{"id":159951,"date":"2018-11-28T06:30:07","date_gmt":"2018-11-27T22:30:07","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=159951"},"modified":"2018-11-27T17:31:36","modified_gmt":"2018-11-27T09:31:36","slug":"%e5%8d%8e%e4%b8%ad%e7%a7%91%e5%a4%a7%e5%90%b4%e7%87%95%e5%ba%86%e6%95%99%e6%8e%88nature-commun-%ef%bc%9a%e5%9f%ba%e4%ba%8e%e5%a4%a7%e9%9d%a2%e7%a7%af%e5%8f%8c%e5%b1%82mos2%e7%9a%84%e5%8f%af%e6%89%a9","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=159951","title":{"rendered":"\u534e\u4e2d\u79d1\u5927\u5434\u71d5\u5e86\u6559\u6388Nature Commun.\uff1a\u57fa\u4e8e\u5927\u9762\u79ef\u53cc\u5c42MoS2\u7684\u53ef\u6269\u5c55\u9ad8\u6027\u80fd\u5c04\u9891\u7535\u5b50\u8bbe\u5907"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u4e8c\u7ef4\u534a\u5bfc\u4f53\u56e0\u5176\u539f\u5b50\u7ea7\u7684\u8584\u4f53\u548c\u4f18\u5f02\u7684\u8f7d\u4f53\u4f20\u8f93\u6027\u80fd\u800c\u5728\u8bf8\u5982\u4f20\u611f\u5668\u3001\u5b58\u50a8\u5668\u4ee5\u53ca\u903b\u8f91\u5e94\u7528\u7b49\u65b0\u5174\u7684\u7535\u5b50\u4ea7\u54c1\u9886\u57df\u5e94\u7528\u4e2d\u53d7\u5230\u6781\u5927\u7684\u5173\u6ce8\u3002\u65e0\u7ebf\u901a\u4fe1\u4e2d\u7684\u67d4\u6027\u7535\u5b50\u5668\u4ef6\u662f\u76ee\u524d\u6700\u6709\u524d\u666f\u7684\u9886\u57df\u4e4b\u4e00\uff0c\u5176\u4e2d\u67d4\u6027\u65e0\u6e90\u5143\u4ef6\u548c\u6709\u6e90\u5143\u4ef6\u53d6\u5f97\u4e86\u5feb\u901f\u53d1\u5c55\u3002\u5c3d\u7ba1\u77f3\u58a8\u70ef\u6676\u4f53\u7ba1\u5728\u6709\u6e90\u5c04\u9891\u5143\u4ef6\u4e2d\u5e7f\u53d7\u5173\u6ce8\uff0c\u77f3\u58a8\u70ef\u7684\u65e0\u95f4\u9699\u6027\u8d28\u5bfc\u81f4\u8fd9\u4e9b\u6676\u4f53\u7ba1\u4e2d\u7684\u7535\u6d41\u9971\u548c\u5ea6\u548c\u8f93\u51fa\u7535\u5bfc\u7387\u8f83\u5dee\uff0c\u5bf9\u4e8e\u653e\u5927\u548c\u6df7\u5408\u9ad8\u9891\u4fe1\u53f7\u662f\u4e0d\u5229\u7684\u3002\u6700\u8fd1\uff0c\u57fa\u4e8eMoS<sub>2<\/sub>\u7b49\u4e8c\u7ef4\u8fc7\u5ea6\u91d1\u5c5e\u786b\u5316\u7269\u7684\u9ad8\u9891\u6676\u4f53\u7ba1\u548c\u7535\u8def\u65b9\u9762\u53d6\u5f97\u4e86\u5f88\u5927\u7814\u7a76\u8fdb\u5c55\uff0c\u5176\u80fd\u591f\u514b\u670d\u77f3\u58a8\u70ef\u7684\u4e0a\u8ff0\u5173\u952e\u7f3a\u70b9\u3002\u4e3a\u4e86\u83b7\u5f97\u4f4e\u6210\u672c\u3001\u53ef\u6269\u5c55\u7684\u89e3\u51b3\u65b9\u6848\uff0c\u8bb8\u591a\u7814\u7a76\u5c0f\u7ec4\u53d1\u5c55\u4e86\u5229\u7528\u5316\u5b66\u6c14\u76f8\u6c89\u79ef\uff08CVD\uff09\u5927\u9762\u79ef\u5408\u6210MoS<sub>2