{"id":162174,"date":"2018-12-20T06:30:09","date_gmt":"2018-12-19T22:30:09","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=162174"},"modified":"2018-12-19T09:53:44","modified_gmt":"2018-12-19T01:53:44","slug":"%e5%8c%97%e4%ba%ac%e5%8c%96%e5%b7%a5%e5%a4%a7%e5%ad%a6%e6%9d%a8%e5%84%92%e3%80%81%e7%8e%8b%e5%b3%b0%e3%80%81%e5%8d%a2%e4%be%a0aem%e7%a6%bb%e5%ad%90%e4%ba%a4%e6%8d%a2%e6%b3%95%e5%88%b6%e5%a4%87","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=162174","title":{"rendered":"\u5317\u4eac\u5316\u5de5\u5927\u5b66\u6768\u5112\u3001\u738b\u5cf0\u3001\u5362\u4fa0AEM:\u79bb\u5b50\u4ea4\u6362\u6cd5\u5236\u5907\u94be\u6c34\u94a0\u9530\u77ff\u53ca\u5176\u50a8\u94be\u3001\u534f\u540c\u6269\u6563\u673a\u7406\u7684\u7814\u7a76"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u53ef\u5145\u7535\u7535\u6c60\u5728\u7535\u5b50\u4ea7\u54c1\u548c\u5927\u89c4\u6a21\u7684\u7535\u80fd\u50a8\u5b58\u65b9\u9762\u626e\u6f14\u7740\u91cd\u8981\u89d2\u8272\uff0c\u4f46\u5728\u5173\u4e8e\u6210\u672c\u548c\u7a33\u5b9a\u6027\u65b9\u9762\u7684\u8bb8\u591a\u95ee\u9898\u4ecd\u672a\u89e3\u51b3\u3002\u5728\u4f17\u591a\u7684\u9502\u79bb\u5b50\u7535\u6c60\u66ff\u4ee3\u8005\u4e2d\uff0c\u7531\u4e8e\u94be(K)\u7684\u4f4e\u6210\u672c\u548c\u8f83\u4f4e\u7684\u6807\u51c6\u7535\u4f4d\uff0c\u94be\u79bb\u5b50\u7535\u6c60\u5728\u4ef7\u683c\u548c\u80fd\u91cf\u5bc6\u5ea6\u65b9\u9762\u5177\u6709\u4e00\u5b9a\u7684\u4f18\u52bf\u3002\u6700\u8fd1\u5bf9\u94be\u79bb\u5b50\u7535\u6c60\u7684\u7814\u7a76\u5c42\u51fa\u4e0d\u7a77\uff0c\u4f46\u5927\u591a\u96c6\u4e2d\u5728\u5bf9\u65b0\u578b\u7535\u6781\u6750\u6599\u7684\u5f00\u53d1\u4e0a\uff0c\u800c\u5bf9\u94be\u79bb\u5b50\u5b58\u50a8\u4e0e\u4f20\u8f93\u673a\u7406\u7684\u7814\u7a76\u5c1a\u7f3a\u5c11\u6df1\u523b\u7684\u8ba4\u8bc6\u3002\u7136\u800c\uff0c\u8fd9\u6070\u6070\u662f\u94be\u79bb\u5b50\u7535\u6c60\u6280\u672f\u53d6\u5f97\u7a81\u7834\u7684\u5173\u952e\u3002<\/p>\n<p>\u6c34\u94a0\u9530\u77ff\u662f\u4e00\u79cd\u5c42\u72b6\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269\uff0c\u5728\u81ea\u7136\u754c\u4e2d\u666e\u904d\u5b58\u5728\uff0c\u5176\u7247\u5c42\u7531\u9530\u6c27\u516b\u9762\u4f53\u00a0MnO<sub>6<\/sub>\u5171\u8fb9\u6216\u5171\u89d2\u6784\u6210\uff0c\u5c42\u95f4\u7531\u6c34\u5206\u5b50\u3001K<sup>+<\/sup>\u76f8\u4e92\u5360\u636e\u586b\u5145\uff0c\u5c42\u95f4\u8ddd\u7ea60.7 nm\uff0c\u5e76\u968f\u5176\u542b\u6c34\u91cf\u548c\u78b1\u91d1\u5c5e\u79bb\u5b50\u7684\u542b\u91cf\u4e0d\u540c\u800c\u6709\u5dee\u5f02\u3002\u5c42\u72b6\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269\u5df2\u88ab\u5e7f\u6cdb\u5e94\u7528\u4e8e\u53ef\u5145\u7535\u7535\u6c60\u7684\u6b63\u6781\u6750\u6599(\u9502\u3001\u94a0\u79bb\u5b50\u7535\u6c60)\uff0c\u7136\u800c\uff0c\u5982\u6b64\u7d27\u51d1\u7684\u6676\u4f53\u7ed3\u6784\u96be\u4ee5\u5bb9\u7eb3\u8f83