\u7edf\u7684\u52bf\u80fd\u56fe\u666f\uff0c\u662f\u4e00\u4e2a\u5305\u542b\u8bb8\u591a\u4e0d\u540c\u672c\u5f81\u7ed3\u6784\u7684\u591a\u7ef4\u7ed3\u6784\uff1b<\/p>\n<p>(b) \u591a\u7ef4\u52bf\u80fd\u56fe\u666f\u4e0a\u672c\u5f81\u7ed3\u6784\u5448\u73b0\u4e0d\u5747\u5300\u5206\u5e03\uff1b<\/p>\n<p>(c) \u9ad8\u80fd\u7ea7\u5904\uff0c\u5c40\u57df\u6781\u5c0f\u503c\u7684\u5bc6\u5ea6\u66f4\u5927\uff0c\u76f8\u90bb\u672c\u5f81\u7ed3\u6784\u4e4b\u95f4\u7684\u6fc0\u6d3b\u80fd\u5792\u66f4\u5c0f\uff0c\u800c\u4f4e\u80fd\u7ea7\u5904\uff0c\u5c40\u57df\u6781\u5c0f\u503c\u7684\u5bc6\u5ea6\u66f4\u5c0f\uff0c\u6fc0\u6d3b\u80fd\u5792\u66f4\u5927\u3002<\/p>\n<p>\u56fe2\uff1a\u4e0d\u540c\u51b7\u5374\u901f\u7387\u4e0b\uff0c\u4f53\u7cfb\u4e2d\u5355\u4e2a\u539f\u5b50\u7684\u672c\u5f81\u7ed3\u6784\u80fd\u91cfE<sub>IS<\/sub>\u7684\u53d8\u5316\u60c5\u51b5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-156060\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/2-6.png\" alt=\"\" width=\"600\" height=\"438\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/2-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/2-6-300x219.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe3\uff1a\u5355\u539f\u5b50\u7684\u5e73\u5747\u6fc0\u6d3b\u80fd\u3001\u672c\u5f81\u7ed3\u6784\u80fd\u548c\u6e29\u5ea6\u4e4b\u95f4\u7684\u5173\u8054\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-156061\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/3-6.png\" alt=\"\" width=\"600\" height=\"607\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/3-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/3-6-297x300.png 297w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u52bf\u80fd\u56fe\u666f\u4e2d\u4ece\u5c40\u57df\u6781\u5c0f\u503c\u5230\u8fd1\u90bb\u978d\u70b9\u6001\u7684\u6fc0\u6d3b\u80fd\u548c\u6700\u5927\u539f\u5b50\u4f4d\u79fb\u4e4b\u95f4\u7684\u5173\u7cfb\uff1b<\/p>\n<p>(b)\u4e00\u4e2a\u672c\u5f81\u7ed3\u6784\u80fd\u91cf\u3001\u5047\u60f3\u6e29\u5ea6\u548c\u5e73\u5747\u6fc0\u6d3b\u80fd\u4e4b\u95f4\u5173\u8054\u7684\u4e09\u7ef4\u89c6\u89d2\u3002<\/p>\n<p>\u56fe4\uff1a10<sup>13<\/sup>K\/s\u81f310<sup>9<\/sup>K\/s\u4e0d\u540c\u51b7\u5374\u901f\u7387\u4e0b\uff0c\u52bf\u80fd\u56fe\u666f\u4e2d\u4ece\u5c40\u57df\u6781\u5c0f\u503c\u5230\u8fd1\u90bb\u978d\u70b9\u6001\u7684\u6700\u5927\u539f\u5b50\u4f4d\u79fb\u7684\u5206\u5e03\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-156062\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/4-7.png\" alt=\"\" width=\"600\" height=\"487\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/4-7.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/4-7-300x244.