<\/sub>\u539f\u5b50\u8584\u819c\u7684\u65b9\u6cd5\u3002\u57fa\u4e8eCVD\u751f\u957f\u5355\u5c42MoS<sub>2<\/sub>\u7684\u67d4\u6027\u805a\u9170\u4e9a\u80fa\u57fa\u677f\u4e0a\u7684\u5c04\u9891\u6676\u4f53\u7ba1\u53c2\u6570\u4ecd\u8fdc\u4f4e\u4e8e\u57fa\u4e8e\u5265\u79bbMoS<sub>2<\/sub>\u7684\u5668\u4ef6\uff0c\u56e0\u800c\u4e25\u91cd\u9650\u5236\u4e86\u5b83\u4eec\u7684\u9ad8\u9891\u5e94\u7528\u3002\u53cc\u5c42MoS<sub>2<\/sub>\u7684\u8f7d\u6d41\u5b50\u8fc1\u79fb\u7387\u8981\u9ad8\u4e8e\u5355\u5c42\u7684\u8f7d\u6d41\u5b50\u8fc1\u79fb\u7387\uff0c\u4f46\u662f\u901a\u8fc7CVD\u65b9\u6cd5\u751f\u957f\u7684\u53cc\u5c42MoS<sub>2<\/sub>\u5c3a\u5bf8\u5c0f\u4e14\u8fc1\u79fb\u7387\u8f83\u5dee\uff0c\u9650\u5236\u4e86\u5176\u5668\u4ef6\u6027\u80fd\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u534e\u4e2d\u79d1\u6280\u5927\u5b66<\/strong><strong>\u5434\u71d5\u5e86<\/strong><strong>\u6559\u6388\u8bfe\u9898\u7ec4<\/strong>\u62a5\u9053\u4e86\u4e00\u79cd\u901a\u8fc7\u8c03\u63a7CVD\u751f\u957f\u671f\u95f4MoO<sub>3<\/sub>\u524d\u4f53\u91cd\u91cf\u6765\u5b9e\u73b0\u7194\u878d\u73bb\u7483\u4e0a\u5177\u6709\u9ad8\u8fc1\u79fb\u7387\u3001\u5927\u9762\u79ef\u53cc\u5c42MoS<sub>2<\/sub>\u7684\u5236\u5907\u65b9\u6cd5\u3002\u5229\u7528\u8be5\u65b9\u6cd5\u53ef\u4ee5\u83b7\u5f97\u9ad8\u8fbe200 \u03bcm\u7684\u7574\u5c3a\u5bf8\uff0c\u5e76\u4e14\u6240\u5f97\u5230\u7684\u5355\u6676\u4e09\u89d2\u5f62\u53cc\u5c42MoS<sub>2<\/sub>\u5c55\u73b0\u51fa36 cm<sup>2<\/sup> V<sup>\u22121<\/sup> s<sup>\u22121<\/sup>\u7684\u5ba4\u6e29\u7535\u5b50\u8fc1\u79fb\u7387\u3002\u5177\u6709\u4f18\u5316\u7684\u9ad8\u03ba\u7535\u4ecb\u8d28\u7684\u9ad8\u6027\u80fd\u6676\u4f53\u7ba1\u5728300 K\u65f6\u80fd\u591f\u63d0\u4f9b427 \u03bcA \u03bcm<sup>-1<\/sup>\u7684\u5bfc\u901a\u7535\u6d41\uff0c\u540c\u65f6\u57284.3 K\u65f6\u63d0\u4f9b\u4e861.52 mA \u03bcm<sup>-1<\/sup>\u521b\u7eaa\u5f55\u7684\u9ad8\u5bfc\u901a\u7535\u6d41\u3002\u6b64\u5916\uff0c\u5c04\u9891\u6676\u4f53\u7ba1\u7684\u5916\u90e8\u9ad8\u622a\u6b62\u9891\u7387\u4e3a7.2 GHz\uff0c\u8bb0\u5f55\u7684\u5916\u90e8\u6700\u9ad8\u632f\u8361\u9891\u7387\u4e3a\u521b\u7eaa\u5f55\u768423 GHz\u3002\u8be5\u6210\u679c\u4ee5\u9898\u4e3a&#8221;<strong>Scalable high performance radio frequency electronics based on large domain bilayer MoS<sub>2<\/sub><\/strong>&#8220;\u53d1\u8868\u5728\u56fd\u9645\u8457\u540d\u671f\u520a<strong>Nature Communications<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe1 \u53cc\u5c42MoS<sub>2<\/sub>\u5728\u7194\u878d\u73bb\u7483\u4e0a\u7684\u5408\u6210\u548c\u5f62\u8c8c\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-159952 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/1-40.jpg\" alt=\"\" width=\"600\" height=\"614\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/1-40.