\u5927\u7684\u94be\u79bb\u5b50\uff0c\u5bfc\u81f4\u521d\u59cb\u6b63\u6781\u6750\u6599\u5177\u6709\u4f4e\u7684\u94be\u542b\u91cf\uff0c\u5982P2-K<sub>0.3<\/sub>MnO<sub>2<\/sub>, P2-K<sub>0.6<\/sub>CoO<sub>2<\/sub>, P3-K<sub>0.5<\/sub>MnO<sub>2<\/sub>\u3002\u94be\u79bb\u5b50\u7535\u6c60\u4f9d\u9760\u94be\u79bb\u5b50\u5728\u6b63\u8d1f\u6781\u4e4b\u95f4\u8131\u5d4c\u6765\u5b58\u50a8\u91ca\u653e\u80fd\u91cf\uff0c\u4f46\u8d1f\u6781\u6750\u6599\u5927\u591a\u4e3a\u4e0d\u542b\u94be\u7684\u6750\u6599\uff0c\u56e0\u6b64\u6b63\u6781\u6750\u6599\u4f5c\u4e3a\u94be\u79bb\u5b50\u7684\u4e3b\u8981\u63d0\u4f9b\u8005\uff0c\u8d2b\u94be\u6750\u6599\u663e\u7136\u4e0d\u662f\u7406\u60f3\u7684\u6b63\u6781\u6750\u6599\uff0c\u94be\u578b\u6c34\u94a0\u9530\u77ff\u4e5f\u53d7\u9650\u4e8e\u6b64\u3002\u79bb\u5b50\u4ea4\u6362\u6cd5\u4f5c\u4e3a\u4e00\u79cd\u5e7f\u6cdb\u7684\u8f6f\u5316\u5b66\u5408\u6210\u65b9\u6cd5\uff0c\u5176\u66fe\u88ab\u7528\u6765\u5728K<sub>0.55<\/sub>CoO<sub>2<\/sub>\u4e2d\u5b9e\u73b0\u94be\u79bb\u5b50\u7684\u8131\u5d4c\uff0c\u56e0\u6b64\u6211\u4eec\u91c7\u7528\u79bb\u5b50\u4ea4\u6362\u6cd5\u589e\u52a0\u94be\u578b\u6c34\u94a0\u9530\u77ff\u4e2d\u94be\u79bb\u5b50\u7684\u542b\u91cf\uff0c\u4ee5\u671f\u63d0\u9ad8\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u94be\u79bb\u5b50\u7684\u6570\u91cf\uff0c\u8fbe\u5230\u6539\u5584\u5176\u7535\u5316\u5b66\u6027\u80fd\u7684\u76ee\u7684\u3002<\/p>\n<p>\u4f20\u7edf\u7684\u79bb\u5b50\u6269\u6563\u662f\u57fa\u4e8e\u5355\u79bb\u5b50\u5728\u76f8\u90bb\u7a7a\u4f4d\u4e4b\u95f4\u8df3\u8dc3\u7684\u6a21\u578b\uff0c\u7136\u800c\u8d2b\u94be\u6750\u6599\u7684\u6676\u4f53\u7ed3\u6784\u4e2d\u5177\u6709\u5927\u91cf\u7684\u94be\u79bb\u5b50\u7a7a\u4f4d\uff0c\u4ece\u800c\u5bfc\u81f4\u94be\u79bb\u5b50\u6269\u6563\u7684\u590d\u6742\u5316\uff0c\u5982\u95f4\u9699\u6269\u6563\u3001\u7fa4\u6269\u6563\u3001\u534f\u540c\u79bb\u5b50\u6269\u6563\u7b49\u7b49\u3002\u5728\u6b64\u5de5\u4f5c\u4e2d\uff0c\u6211\u4eec\u901a\u8fc7\u7b2c\u4e00\u6027\u539f\u7406\uff0c\u9996\u6b21\u5c06\u534f\u540c\u79bb\u5b50\u6269\u6563\u5f15\u5165\u94be\u79bb\u5b50\u7535\u6781\u6750\u6599\u7684\u7814\u7a76\uff0c\u89e3\u91ca\u4e86K-Birnessite\u4f5c\u4e3a\u94be\u79bb\u5b50\u7535\u6c60\u7535\u6781\u6750\u6599\u4f18\u5f02\u7535\u6027\u80fd\u7684\u8d77\u6e90\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u5317\u4eac\u5316\u5de5\u5927\u5b66\u6768\u5112\u6559\u6388\u3001\u738b\u5cf0\u6559\u6388\u3001\u5362\u4fa0\u6559\u6388(\u5171\u540c\u901a\u8baf\u4f5c\u8005)<\/strong>\u7b49\u5408\u4f5c\u5728\u300aAdvanced Energy Materials\u300b\u4e0a\u53d1\u8868\u4e86\u4e00\u7bc7\u540d\u4e3a\u201c<strong>K-Birnessite Electrode Obtained by Ion Exchange for Potassium\u2010Ion Batteries: Insight into the Concerted Ionic Diffusion and K Storage