{"id":159055,"date":"2018-11-14T06:30:40","date_gmt":"2018-11-13T22:30:40","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=159055"},"modified":"2018-11-13T21:07:30","modified_gmt":"2018-11-13T13:07:30","slug":"adv-eng-mater-%e7%bb%bc%e8%bf%b0%e5%b8%a6%e4%bd%a0%e4%ba%86%e8%a7%a3%e7%ba%b3%e7%b1%b3%e7%8e%bb%e7%92%83%e7%9a%84%e7%bb%93%e6%9e%84%e4%b8%8e%e6%80%a7%e8%83%bd","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=159055","title":{"rendered":"Adv. Eng. Mater.\u7efc\u8ff0\u5e26\u4f60\u4e86\u89e3\u7eb3\u7c73\u73bb\u7483\u7684\u7ed3\u6784\u4e0e\u6027\u80fd"},"content":{"rendered":"<p>\u3010\u5f15\u8a00\u3011<\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u7eb3\u7c73\u73bb\u7483\u7684\u53d1\u73b0\u4f7f\u5f97\u975e\u6676\u6001\u91d1\u5c5e\u6216\u91d1\u5c5e\u73bb\u7483\u9886\u57df\u66f4\u4e3a\u4e30\u5bcc\u3002\u7eb3\u7c73\u73bb\u7483\u5177\u6709\u957f\u5ea6\u5c3a\u5ea6\u5728\u51e0\u7eb3\u7c73\u7684\u5185\u90e8\u7ed3\u6784\u7279\u5f81\uff0c\u53ef\u901a\u8fc7\u5c40\u57df\u81ea\u7531\u4f53\u79ef\u548c\u5316\u5b66\u7ec4\u6210\u7684\u663e\u8457\u53d8\u5316\u6765\u8868\u5f81\u3002\u73b0\u6709\u7814\u7a76\u53d1\u73b0\uff0c\u7eb3\u7c73\u73bb\u7483\u7684\u7ed3\u6784\u548c\u4f20\u7edf\u65b9\u6cd5\u5236\u5907\u5f97\u5230\u7684\u91d1\u5c5e\u73bb\u7483\u6709\u7740\u663e\u8457\u5dee\u5f02\u3002\u901a\u5e38\u8ba4\u4e3a\u7eb3\u7c73\u73bb\u7483\u7684\u7ed3\u6784\u5305\u542b\u4e24\u4e2a\u4e0d\u540c\u7684\u975e\u6676\u6001\u533a\u57df\uff0c\u4ece\u800c\u5f15\u53d1\u4e00\u7cfb\u5217\u663e\u8457\u4e0d\u540c\u4e8e\u5feb\u51b7\u91d1\u5c5e\u73bb\u7483\u7684\u529b\u5b66\u3001\u70ed\u5b66\u548c\u78c1\u6027\u80fd\u3002\u56e0\u6b64\uff0c\u7eb3\u7c73\u73bb\u7483\u4f5c\u4e3a\u4e00\u79cd\u65b0\u7684\u975e\u6676\u56fa\u6001\u6750\u6599\uff0c\u5728\u4f17\u591a\u7ed3\u6784\u548c\u529f\u80fd\u5e94\u7528\u4e2d\u5177\u6709\u7740\u5f00\u521b\u6027\u7684\u673a\u9047\u548c\u6f5c\u529b\u3002<\/p>\n<p>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u5fb7\u56fd\u5361\u5c14\u65af\u9c81\u5384\u7406\u5de5\u5b66\u9662<\/strong>\u7684<strong>Yulia Ivanisenko<\/strong><strong>\u7814\u7a76\u5458\uff08\u7b2c\u4e00\u4f5c\u8005\u517c\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u548c<strong>Horst Hahn<\/strong><strong>\u7814\u7a76\u5458\uff08\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u5728<strong>Advanced Engineering Materials<\/strong>\u4e0a\u53d1\u8868\u4e86\u9898\u4e3a\u201c<strong>Structure and Properties of