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/1-40-293x300.jpg 293w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u7528\u4e8e\u5728\u7194\u878d\u73bb\u7483\u4e0a\u5408\u6210\u53cc\u5c42MoS<sub>2<\/sub>\u7684CVD\u88c5\u7f6e\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>(b-e) CVD\u751f\u957f\u7684MoS<sub>2<\/sub>\u5728\u7194\u878d\u73bb\u7483\u4e0a\u7684\u5149\u5b66\u663e\u5fae\u7167\u7247\uff08\u76f8\u5e94\u7684MoO<sub>3<\/sub>\u91cd\u91cf\u5206\u522b\u4e3a1\u30011.5\u30013\u548c6 mg\uff1b\u6bd4\u4f8b\u5c3a\u5206\u522b\u4e3a30\u300140\u300150\u548c100 \u03bcm\uff09\uff1b<\/p>\n<p>(f-g) \u8f6c\u79fb\u540eSiO<sub>2<\/sub>\/Si\u886c\u5e95\u4e0a\u53cc\u5c42MoS<sub>2<\/sub>\u7684AFM\u56fe\u50cf\uff08\u6bd4\u4f8b\u5c3a\u4e3a1 \u03bcm\uff09\uff1b<\/p>\n<p>(h) \u7ebf\u5207\u5272A-B\uff0cC-D\u548cE-F\u5bf9\u5e94\u4e8e\u5355\u5c42MoS<sub>2<\/sub>\u7684\u539a\u5ea6\u7684AFM\u6570\u636e\u3002<\/p>\n<p><strong>\u56fe2 \u6750\u6599\u6210\u50cf\u548c\u6676\u4f53\u7ed3\u6784\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-159953 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/2-41.jpg\" alt=\"\" width=\"600\" height=\"557\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/2-41.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/2-41-300x279.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) CVD\u5355\u5c42\uff08\u9ed1\u7ebf\uff09\u548c\u53cc\u5c42MoS<sub>2<\/sub>\uff08\u54c1\u7ea2\u7ebf\uff09\u7684\u62c9\u66fc\u5149\u8c31\uff1b<\/p>\n<p>(b) \u5728385 cm<sup>-1<\/sup>\u5904\u7684\u5cf0\u7684\u62c9\u66fc\u5149\u8c31\u56fe\uff1b<\/p>\n<p>(c) \u5728405 cm<sup>-1<\/sup>\u5904\u7684\u5cf0\u7684\u62c9\u66fc\u5149\u8c31\u56fe\uff1b<\/p>\n<p>(d) CVD\u5355\u5c42\uff08\u9ed1\u7ebf\uff09\u548c\u53cc\u5c42\uff08\u54c1\u7ea2\u7ebf\uff09MoS<sub>2<\/sub>\u7684\u5149\u81f4\u53d1\u5149\u5149\u8c31\uff1b<\/p>\n<p>(e) \u57281.85 