Mechanism<\/strong>\u201d\u7684\u7814\u7a76\u8bba\u6587\u3002\u5728\u8be5\u7814\u7a76\u4e2d\uff0c\u4f5c\u8005\u9996\u5148\u4f7f\u7528\u4f20\u7edf\u7684\u56fa\u76f8\u53cd\u5e94\u63a2\u7d22\u4e86K\u578b\u6c34\u94a0\u9530\u77ff(K-Birnessite)\u7684\u5408\u6210\u6761\u4ef6\uff0c\u8fdb\u800c\u9488\u5bf9\u6b64\u6750\u6599\u4e2d\u94be\u542b\u91cf\u8f83\u4f4e\u7684\u95ee\u9898\uff0c\u91c7\u7528\u79bb\u5b50\u4ea4\u6362\u6cd5(\u5982\u56fe1)\u63d0\u9ad8\u5176\u94be\u542b\u91cf\uff0c\u6b64\u8fc7\u7a0b\u540c\u65f6\u4e5f\u5bf9\u6750\u6599\u7684\u521d\u59cb\u7ed3\u6784\u8d77\u5230\u4e86\u5f88\u597d\u7684\u6d3b\u5316\u4f5c\u7528\u3002\u4f18\u5316\u540e\u7684\u94be\u79bb\u5b50\u7535\u6c60\u7535\u6781\u6750\u6599K-Birnessite<em><i>\u00a0<\/i><\/em>(<em><i>s<\/i><\/em>-KBir)\u57280.2 C\u7684\u500d\u7387\u4e0b\uff0c\u5177\u6709125 mAh g<sup>-1<\/sup>\u7684\u6bd4\u5bb9\u91cf(\u5982\u56fe3)\u3002\u539f\u4f4dXRD\u6280\u672f\u8bba\u8bc1\u4e86\u6b64\u6750\u6599\u5728\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u53ef\u9006\u7684\u7ed3\u6784\u53d8\u5316\uff0c\u5bf9\u7535\u6781\u6750\u6599\u7684\u50a8\u94be\u673a\u5236\u6709\u4e86\u66f4\u6df1\u5165\u7684\u5206\u6790(\u5982\u56fe4)\u3002\u7ed3\u5408\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\u00a0(DFT) \u9996\u6b21\u5c06\u534f\u540c\u79bb\u5b50\u6269\u6563\u673a\u5236(\u5982\u56fe5)\u5f15\u5165\u94be\u79bb\u5b50\u7535\u6c60\u7684\u7814\u7a76\uff0c\u63ed\u793a\u4e86\u5728\u5927\u91cf\u7a7a\u4f4d\u5b58\u5728\u65f6\uff0c\u94be\u79bb\u5b50\u5c06\u4f1a\u4ee5\u534f\u540c\u7684\u65b9\u5f0f\u8fdb\u884c\u6269\u6563\uff0c\u6210\u529f\u89e3\u91ca\u4e86K-Birnessite\u4f5c\u4e3a\u94be\u79bb\u5b50\u7535\u6c60\u7535\u6781\u6750\u6599\u4f18\u5f02\u7535\u6027\u80fd\u7684\u8d77\u6e90\u3002\u540c\u65f6\uff0c\u6b64\u7406\u8bba\u4e5f\u52a0\u6df1\u4e86\u5bf9\u56fa\u6001\u79bb\u5b50\u53ca\u7535\u6c60\u7535\u6781\u8fc7\u7a0b\u52a8\u529b\u5b66\u7684\u7406\u89e3\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>1 <\/b><\/strong><strong><b>\u4e0d\u540c\u56fa\u76f8\u5408\u6210\u6e29\u5ea6\u4e0d\u540c<\/b><\/strong><strong><b>K\/Mn<\/b><\/strong><strong><b>\u6469\u5c14\u914d\u6bd4\u6837\u54c1\u7684<\/b><\/strong><strong><b>XRD<\/b><\/strong><strong><b>\u56fe<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162175 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72471-12.png\" alt=\"\" width=\"600\" height=\"297\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72471-12.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72471-12-300x149.