Nanoglasses<\/strong>\u201d\u7684\u7efc\u8ff0\u6587\u7ae0\u3002\u6b64\u7bc7\u7efc\u8ff0\u7684\u57fa\u672c\u7ed3\u6784\u5982\u4e0b\uff1a\u9996\u5148\u63cf\u8ff0\u4e86\u7eb3\u7c73\u73bb\u7483\u80cc\u540e\u7684\u57fa\u7840\u6982\u5ff5\uff1b\u63a5\u7740\u5bf9\u5176\u5408\u6210\u548c\u5236\u5907\u8def\u5f84\u4f5c\u4e86\u603b\u7ed3\uff0c\u8bc1\u660e\u7eb3\u7c73\u73bb\u7483\u539f\u5b50\u7ed3\u6784\u7684\u663e\u8457\u5dee\u5f02\uff1b\u6700\u540e\uff0c\u8bf4\u660e\u7eb3\u7c73\u73bb\u7483\u7684\u7ed3\u6784\u4e0d\u5747\u5300\u6027\u662f\u5982\u4f55\u5bfc\u81f4\u5176\u6027\u80fd\u7684\u5267\u70c8\u53d8\u5316\u7684\u3002<\/p>\n<p>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/p>\n<p>\u56fe1\uff1a\u57fa\u4e8eGleiter\u7b49\u4eba\u7684\u5de5\u4f5c\uff0c\u56fe\u793a\u7eb3\u7c73\u6676\u6750\u6599\u548c\u7eb3\u7c73\u73bb\u7483\u7684\u7f3a\u9677\u548c\u5316\u5b66\u663e\u5fae\u7ed3\u6784\u4e4b\u95f4\u7684\u7c7b\u6bd4\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159056\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/1-3.png\" alt=\"\" width=\"600\" height=\"331\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/1-3.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/1-3-300x166.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe2\uff1a\u5f84\u5411\u5206\u5e03\u51fd\u6570\u7684\u793a\u610f\u56fe\uff1a\u65e0\u5e8f\u539f\u5b50\u7ed3\u6784\uff0c\u8ba1\u7b97\u5f97\u5230\u7684\u5bf9\u5206\u5e03\u51fd\u6570\u548c\u8ba1\u7b97\u5f97\u5230\u7684\u5f84\u5411\u5206\u5e03\u51fd\u6570\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159057\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/2-3.png\" alt=\"\" width=\"600\" height=\"276\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/2-3.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/2-3-300x138.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe3\uff1a\u7eb3\u7c73\u675f\u884d\u5c04\u5e8f\u5217acquisition\u7684\u793a\u610f\u56fe\uff0c\u540e\u7eed\u8fdb\u884cRDF\u5904\u7406\u4ee5\u5f97\u5230RDF\u7acb\u65b9\u4f53\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159058\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/3-2.png\" alt=\"\" width=\"600\" height=\"407\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/3-2.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/3-2-300x204.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe4\uff1aTEM\u663e\u5fae\u5f62\u8c8c\u8868\u5f81\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159059\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/4-2.png\" alt=\"\" width=\"600\" height=\"334\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/4-2.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/4-2-300x167.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u672a\u8fc7\u6ee4\u7684TEM\u56fe\u50cf\uff1b<\/p>\n<p>(b)\u76f8\u5e94\u7684Ti\u7684EFTEM\u5206\u5e03\uff1b<\/p>\n<p>(c)\u76f8\u5e94\u7684Ni\u7684EFTEM\u5206\u5e03;<\/p>\n<p>(d)Ni50Ti45Cu5\u8584\u819c\u7684\u53e0\u52a0\u5f69\u56fe\uff1b<\/p>\n<p>(e)\u975e\u6676\u6001Ni50Ti45Cu5\u7ed3\u6784\u7684HRTEM\u56fe\u50cf\u3002<\/p>\n<p>\u56fe5\uff1a\u51dd\u805a\u6001\u7269\u8d28\u7684Voronoi\u591a\u9762\u4f53\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159060\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/5-2.png\" alt=\"\" width=\"600\" height=\"624\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/5-2.