eV\u5cf0\u503c\u5904\u7684PL\u5149\u8c31\u56fe\uff1b<\/p>\n<p>(f) \u53cc\u5c42\uff08\u53f3\uff09\u548c\u5355\u5c42\uff08\u5de6\uff09\u4e4b\u95f4\u8fb9\u754c\u7684\u4f4e\u5206\u8fa8\u7387TEM\u56fe\u50cf\uff1b<\/p>\n<p>(g) (f)\u4e2d\u53cc\u5c42\u533a\u57df\u4e2d\u7684\u5178\u578bSAED\u56fe\u6848\u7684\u56fe\u50cf\uff1b<\/p>\n<p>(h) AA\u5806\u53e0\u53cc\u5c42MoS<sub>2<\/sub>\u7684HRTEM\u56fe\u50cf\u548c\u539f\u5b50\u7ed3\u6784\uff1b<\/p>\n<p>(i) \u4ece\u53cc\u5c42MoS<sub>2<\/sub>\u7684\u6298\u53e0\u8fb9\u7f18\u8bb0\u5f55\u7684HRTEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe3 \u5ba4\u6e29\u548c\u4f4e\u6e29\u4e0b\u80cc\u95e8\u53cc\u5c42MoS<sub>2<\/sub>\u6676\u4f53\u7ba1\u7684\u76f4\u6d41\u7535\u7279\u6027<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-159954 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/3-39.jpg\" alt=\"\" width=\"600\" height=\"447\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/3-39.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/3-39-300x224.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u5177\u6709\u4e0d\u540c\u6c9f\u9053\u957f\u5ea6\u7684\u80cc\u95e8MoS<sub>2<\/sub>\u6676\u4f53\u7ba1\u7684\u5149\u5b66\u663e\u5fae\u7167\u7247\uff08\u6bd4\u4f8b\u5c3a\u4e3a10 \u03bcm\uff09\uff1b<\/p>\n<p>(b) \u6709\u6e90\u5668\u4ef6\u533a\u57df\u548c\u653e\u5927\u56fe\u7247\u7684\u76f8\u5e94SEM\u56fe\u50cf\uff1b<\/p>\n<p>(c) 3 \u03bcm\u6c9f\u9053\u957f\u5ea6\u7684\u80cc\u95e8\u5355\u5c42\uff08\u5206\u522b\u4e3a\u84dd\u7ebf\u548c\u7a7a\u5fc3\u83f1\u5f62\uff09\u548c\u53cc\u5c42\uff08\u6d0b\u7ea2\u8272\u7ebf\u548c\u5f00\u653e\u5f0f\u83f1\u5f62\uff09MoS<sub>2<\/sub>\u6676\u4f53\u7ba1\u572850 mV\u504f\u7f6e\u7535\u538b\u4e0b<em>I<\/em><sub>ds<\/sub> &#8211; <em>V<\/em><sub>gs<\/sub>\u4f20\u9012\u7279\u6027\u548c\u57281 V\u504f\u7f6e\u7535\u538b\u4e0b<em>g<\/em><sub>m<\/sub> &#8211;<em>V<\/em><sub>gs<\/sub>\u66f2\u7ebf\uff1b<\/p>\n<p>(d) \u53cc\u5c42MoS<sub>2<\/sub>\u6676\u4f53\u7ba1\u5728300 K\u7684<em>I<\/em><sub>ds<\/sub> \u2013 <em>V<\/em><sub>ds<\/sub>\u8f93\u51fa\u7279\u6027\uff1b<\/p>\n<p>(e) \u53cc\u5c42MoS<sub>2<\/sub>\u6676\u4f53\u7ba1\u57284.3 K\u7684<em>I<\/em><sub>ds<\/sub> \u2013 <em>V<\/em><sub>ds<\/sub>\u8f93\u51fa\u7279\u6027\uff1b<\/p>\n<p>(f) \u63d0\u53d6\u7684\u56fa\u6709\u573a\u6548\u5e94\u8fc1\u79fb\u7387\u4e0e\u53cc\u5c42MoS<sub>2<\/sub> FET\u6e29\u5ea6\u7684\u5173\u7cfb\u56fe\uff1b<\/p>\n<p>(g) 40 nm\uff08\u54c1\u7ea2\u8272\u7ebf\uff09\u3001500 nm\uff08\u84dd\u8272\u7ebf\uff09\u548c3 \u03bcm\uff08\u9ed1\u8272\u7ebf\uff09\u4e0d\u540c\u6c9f\u9053\u957f\u5ea6\u7684\u53cc\u5c42MoS<sub>2<\/sub>\u6676\u4f53\u7ba1\u5728\u5ba4\u6e29\u300150 