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe5\uff1a\u5c40\u57df\u52bf\u80fd\u56fe\u666f\u6781\u5c0f\u503c\u76f8\u5bf9\u5bc6\u5ea6\u548c\u5047\u60f3\u6e29\u5ea6\u4e4b\u95f4\u7684\u5173\u7cfb\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-156063\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/5-1.png\" alt=\"\" width=\"600\" height=\"640\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/5-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/5-1-281x300.png 281w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe6\uff1a\u56fa\u5b9a\u4f53\u79ef\u548c\u56fa\u5b9a\u538b\u5f3a\u7684\u7ed3\u679c\u7684\u6bd4\u8f83\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-156064\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/6-1.png\" alt=\"\" width=\"600\" height=\"719\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/6-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/10\/6-1-250x300.png 250w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u8be5\u5de5\u4f5c\u4e2d\uff0c\u5c40\u57df\u52bf\u80fd\u56fe\u666f\u4e2d\u6781\u5c0f\u503c\u5bc6\u5ea6\u662f\u57fa\u4e8e\u5e73\u5747\u6700\u5927\u539f\u5b50\u4f4d\u79fb\u8ba1\u7b97\u7684\uff0c\u7136\u800c\uff0c\u539f\u5b50\u4f4d\u79fb\u8868\u73b0\u51fa\u8f83\u5bbd\u7684\u5206\u5e03\uff0c\u8fd9\u662f\u975e\u6676\u6001\u6750\u6599\u672c\u5f81\u65e0\u5e8f\u7684\u5fc5\u7136\u8868\u73b0\u3002\u6240\u6709\u7684\u975e\u6676\u73bb\u7483\u7ed3\u6784\u53c2\u91cf\u90fd\u5448\u5bbd\u4e14\u8fde\u7eed\u7684\u5206\u5e03\uff0c\u8fd9\u548c\u6676\u4f53\u4e2d\u7f3a\u9677\u7684\u62d3\u6251\u7ed3\u6784\u6709\u7740\u9c9c\u660e\u7684\u53cd\u5dee\u3002\u9274\u4e8e\u8fd9\u79cd\u5185\u79c9\u968f\u673a\u6027\uff0c\u5728\u975e\u6676\u6750\u6599\u4e2d\u6240\u5f97\u7684\u7ed3\u679c\u5e94\u8be5\u5728\u7edf\u8ba1\u5b66\u610f\u4e49\u4e0b\u7406\u89e3\u3002\u503c\u5f97\u5f3a\u8c03\u7684\u662f\uff0c\u8be5\u5de5\u4f5c\u4e2d\u89c2\u5bdf\u5230\u7684Arrhenius\u5173\u7cfb\u4e0eFalk\u548cLanger\u7684\u526a\u5207\u8f6c\u53d8\u533a\u5bc6\u5ea6\u5047\u8bf4\u543b\u5408\u5f97\u5f88\u597d\uff0c\u4ece\u800c\u4ece\u52bf\u80fd\u56fe\u666f\u7684\u89d2\u5ea6\u8d4b\u4e88\u4e86\u73bb\u7483\u4f53\u4e2d\u5f62\u53d8\u5355\u5143\u66f4\u6df1\u5c42\u6b21\u7684\u9610\u91ca\u3002\u53e6\u5916\uff0c\u8be5\u5de5\u4f5c\u53d1\u73b0\u57281.3-1.4T<sub>g<\/sub>\u9644\u8fd1\u7684\u4e34\u754c\u6e29\u5ea6\u5931\u6548\uff1a\u5728\u66f4\u9ad8\u6e29\u5ea6\u4e0b\u5c40\u57df\u6781\u5c0f\u503c\u5bc6\u5ea6\u8fbe\u5230\u9971\u548c\uff0c\u8fd9\u4e0e\u6700\u8fd1\u7684\u60ac\u6d6e\u6563\u5c04\u5b9e\u9a8c\u6240\u89c2\u6d4b\u5230\u7684\u52a8\u529b\u5b66\u8f6c\u6298\u6e29\u5ea6\u76f8\u7b26\u5408\u3002\u8fd9\u8868\u660e\u52bf\u80fd\u56fe\u666f\u5c06\u6210\u4e3a\u6709\u6548\u63cf\u8ff0\u975e\u6676\u6001\u6750\u6599\u6027\u80fd\u7684\u5b9a\u91cf\u5de5\u5177\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5<\/strong>\uff1a<a href=\"https:\/\/www.sciencedirect.com\/science\/article\/pii\/S1359645418307250\" target=\"_blank\" rel=\"noopener\">Correlating Defects Density in Metallic Glasses with the Distribution of Inherent<\/a><\/p>\n<p><a href=\"https:\/\/www.sciencedirect.com\/science\/article\/pii\/S1359645418307250\">Structures in Potential Energy Landscape<\/a>\uff08Acta Mater.,2018,DOI: 10.1016\/j.actamat.2018.09.021\uff09<\/p>\n<p><strong>\u3010\u56e2\u961f\u4ecb\u7ecd\u3011<\/strong><\/p>\n<p><strong>\u8303\u60a6\uff1a<\/strong><\/p>\n<h5 style=\"text-align: left;\"><strong>A. Education