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/5-2-288x300.png 288w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u9762\u5fc3\u7acb\u65b9\u6676\u683c\u4e2d\u539f\u5b50\u5468\u56f4\u7684\u591a\u9762\u4f53\uff1b<\/p>\n<p>(b)\u9762\u5fc3\u7acb\u65b9\u683c\u5b50\u76f8\u5e94\u7684Voronoi\u591a\u9762\u4f53\u662f\u4e00\u4e2a\u83f1\u5f62\u5341\u4e8c\u9762\u4f53\uff1b<\/p>\n<p>(c)\u5c55\u5f00\u591a\u9762\u4f53\u53ef\u4ee5\u770b\u523012\u4e2a\u83f1\u9762\u4f53\uff0c\u4ece\u800c\u7ed9\u51faVoronoi\u6307\u6570&lt;0,12,0,0&gt;;<\/p>\n<p>(d)\u5728\u975e\u6676\u6001Cu64Zr36\u4e2d\u4ee5Cu\u4e3a\u4e2d\u5fc3\u7684\u4e8c\u5341\u9762\u4f53\u5355\u5143\uff1b<\/p>\n<p>(e)(d)\u56fe\u4e2d\u5bf9\u5e94\u7684Voronoi\u591a\u9762\u4f53\u662f\u6b63\u5341\u4e8c\u9762\u4f53\uff1b<\/p>\n<p>(f)\u5c06(e)\u56fe\u7ecf\u5c55\u5f00\u5e73\u94fa\u540e\u5f97\u523012\u4e2a\u4e94\u8fb9\u5f62\u9762\u3002<\/p>\n<p>\u56fe6\uff1a\u7eb3\u7c73\u73bb\u7483\u7684TEM\u8868\u5f81\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159061\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/6-2.png\" alt=\"\" width=\"600\" height=\"315\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/6-2.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/6-2-300x158.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)Cu50Zr50\u975e\u6676\u6001\u7eb3\u7c73\u9897\u7c92\u7684TEM\u56fe\u50cf\uff0c\u5185\u63d2\u56fe\u8868\u793a\u901a\u8fc7SAED\u786e\u5b9a\u7c89\u672b\u7684\u975e\u6676\u6001\u672c\u8d28\uff1b<\/p>\n<p>(b)HRTEM\u56fe\u50cf\u663e\u793a\u7eb3\u7c73\u73bb\u7483\u4e3a\u65e0\u6676\u76f8\u533a\u57df\u7684\u975e\u6676\u6001\u7ed3\u6784\uff0c\u76f8\u5e94\u7684\u884d\u5c04\u6a21\u5f0f\u95f4\u5185\u63d2\u56fe\u3002<\/p>\n<p>\u56fe7\uff1aNi50Ti45Cu5\u78c1\u63a7\u6e85\u5c04\u8584\u819c\u7684\u663e\u5fae\u7ed3\u6784\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159062\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/7-1.png\" alt=\"\" width=\"600\" height=\"262\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/7-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/7-1-300x131.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)1\u03bcm\u539a\u7684\u8584\u819c\u8868\u9762\u5f62\u8c8c\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>(b)\u5728Si\/SiO2\u57fa\u5e95\u4e0a\u6c89\u79ef\u5f97\u5230\u7684\u8584\u819c\uff0c\u7ecfFIB\u5236\u5907\u7684\u6a2a\u622a\u9762STEM\u56fe\u50cf\u3002<\/p>\n<p>\u56fe8\uff1a\u521d\u7ea7Fe90Sc10\u975e\u6676\u6001\u7eb3\u7c73\u9897\u7c92\u4e2dFe\u548cSc\u5206\u5e03\u60c5\u51b5\u7684EELS\u5206\u5e03\u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159063\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/8-1.png\" alt=\"\" width=\"600\" height=\"348\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/8-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/8-1-300x174.