mV\u504f\u538b\u4e0b<em>I<\/em><sub>ds<\/sub> \u2013 <em>V<\/em><sub>ds<\/sub>\u4f20\u8f93\u7279\u6027\uff1b<\/p>\n<p>(h) \u6c9f\u9053\u957f\u5ea6\u4e3a40 nm\u7684\u53cc\u5c42MoS<sub>2<\/sub>\u6676\u4f53\u7ba1\u5728300 K\u548c4.3 K\u6761\u4ef6\u4e0b<em>I<\/em><sub>ds<\/sub> \u2013 <em>V<\/em><sub>ds<\/sub>\u8f93\u51fa\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe4 \u77ed\u6c9f\u9053RF\u6676\u4f53\u7ba1\u7684\u9ad8\u9891\u6d4b\u91cf<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-159955 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/4-39.jpg\" alt=\"\" width=\"600\" height=\"471\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/4-39.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/4-39-300x236.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u53cc\u5c42MoS<sub>2<\/sub> RF\u6676\u4f53\u7ba1\u7684\u793a\u610f\u56fe\uff08S\uff1a\u6e90\u6781\uff1bD\uff1a\u6f0f\u6781\uff1bG\uff1a\u6805\u6781\uff09\uff1b<\/p>\n<p>(b) \u5177\u6709\u53cc\u6c9f\u9053\u7ed3\u6784\u7684MoS<sub>2<\/sub> RF\u6676\u4f53\u7ba1\u7684SEM\u56fe\u50cf\uff08\u6bd4\u4f8b\u5c3a\u4e3a500 nm\uff09\uff1b<\/p>\n<p>(c) \u5bf9\u4e8e\u6805\u6781\u957f\u5ea6\u4e3a90 nm\u7684\u5668\u4ef6\uff0c\u5c0f\u4fe1\u53f7\u7535\u6d41\u589e\u76ca| h<sub>21<\/sub> |\u4e0e\u9891\u7387\u7684\u5173\u7cfb\u56fe\uff1b<\/p>\n<p>(d) \u5bf9\u4e8e\u6805\u6781\u957f\u5ea6\u4e3a90 nm\u7684\u5668\u4ef6\uff0c\u5355\u8fb9\u529f\u7387\u589e\u76caU\u4e0e\u9891\u7387\u7684\u5173\u7cfb\u56fe\uff1b<\/p>\n<p>(e) \u5bf9\u4e8e\u6805\u6781\u957f\u5ea6\u4e3a90 nm\u7684\u5668\u4ef6\uff0c\u7535\u538b\u589e\u76ca\u4e0e\u9891\u7387\u7684\u5173\u7cfb\u56fe\uff1b<\/p>\n<p>(f) \u5916\u90e8<em>f<\/em><sub>T<\/sub>\u4e0e\u6805\u6781\u957f\u5ea6\u7684\u5173\u7cfb\u56fe\uff1b<\/p>\n<p>(g) \u5916\u90e8<em>f<\/em><sub>max<\/sub>\u4e0e\u6805\u6781\u957f\u5ea6\u7684\u5173\u7cfb\u56fe\uff1b<\/p>\n<p>(h)<em> f<\/em><sub>max<\/sub> \/ <em>f<\/em><sub>T<\/sub>\u4e0e\u6805\u6781\u957f\u5ea6\u7684\u5173\u7cfb\u56fe\u3002<\/p>\n<p><strong>\u56fe5 \u521a\u6027\u548c\u67d4\u6027\u57fa\u677f\u4e0aGigahertz MoS<sub>2<\/sub>\u6df7\u9891\u5668<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-159956 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/5-23.jpg\" alt=\"\" width=\"600\" height=\"315\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/5-23.