and training<\/strong><\/h5>\n<table style=\"width: 716px; height: 188px;\">\n<tbody>\n<tr>\n<td style=\"width: 316px; text-align: center;\"><strong><u>College\/University<\/u><\/strong><\/td>\n<td style=\"width: 282px; text-align: center;\"><strong>\u00a0<u>Field<\/u><\/strong><\/td>\n<td style=\"width: 150px; text-align: center;\"><strong>\u00a0<\/strong><strong>\u00a0<u>Degree &amp; Year<\/u><\/strong><\/td>\n<\/tr>\n<tr>\n<td style=\"width: 316px; text-align: center;\">Peking University<\/td>\n<td style=\"width: 282px; text-align: center;\">Physics\u00a0<\/td>\n<td style=\"width: 150px; text-align: center;\">\u00a0B.S., 2008<\/td>\n<\/tr>\n<tr>\n<td style=\"width: 316px; text-align: center;\">Massachusetts Institute of Technology\u00a0<\/td>\n<td style=\"width: 282px; text-align: center;\">\u00a0Nuclear Science and Engineering<\/td>\n<td style=\"width: 150px; text-align: center;\">\u00a0 \u00a0Ph.D., 2013<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<h5><strong>b. Professional experience<\/strong><\/h5>\n<p>2017-present:\u00a0\u00a0\u00a0 Assistant Professor of Mechanical Engineering, University of Michigan<\/p>\n<p>2013-2016:\u00a0\u00a0\u00a0\u00a0\u00a0 Eugene P. Wigner Fellow\/Staff Scientist, Materials Science and Technology Division, Oak Ridge National Lab<\/p>\n<h5><strong>C. Selected honors and awards<\/strong><\/h5>\n<ul>\n<li>\u201c<strong>Haythornthwaite Young Investigator Award<\/strong>\u201d Nov 2017, from American Society of Mechanical Engineers (ASME) Applied Mechanics Division (AMD);<\/li>\n<li>\u201c<strong>Ralph E. Powe Junior Faculty Enhancement Award<\/strong>\u201d June 2017, from Oak Ridge Associated Universities (ORAU);<\/li>\n<li>&#8220;<strong>Manson Benedict Award<\/strong>&#8221; May 2013, from MIT;<\/li>\n<li>&#8220;<strong>Eugene P. Wigner Fellowship<\/strong>&#8221; Jan 2013, from Oak Ridge National Lab;<\/li>\n<li>\u201c<strong>Aneesur Rahman Postdoctoral Fellowship<\/strong>\u201d Dec 2012, from Argonne National Lab;<\/li>\n<li><em>Declined due to the conflict with Eugene P. Wigner Fellowship<\/em><\/li>\n<li>\u201c<strong>Young Scientist Best Presentation Award<\/strong>\u201d Oct 2010, from the Nuclear Materials Conference;<\/li>\n<\/ul>\n<h5><strong>D<\/strong><strong>. Related publications<\/strong><\/h5>\n<ul>\n<li>Yue Fan*, Takuya Iwashita, and Takeshi Egami. \u201cEnergy landscape-driven nonequilibrium evolution of inherent structure in disordered material\u201d, <em><u>Nature Communications<\/u><\/em> 8, 15417 (2017)<\/li>\n<li>Yue Fan*, Takuya Iwashita, and Takeshi Egami. \u201cCrossover from localized to cascade relaxations in metallic glasses\u201d, <em><u> Rev. Lett.