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)STEM\u56fe\u50cf\uff1b<\/p>\n<p>(b)Fe\u7684\u5206\u5e03\u56fe\uff1b<\/p>\n<p>(c)Sc\u7684\u5206\u5e03\u56fe\uff1b<\/p>\n<p>(d)\u5c06(b)\u548c(c)\u53e0\u52a0\u5f97\u5230\u7684\u56fe\u50cf\uff0c\u7ea2\u8272\u4ee3\u8868Fe,\u7eff\u8272\u4ee3\u8868Sc\uff1b<\/p>\n<p>(e)\u5206\u5b50\u52a8\u529b\u5b66\u6a21\u62df\u7ed3\u679c\u8868\u660e\uff0c\u7531\u4e8e\u8868\u9762\u504f\u6790\u6548\u5e94\uff0c\u5728IGC\u65b9\u6cd5\u5236\u5907\u5f62\u6210\u7684\u975e\u6676\u6001\u7403\u4f53\u4e2d\u5b58\u5728\u6210\u5206\u5dee\u5f02\uff1b<\/p>\n<p>(f)\u5206\u5b50\u52a8\u529b\u5b66\u6a21\u62df\u5f97\u5230\u76f4\u5f84\u5c3a\u5bf8\u57286-8nm\u7684Cu50Zr50\u975e\u6676\u6001\u7403\u4f53\u3002<\/p>\n<p>\u56fe9\uff1aFe25Sc75\u7eb3\u7c73\u73bb\u7483\u7684RDF\u5206\u5e03\u8868\u793a\u7ed3\u6784\u6da8\u843d\u53ca\u5176\u4e0e\u5143\u7d20\u504f\u6790\u4e4b\u95f4\u7684\u5173\u8054\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159064\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/9.png\" alt=\"\" width=\"600\" height=\"381\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/9-300x191.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)STEM-HAADF\u56fe\u50cf\uff1b<\/p>\n<p>(b)\u5728RDF\u5206\u5e03\u4e2d\u53d1\u73b0\u7684\u4e24\u79cd\u5178\u578bRDF\uff0c\u53ef\u63cf\u8ff0\u4e24\u7c7b\u6210\u5206\u76f8\u7684\u4e0d\u540c\u539f\u5b50\u5806\u79ef\u60c5\u51b5\uff1b<\/p>\n<p>(c)\u6210\u52061\uff08\u7eff\u8272\uff09\u5305\u542b\u66f4\u591a\u7684Sc-Sc\u952e\uff0c\u56e0\u6b64\u8868\u793a\u5bccSc\u73af\u5883\uff0c\u800c\u6210\u52062(\u7ea2\u8272)\u5305\u542b\u66f4\u591a\u7684Fe-Sc\u952e\uff0c\u8868\u793a\u5bccFe\u73af\u5883\uff1b<\/p>\n<p>(d)\u76f8\u5206\u5e03\u8868\u793a\u5c3a\u5bf8\u57285-8\u7eb3\u7c73\u7684\u4e24\u79cd\u6210\u5206\u76f8\u7684\u56e2\u7c07\u7c7b\u578b\u5206\u5e03\uff1b<\/p>\n<p>(e)\u4e24\u76f8\u7684RGB\u5206\u5e03\uff1b<\/p>\n<p>(f)\u76f8\u540c\u6837\u54c1\u7684STEM-EELS\u5206\u5e03\u3002<\/p>\n<p>\u56fe10\uff1aCu50Zr50\u7eb3\u7c73\u73bb\u7483\u6837\u54c1\u7684\u6210\u5206\u5206\u5e03\u60c5\u51b5\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159065\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/10-1.png\" alt=\"\" width=\"600\" height=\"291\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/10-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/10-1-300x146.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u5c16\u7aef\u4e3aCu50Zr50\u7eb3\u7c73\u73bb\u7483\u6837\u54c1\u5236\u5907\u7684\u539f\u5b50\u63a2\u9488\u56fe\u50cf\uff1b<\/p>\n<p>(b)\u6cbf(a)\u56fe\u7bad\u5934\u65b9\u5411\u8868\u793a\u7684Cu\u548cZr\u7684\u6210\u5206\u5206\u5e03\u3002<\/p>\n<p>\u56fe11\uff1a\u5206\u5b50\u52a8\u529b\u5b66\u6a21\u62df\u5f97\u5230\u7684Cu50Zr50\u7eb3\u7c73\u73bb\u7483\u7684\u663e\u5fae\u7ed3\u6784\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159066\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/11.png\" alt=\"\" width=\"600\" height=\"199\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/11-300x100.