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/11\/5-23-300x158.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u57fa\u4e8eMoS<sub>2<\/sub> FET\u7684RF\u6df7\u9891\u5668\u7684\u7535\u8def\u539f\u7406\u56fe\uff1b<\/p>\n<p>(b) \u5f53<em>f<\/em><sub>RF<\/sub> = 1.5 GHz\u3001<em>P<\/em><sub>RF<\/sub> = 2 dBm\u3001<em>f<\/em><sub>LO<\/sub> = 1.4 GHz\u3001<em>P<\/em><sub>LO<\/sub> = 9 dBm\u65f6\u5728\u521a\u6027\u57fa\u677f\u4e0a\u6df7\u9891\u5668\u7684\u8f93\u51fa\u9891\u8c31\uff1b<\/p>\n<p>(c) \u521a\u6027\u57fa\u677f\u4e0a\u6df7\u5408\u5668\u5728<em>f<\/em><sub>RF<\/sub> = 1.5 GHz\u3001<em>P<\/em><sub>RF<\/sub> = 2 dBm\u3001<em>f<\/em><sub>LO<\/sub> = 1.4 GHz\u65f6\u8f6c\u6362\u589e\u76ca\u4e0eLO\u529f\u7387\u7684\u5173\u7cfb\u56fe\uff1b<\/p>\n<p>(d) \u5bf9\u4e8e\u6805\u6781\u957f\u5ea6\u4e3a300 nm\u5668\u4ef6\u5728\u805a\u9170\u4e9a\u80fa\u4e0a\u5c0f\u4fe1\u53f7\u7535\u6d41\u589e\u76ca| h<sub>21<\/sub> |\u548c\u5355\u8fb9\u529f\u7387\u589e\u76caU\u4e0e\u9891\u7387\u7684\u5173\u7cfb\u56fe\uff1b<\/p>\n<p>(e) \u5f53<em>f<\/em><sub>RF<\/sub> = 1.5 GHz\u3001<em>P<\/em><sub>RF<\/sub> = 9 dBm\u3001<em>f<\/em><sub>LO<\/sub> = 1.4 GHz\u3001<em>P<\/em><sub>LO<\/sub> = 9 dBm\u65f6\u5728\u67d4\u6027\u57fa\u677f\u4e0a\u6df7\u5408\u5668\u7684\u8f93\u51fa\u9891\u8c31\uff1b<\/p>\n<p>(f) \u5f53<em>f<\/em><sub>RF<\/sub> = 1.5 GHz\u3001<em>P<\/em><sub>RF<\/sub> = 9 dBm\u3001<em>f<\/em><sub>LO<\/sub> = 1.4 GHz\u65f6\u5728\u67d4\u6027\u57fa\u677f\u4e0a\u6df7\u5408\u5668\u8f6c\u6362\u589e\u76ca\u4e0eLO\u529f\u7387\u7684\u5173\u7cfb\u56fe\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u6587\u62a5\u9053\u4e86\u4e00\u79cd\u901a\u8fc7\u8c03\u63a7CVD\u751f\u957f\u671f\u95f4MoO<sub>3<\/sub>\u524d\u4f53\u91cd\u91cf\u6765\u5236\u5907\u5177\u6709\u9ad8\u8fc1\u79fb\u7387\u3001\u5927\u9762\u79ef\u53cc\u5c42MoS<sub>2<\/sub>\u7684\u65b9\u6cd5\uff0c\u901a\u8fc7\u4f18\u5316\u7684\u751f\u957f\u6761\u4ef6\u53ef\u4ee5\u5b9e\u73b0\u5c3a\u5bf8\u9ad8\u8fbe200 \u03bcm\u3002\u57fa\u4e8e\u53cc\u5c42MoS<sub>2<\/sub>\u5236\u9020\u7684\u6676\u4f53\u7ba1\u663e\u793a\u51fa\u9ad8\u573a\u6548\u5e94\u8fc1\u79fb\u7387\u4ee5\u53ca\u9ad8\u5bfc\u901a\u7535\u6d41\u3002\u6b64\u5916\uff0c\u57fa\u4e8e\u8fd9\u4e9b\u53cc\u5c42MoS<sub>2<\/sub>\u7684\u9ad8\u6027\u80fd\u5c04\u9891\u6676\u4f53\u7ba1\u88ab\u8bc1\u660e\u5177\u6709\u57fa\u4e8e\u9876\u95e8\u63a7\u5c04\u9891\u6676\u4f53\u7ba1\u521b\u8bb0\u5f55\u7684\u9ad8\u5916\u90e8<em>f<\/em><sub>T<\/sub>\u548c<em>f<\/em><sub>max<\/sub>\u3002\u8be5\u5de5\u4f5c\u5c55\u793a\u4e86CVD\u53cc\u5c42MoS<sub>2<\/sub>\u5728\u9ad8\u9891\u5e94\u7528\u548c\u7075\u6d3b\u65e0\u7ebf\u901a\u4fe1\u65b9\u9762\u7684\u5de8\u5927\u6f5c\u529b\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><a