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>2 \u00a0<\/b><\/strong>K-Birnessite<strong><b>\u76f8\u56fe<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162176 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72472-12.png\" alt=\"\" width=\"469\" height=\"356\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72472-12.png 469w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72472-12-300x228.png 300w\" sizes=\"(max-width: 469px) 100vw, 469px\" \/><\/b><\/strong><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>3 <\/b><\/strong><strong><b>\u79bb\u5b50\u4ea4\u6362\u8fc7\u7a0b\u793a\u610f\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162177 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72473-12.png\" alt=\"\" width=\"600\" height=\"396\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72473-12.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72473-12-300x198.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4 <\/b><\/strong><strong><b>\u6c34\u6eb6\u6db2\u4f53\u7cfb\u79bb\u5b50\u4ea4\u6362\u6837\u54c1<\/b><\/strong><strong><b>(<\/b><\/strong><strong><em><b><i>s<\/i><\/b><\/em><\/strong><strong><b>-KBir<\/b><\/strong><strong><b>)<\/b><\/strong><strong><b>\u7684\u7ed3\u6784\u8868\u5f81<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162178 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72474-12.png\" alt=\"\" width=\"600\" height=\"479\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72474-12.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72474-12-300x240.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) <em><i>s<\/i><\/em>-KBir \u7684\u7cbe\u4feeXRD\u56fe\uff1b<\/p>\n<p>(b,c) <em><i>s<\/i><\/em>-KBir \u7684\u539f\u5b50\u7ed3\u6784\u793a\u610f\u56fe\uff1b<\/p>\n<p>(d) <em><i>s<\/i><\/em>-KBir \u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>(e,f) <em><i>s<\/i><\/em>-KBir \u7684HRTEM\u56fe\u50cf\uff1b<\/p>\n<p>(g) <em><i>s<\/i><\/em>-KBir \u7684STEM\u56fe\u50cf\uff1b<\/p>\n<p>(h-k) <em><i>s<\/i><\/em>-KBir \u7684EDS\u5143\u7d20\u5206\u5e03\u56fe\u50cf\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>5 \u00a0<\/b><\/strong><strong><b>K<\/b><\/strong><strong><b>&#8211;<\/b><\/strong><strong><b>Birnessite<\/b><\/strong><strong><b>\u7684\u7535\u5316\u5b66\u6027\u80fd<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162179 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72475-12.png\" alt=\"\" width=\"600\" height=\"451\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72475-12.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72475-12-300x226.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u00a0\u79bb\u5b50\u4ea4\u6362\u524d\u540e\u6837\u54c1\u7684\u9996\u5708\u5145\/\u653e\u7535\u66f2\u7ebf\uff1bKBir:\u672a\u7ecf\u79bb\u5b50\u4ea4\u6362\u7684\u6837\u54c1\uff1b<em><i>s<\/i><\/em>-KBir\uff1a\u6c34\u6eb6\u6db2\u57fa\u79bb\u5b50\u4ea4\u6362\u6837\u54c1\uff1b<em><i>h<\/i><\/em>-KBir\uff1a\u9ad8\u6e29\u79bb\u5b50\u4ea4\u6362\u6837\u54c1\uff1b<\/p>\n<p>(b) <em><i>s<\/i><\/em>-KBir\u7684\u524d\u4e09\u5708\u5faa\u73af\u4f0f\u5b89\u66f2\u7ebf\u00a0(0.1 mV