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u6210\u5206\u5b9a\u4e49\u7684\u663e\u5fae\u7ed3\u6784\uff1b<\/p>\n<p>(b)\u539f\u5b50\u6839\u636e\u5176von Mises\u526a\u5207\u5e94\u53d8\u6d82\u8272\uff0c\u8868\u793a\u77ed\u7a0b\u5e8f\u53d8\u5316\u5b9a\u4e49\u7684\u663e\u5fae\u7ed3\u6784\uff1b<\/p>\n<p>(c)\u526a\u5207\u540e\u539f\u5b50\u5728\u5408\u6210\u8fc7\u7a0b\u7684\u8f7b\u5fae\u53d8\u5316\u548c\u663e\u8457\u53d8\u5316\u3002<\/p>\n<p>\u56fe12\uff1a\u539f\u59cb\u548c\u88ab\u538b\u7f29\u7684Fe90Sc10\u975e\u6676\u6001\u7eb3\u7c73\u9897\u7c92\u7684\u5c0f\u89d2X\u5c04\u7ebf\u6563\u5c04\u7ed3\u679c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159067\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/12-1.png\" alt=\"\" width=\"600\" height=\"838\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/12-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/12-1-215x300.png 215w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)SAXS\u8c31\u4e2d\uff0c\u80cc\u666f\u6563\u5c04\u5df2\u88ab\u51cf\u53bb\uff1b<\/p>\n<p>(b)ln[l(q)\u00b7q4]-q<sup>2<\/sup>\u56fe\u786e\u5b9a\u539f\u59cb\u548c\u88ab\u538b\u7f29\u7684\u975e\u6676\u6001\u7eb3\u7c73\u9897\u7c92\u7684\u539a\u5ea6\u3002<\/p>\n<p>\u56fe13\uff1a\u901a\u8fc7\u7194\u878d\u7eba\u4e1d\u548c\u5185\u90e8\u6c14\u76f8\u51dd\u805a\uff08IGC\uff09\u5236\u5907\u5f97\u5230\u7684\u975e\u6676\u6001Fe90Sc10\u5408\u91d1\u7684RDF\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159068\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/13-1.png\" alt=\"\" width=\"600\" height=\"584\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/13-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/13-1-300x292.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe14\uff1a\u7194\u4f53\u7529\u5e26\u7684\u5e26\u6750(a)\u548c\u7eb3\u7c73\u73bb\u7483(b)\u7684\u4f4e\u6e29Mossbauer\u8c31\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159069\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/14.png\" alt=\"\" width=\"600\" height=\"685\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/14.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/14-263x300.png 263w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe15\uff1a\u8bbe\u60f3\u4e2d\u7684\u7eb3\u7c73\u73bb\u7483\u7ed3\u6784\u7684\u6a21\u578b\u793a\u610f\u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159070\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/15.png\" alt=\"\" width=\"600\" height=\"399\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/15.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/15-300x200.