href=\"https:\/\/www.nature.com\/articles\/s41467-018-07135-8\" target=\"_blank\" rel=\"noopener\">Scalable high performance radio frequency electronics based on large domain bilayer MoS<\/a><sub><a href=\"https:\/\/www.nature.com\/articles\/s41467-018-07135-8\" target=\"_blank\" rel=\"noopener\">2<\/a>\u00a0<\/sub>(Nat. Commun. 2018, DOI: 10.1038\/s41467-018-07135-8)<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u751f\u7269\u5b66\u672f\u7ec4biotech\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u5ba1\u6838\u6574\u7406\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6295\u7a3f\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenkefu\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u4e8c\u7ef4\u534a\u5bfc\u4f53\u56e0\u5176\u539f\u5b50\u7ea7\u7684\u8584\u4f53\u548c\u4f18\u5f02\u7684\u8f7d\u4f53\u4f20\u8f93\u6027\u80fd\u800c\u5728\u8bf8\u5982\u4f20\u611f\u5668\u3001\u5b58\u50a8\u5668\u4ee5\u53ca\u903b\u8f91\u5e94\u7528\u7b49\u65b0\u5174\u7684\u7535\u5b50\u4ea7\u54c1\u9886\u57df\u5e94\u7528\u4e2d\u53d7\u5230\u6781\u5927\u7684\u5173\u6ce8\u3002\u65e0\u7ebf\u901a\u4fe1\u4e2d\u7684\u67d4\u6027\u7535\u5b50\u5668\u4ef6\u662f\u76ee&#8230;<\/p>\n","protected":false},"author":7746,"featured_media":159952,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[2780,3737],"class_list":["post-159951","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-mos2","tag-3737"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/159951"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7746"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=159951"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/159951\/revisions"}],"predecessor-version":[{"id":160386,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/159951\/revisions\/160386"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/159952"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=159951"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=159951"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=159951"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}