s<sup>-1<\/sup>);<\/p>\n<p>(c) <em><i>s<\/i><\/em>-KBir\u57280.2C\u4e0b\u7684\u7535\u538b\u5bb9\u91cf\u66f2\u7ebf\uff1b<\/p>\n<p>(d) <em><i>s<\/i><\/em>-KBir\u4e0d\u540c\u500d\u7387\u4e0b\u7684\u5faa\u73af\u6027\u80fd\u3002<\/p>\n<p><strong><b>\u00a0<\/b><\/strong><strong><b>\u56fe<\/b><\/strong><strong><b>6 \u00a0<\/b><\/strong><strong><em><b><i>s<\/i><\/b><\/em><\/strong><strong><b>-KBir<\/b><\/strong><strong><b>\u7535\u6781\u524d\u4e24\u5708\u5145\u653e\u7535\u7684\u539f\u4f4d<\/b><\/strong><strong><b>XRD<\/b><\/strong><strong><b>\u8868\u5f81<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162180 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72476-10.png\" alt=\"\" width=\"600\" height=\"443\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72476-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72476-10-300x222.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u5145\/\u653e\u7535\u66f2\u7ebf(5 mA g<sup>-1<\/sup>);<\/p>\n<p>(b) <em><i>s<\/i><\/em>-KBir\u7684\u539f\u4f4dXRD\u56fe\u8c31\uff1b<\/p>\n<p>(c) \u653e\u5927\u7684(004)\u5cf0\u3002<\/p>\n<p><strong><b>\u00a0<\/b><\/strong><strong><b>\u56fe<\/b><\/strong><strong><b>7 <\/b><\/strong><strong><b>\u94be\u79bb\u5b50\u534f\u540c\u6269\u6563<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162181 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72477-11.png\" alt=\"\" width=\"600\" height=\"519\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72477-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72477-11-300x260.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u4f18\u5316\u7684P2-K<sub>0.3<\/sub>MnO<sub>2<\/sub>\u7ed3\u6784\u793a\u610f\u56fe\uff0c\u53ca6\u79cd\u94be\u79bb\u5b50\u4f20\u8f93\u8def\u5f84\uff1b\u2160\uff1a\u5355\u79bb\u5b50\u6cbfb\u8f74\u65b9\u5411\u8df3\u8dc3\uff1b\u2161: \u53cc\u79bb\u5b50\u540c\u65f6\u6cbfb\u8f74\u65b9\u5411\u8df3\u8dc3\uff1b\u2162: \u4e09\u79bb\u5b50\u540c\u65f6\u6cbfb\u8f74\u65b9\u5411\u8df3\u8dc3\uff1b\u2163: \u53cc\u79bb\u5b50\u540c\u65f6\u6cbfa\u8f74\u65b9\u5411\u8df3\u8dc3\uff1b\u2164: \u57fa\u4e8e\u8def\u5f84\u2163\uff0c\u53cc\u79bb\u5b50\u540c\u65f6\u6cbfa\u8f74\u65b9\u5411\u8df3\u8dc3\uff1b\u2165: \u4e09\u79bb\u5b50\u540c\u65f6\u6cbfa\u8f74\u65b9\u5411\u8df3\u8dc3\uff1b<\/p>\n<p>(b) \u91c7\u7528CI-NEB\u65b9\u6cd5\u5f97\u51fa\u7684\u4e0d\u540c\u8def\u5f84\u7684\u80fd\u5792\u3002<\/p>\n<p><strong><b>TOC Figure<\/b><\/strong><strong><b>: <\/b><\/strong>\u534f\u540c\u79bb\u5b50\u6269\u6563\u793a\u610f\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162182 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72478-9.png\" alt=\"\" width=\"600\" height=\"444\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72478-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72478-9-300x222.