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe16\uff1a\u6676\u6001\u6750\u6599\uff0c\u91d1\u5c5e\u73bb\u7483\u548c\u4e24\u79cd\u7eb3\u7c73\u73bb\u7483\u7684\u81ea\u7531\u80fd\u72b6\u6001\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159071\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/16.png\" alt=\"\" width=\"600\" height=\"548\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/16.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/16-300x274.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe17\uff1a\u5feb\u6dec\u5e26\u6750\u548c\u7eb3\u7c73\u73bb\u7483\u5728\u538b\u75d5\u5e94\u53d8\u901f\u7387\u4e3a0.05s<sup>-1<\/sup>\u65f6\u6d4b\u5f97\u7684\u5178\u578b\u7eb3\u7c73\u538b\u75d5\u66f2\u7ebf\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159072\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/17.png\" alt=\"\" width=\"600\" height=\"427\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/17.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/17-300x214.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe18\uff1a\u5236\u5f97\u7684\u7eb3\u7c73\u73bb\u7483\u548c\u5468\u56f4\u6709\u660e\u663e\u526a\u5207\u5e26\u7684\u7194\u4f53\u7529\u5e26\u7684\u5e26\u6750\u4e2d\u538b\u75d5\u7684SEM\u6210\u50cf\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159073\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/18.png\" alt=\"\" width=\"600\" height=\"276\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/18.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/18-300x138.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u56fe19\uff1a\u7eb3\u7c73\u73bb\u7483\u548c\u5feb\u51b7\u73bb\u7483\u7684\u62c9\u4f38\u5b9e\u9a8c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159074\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/19.png\" alt=\"\" width=\"600\" height=\"289\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/19.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/19-300x145.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u7eb3\u7c73\u73bb\u7483\u548c\u5feb\u51b7\u5757\u4f53\u73bb\u7483\u7684\u62c9\u4f38\u5e94\u529b\u5e94\u53d8\u66f2\u7ebf\uff1b<\/p>\n<p>(b)\u6d4b\u8bd5\u540e\u7684\u5feb\u51b7\u73bb\u7483\u62c9\u4f38\u8bd5\u6837\uff1b<\/p>\n<p>(c)\u8bb0\u5f55\u89c6\u9891\u4e2d\u63d0\u53d6\u7684\u753b\u9762\uff1b<\/p>\n<p>(d)\u6d4b\u8bd5\u540e\u7684\u7eb3\u7c73\u73bb\u7483\u62c9\u4f38\u8bd5\u6837\uff1b<\/p>\n<p>(e)\u540c\u4e3a\u6d4b\u8bd5\u540e\u7684\u7eb3\u7c73\u73bb\u7483\u62c9\u4f38\u8bd5\u6837\uff0c\u5185\u63d2\u56fe\u4e3a\u9009\u533a\u884d\u5c04\u56fe\u50cf\u3002<\/p>\n<p>\u56fe20\uff1aCu50Zr50\u5feb\u51b7\u5e26\u6750\u548c\u7eb3\u7c73\u73bb\u7483\u7684DSC\u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159075\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/20-1.png\" alt=\"\" width=\"600\" height=\"437\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/20-1.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/20-1-300x219.