<\/u><\/em> 115, 045501 (2015)<\/li>\n<li>Yue Fan*, Takuya Iwashita, and Takeshi Egami. \u201cHow thermally activated deformation starts in metallic glass\u201d, <em><u>Nature Communications<\/u><\/em> 5, 5083 (2014)<\/li>\n<\/ul>\n<p><strong>\u7ba1\u9e4f\u98de<\/strong><\/p>\n<p><strong>\u7b80\u4ecb<\/strong><strong>\uff1a<\/strong><\/p>\n<p>\u00a0\u00a0\u00a0 2013\u5e74\u5165\u9009\u4e2d\u7ec4\u90e8\u201c\u9752\u5e74\u5343\u4eba\u201d\u30022014\u5e741\u6708\u52a0\u5165\u5317\u4eac\u8ba1\u7b97\u79d1\u5b66\u7814\u7a76\u4e2d\u5fc3\u30022016\u5e74\u8d77\u62c5\u4efb\u4e2d\u56fd\u6750\u6599\u5b66\u4f1a\u8ba1\u7b97\u6750\u6599\u5206\u4f1a\u59d4\u5458\u3001\u4e2d\u56fd\u91d1\u5c5e\u5b66\u4f1a\u975e\u6676\u5408\u91d1\u53ca\u5e94\u7528\u5206\u4f1a\u59d4\u5458\u3002\u4e3b\u6301\u548c\u53c2\u4e0e\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u9762\u4e0a\u9879\u76ee\uff0c\u79d1\u6280\u90e8\u91cd\u70b9\u7814\u53d1\u8ba1\u5212\uff0c\u4e2d\u56fd\u5de5\u7a0b\u7269\u7406\u7814\u7a76\u9662\u6311\u6218\u8ba1\u5212\uff08\u65b9\u5411\u9996\u5e2d\u79d1\u5b66\u5bb6\uff09\u3002\u5df2\u53d1\u8868SCI\u671f\u520a\u8bba\u658770\u4f59\u7bc7\uff0c\u5305\u62ecNature Materials 2 \u7bc7\u3001PNAS 1 \u7bc7\u3001Phys. Rev. Lett. 7\u7bc7\u3001Advanced Materials 2 \u7bc7\u3001Nature Communications 4 \u7bc7\u3001JACS 1\u7bc7\u3001Angewandte Chemie 1\u7bc7\u3001Acta Materialia 3 \u7bc7\u3002<\/p>\n<p><strong>\u4e3b\u8981\u7814\u7a76\u65b9\u5411<\/strong><strong>\uff1a<\/strong><strong><br \/>\n <\/strong>1. \u7406\u8bba\u6a21\u62df\u4e0e\u6750\u6599\u8bbe\u8ba1\uff1b2. \u975e\u6676\u6001\u6750\u6599\u4e0e\u7269\u7406\uff1b3. \u5148\u8fdb\u6750\u6599\u7269\u6027\u673a\u7406\uff1b4. \u9ad8\u901a\u91cf\u8ba1\u7b97\u4e0e\u4eba\u5de5\u667a\u80fd<\/p>\n<p>&nbsp;<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u8ba1\u7b97\u6750\u6599\u7ec4Isobel\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaokefu<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u7406\u89e3\u6750\u6599\u7684\u7ed3\u6784\u53ca\u5176\u5bf9\u5916\u754c\u523a\u6fc0\u7684\u54cd\u5e94\u81f3\u5173\u91cd\u8981\uff0c\u5176\u5bf9\u4e8e\u5f3a\u5ea6\u3001\u97e7\u6027\u548c\u5931\u6548\u7b49\u4e34\u754c\u529b\u5b66\u6027\u80fd\u8d77\u7740\u51b3\u5b9a\u6027\u4f5c\u7528\u3002\u5728\u975e\u6676\u6001\u6750\u6599\u4e2d\uff0c\u7531\u4e8e\u5176\u65e0\u5e8f\u539f\u5b50\u672c\u8d28\u548c\u70b9\u9635\u5468\u671f\u6027\u6d88\u5931\uff0c\u7ed3&#8230;<\/p>\n","protected":false},"author":4765,"featured_media":156059,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[3612,2798],"class_list":["post-156058","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","category-keji","tag-3612","tag-2798"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/156058"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/4765"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=156058"}],"version-history":[{"count":11,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/156058\/revisions"}],"predecessor-version":[{"id":156182,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/156058\/revisions\/156182"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/156059"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=156058"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=156058"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=156058"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}