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>DSC\u6d4b\u8bd5\u8868\u793a\u51fa\u73bb\u7483\u8f6c\u53d8\u548c\u7ed3\u6676\u6e29\u5ea6\u3002\u7eb3\u7c73\u73bb\u7483\u7684\u7ed3\u6676\u6e29\u5ea6\u8981\u9ad8\u4e8e\u5feb\u51b7\u5e26\u6750\u3002<\/p>\n<p>\u56fe21\uff1aFe25Sc75\u7eb3\u7c73\u73bb\u7483\u7684\u70ed\u5e94\u53d8\u548c\u521d\u59cb\u70ed\u81a8\u80c0\u6d4b\u91cf\u8fc7\u7a0b\u4e2d\u51fa\u73b0\u7684\u4f53\u79ef\u635f\u5931\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-159076\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/21.png\" alt=\"\" width=\"600\" height=\"454\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/21.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/21-300x227.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u3010\u5c0f\u7ed3\u3011<\/p>\n<p>\u7eb3\u7c73\u73bb\u7483\u88ab\u89c6\u4e3a\u65b0\u578b\u7684\u7ed3\u6784\u8c03\u6574\u8fc7\u7684\u91d1\u5c5e\u73bb\u7483\uff0c\u8868\u73b0\u51fa\u4e00\u7cfb\u5217\u5feb\u51b7\u91d1\u5c5e\u73bb\u7483\u4e2d\u672a\u51fa\u73b0\u7684\u65b0\u5947\u6027\u8d28\u3002\u4e0d\u540c\u7684\u7ed3\u6784\u548c\u6027\u8d28\u662f\u7531\u4e8e\u7eb3\u7c73\u73bb\u7483\u5177\u6709\u5b8c\u5168\u4e0d\u540c\u7684\u5236\u5907\u8def\u5f84\u3002\u7eb3\u7c73\u73bb\u7483\u901a\u5e38\u662f\u7ecf\u8fc7\u5728\u9ad8\u538b\u4e0b\u5ba4\u6e29\u5408\u5e76\u975e\u6676\u6001\u9897\u7c92\u3002\u7eb3\u7c73\u73bb\u7483\u7684\u539f\u5b50\u7ed3\u6784\u5305\u542b\u4e24\u79cd\u5177\u6709\u663e\u8457\u5dee\u5f02\u7684\u975e\u6676\u6001\u533a\u57df\uff0c\u4e00\u79cd\u548c\u5feb\u51b7\u73bb\u7483\u7684\u7ed3\u6784\u76f8\u540c\uff0c\u53e6\u4e00\u79cd\u8868\u73b0\u51fa\u66f4\u5927\u7684\u81ea\u7531\u4f53\u79ef\uff0c\u4e14\u4f34\u968f\u7740\u4e2d\u7a0b\u5e8f\u589e\u52a0\u3002\u8fd9\u79cd\u7279\u6b8a\u7684\u539f\u5b50\u7ed3\u6784\u5bfc\u81f4\u7eb3\u7c73\u73bb\u7483\u548c\u540c\u6210\u5206\u7684\u5feb\u51b7\u5757\u4f53\u91d1\u5c5e\u73bb\u7483\u76f8\u6bd4\uff0c\u4f1a\u4ea7\u751f\u4e0d\u540c\u7684\u529b\u5b66\u3001\u70ed\u5b66\u548c\u78c1\u5b66\u6027\u8d28\u3002<\/p>\n<p>\u603b\u7684\u6765\u8bf4\uff0c\u7eb3\u7c73\u73bb\u7483\u662f\u975e\u6676\u6001\u6750\u6599\u5bb6\u65cf\u4e2d\u65b0\u5947\u6709\u8da3\u7684\u4e00\u7c7b\uff0c\u56e0\u800c\u5728\u591a\u4e2d\u7ed3\u6784\u548c\u529f\u80fd\u6027\u5e94\u7528\u4e2d\u6709\u7740\u5de8\u5927\u7684\u6f5c\u529b\u3002\u7136\u800c\uff0c\u8981\u60f3\u613f\u671b\u6210\u771f\uff0c\u8fd8\u9700\u8981\u5bf9\u7eb3\u7c73\u73bb\u7483\u7684\u7ed3\u6784\u53ca\u7ed3\u6784-\u6027\u80fd\u5173\u7cfb\u8fdb\u884c\u6df1\u5165\u7406\u89e3\u3002\u53e6\u5916\uff0c\u4e3a\u4f7f\u5de5\u4e1a\u754c\u7684\u7eb3\u7c73\u73bb\u7483\u6750\u6599\u80fd\u53ef\u6301\u7eed\u7684\u5236\u9020\uff0c\u5728\u53d1\u5c55\u5236\u5907\u6280\u672f\u65b9\u9762\u5e94\u8be5\u52a0\u5927\u529b\u5ea6\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adem.201800404\" target=\"_blank\" rel=\"noopener\">Structure and Properties of Nanoglasses<\/a>\uff08Adv. Eng. Mater.\uff0c2018\uff0cDOI\uff1a10.1002\/adem.201800404\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u91d1\u5c5e\u6750\u6599\u7ec4Isobel\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenvip<\/p>\n<p>\u6750\u6599\u4eba\u91cd\u78c5\u63a8\u51fa\u6750\u6599\u8ba1\u7b97\u89e3\u51b3\u65b9\u6848\uff0c\u7ec4\u5efa\u4e86\u4e00\u652f\u6765\u81ea\u5168\u56fd\u77e5\u540d\u9ad8\u6821\u8001\u5e08\u53ca\u4f01\u4e1a\u5de5\u7a0b\u5e08\u7684\u79d1\u6280\u987e\u95ee\u56e2\u961f\uff0c\u4e13\u6ce8\u4e8e\u4e3a\u5927\u5bb6\u89e3\u51b3\u5404\u7c7b\u8ba1\u7b97\u6a21\u62df\u9700\u6c42\u3002\u5982\u679c\u60a8\u6709\u9700\u6c42\uff0c\u6b22\u8fce\u626b\u4ee5\u4e0b\u4e8c\u7ef4\u7801\u63d0\u4ea4\u60a8\u7684\u9700\u6c42\uff0c\u6216\u76f4\u63a5\u8054\u7cfb\u5fae\u4fe1\u5ba2\u670d\uff08\u5fae\u4fe1\u53f7\uff1acailiaoren001\uff09<\/p>\n<p><a href=\"http:\/\/dn.cailiaoniu.com\/2018\/04\/jisuan-1-1.png\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-141176\" src=\"http:\/\/dn.cailiaoniu.com\/2018\/04\/jisuan-1-1.png\" sizes=\"(max-width: 600px) 100vw, 600px\" srcset=\"http:\/\/dn.cailiaoniu.com\/2018\/04\/jisuan-1-1.png 600w, http:\/\/dn.cailiaoniu.com\/2018\/04\/jisuan-1-1-150x150.png 150w, http:\/\/dn.cailiaoniu.com\/2018\/04\/jisuan-1-1-300x300.png 300w\" alt=\"\" width=\"600\" height=\"600\" \/><\/a><\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u8fd1\u5e74\u6765\uff0c\u7eb3\u7c73\u73bb\u7483\u7684\u53d1\u73b0\u4f7f\u5f97\u975e\u6676\u6001\u91d1\u5c5e\u6216\u91d1\u5c5e\u73bb\u7483\u9886\u57df\u66f4\u4e3a\u4e30\u5bcc\u3002\u7eb3\u7c73\u73bb\u7483\u5177\u6709\u957f\u5ea6\u5c3a\u5ea6\u5728\u51e0\u7eb3\u7c73\u7684\u5185\u90e8\u7ed3\u6784\u7279\u5f81\uff0c\u53ef\u901a\u8fc7\u5c40\u57df\u81ea\u7531\u4f53\u79ef\u548c\u5316\u5b66\u7ec4\u6210\u7684\u663e\u8457\u53d8\u5316\u6765\u8868\u5f81\u3002&#8230;<\/p>\n","protected":false},"author":4765,"featured_media":159060,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[533],"tags":[3702,3701,1830],"class_list":["post-159055","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zongshu","tag-kit","tag-3701","tag-1830"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/159055"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/4765"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=159055"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/159055\/revisions"}],"predecessor-version":[{"id":159144,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/159055\/revisions\/159144"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/159060"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=159055"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=159055"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=159055"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}