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>8 <\/b><\/strong><strong><b>P2-K<\/b><\/strong><strong><em><sub><b><i>x<\/i><\/b><\/sub><\/em><\/strong><strong><b>MnO<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u00a0(<\/b><\/strong><strong><em><b><i>x<\/i><\/b><\/em><\/strong><strong><b>\u00a0= 0.125, 0.25, 0.50 ,0.75 and 1) <\/b><\/strong><strong><b>\u4e2d<\/b><\/strong><strong><b>Mn-O<\/b><\/strong><strong><b>\u952e\u7684\u53d8\u5316<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162183 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72479-6.png\" alt=\"\" width=\"600\" height=\"317\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72479-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u72479-6-300x159.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>9 K\/Mn<\/b><\/strong><strong><b>\u4e92\u5360\u4f4d\u7684\u7814\u7a76<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-162184 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u724710-6.png\" alt=\"\" width=\"600\" height=\"278\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u724710-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/\u56fe\u724710-6-300x139.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u3010\u603b\u7ed3\u3011<\/b><\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u4f5c\u8005\u901a\u8fc7\u4f20\u7edf\u7684\u56fa\u76f8\u53cd\u5e94\u53ca\u968f\u540e\u7684\u79bb\u5b50\u4ea4\u6362\u65b9\u6cd5\u5236\u5907\u4e86K\u578b\u6c34\u94a0\u9530\u77ff(K-Birnessite)\uff1b\u5176\u5177\u6709\u4f18\u5f02\u7684\u7535\u5316\u5b66\u6027\u80fd\uff0c\u57280.2 C\u7684\u500d\u7387\u4e0b\u5177\u6709125 mAh g<sup>-1<\/sup>\u7684\u6bd4\u5bb9\u91cf\uff1b\u4e14\u539f\u4f4dXRD\u6280\u672f\u8bba\u8bc1\u4e86\u6b64\u6750\u6599\u5728\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u53ef\u9006\u7684\u7ed3\u6784\u53d8\u5316\u3002\u7ed3\u5408\u7b2c\u4e00\u6027\u539f\u7406\u8ba1\u7b97\u00a0(DFT) \u9996\u6b21\u5c06\u534f\u540c\u79bb\u5b50\u6269\u6563\u673a\u5236\u5f15\u5165\u94be\u79bb\u5b50\u7535\u6c60\u7684\u7814\u7a76\uff0c\u6b64\u7406\u8bba\u52a0\u6df1\u4e86\u5bf9\u56fa\u6001\u79bb\u5b50\u53ca\u7535\u6c60\u7535\u6781\u8fc7\u7a0b\u52a8\u529b\u5b66\u7684\u7406\u89e3\u3002\u4f5c\u8005\u7684\u5de5\u4f5c\u8868\u660e\uff0cK-Birnessite\u662f\u4e00\u79cd\u975e\u5e38\u6709\u524d\u666f\u7684\u9ad8\u6027\u80fd\u94be\u79bb\u5b50\u7535\u6c60\u7535\u6781\uff0c\u76f8\u4fe1\u8fd9\u4e00\u65b0\u9896\u7684\u7b56\u7565\u53ef\u7528\u4e8e\u5f00\u53d1\u5927\u89c4\u6a21\u50a8\u80fd\u5e94\u7528\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong>K-Birnessite Electrode Obtained by Ion Exchange for Potassium-Ion Batteries: Insight into the Concerted Ionic Diffusion and K Storage Mechanism (<em><i>Adv. Energy Mater<\/i><\/em>., 2018, DOI: 10.1002\/aenm.201802739)<\/p>\n<p><strong><b>\u81f4\u8c22\uff1a<\/b><\/strong><\/p>\n<p>\u6b64\u5de5\u4f5c\u5f97\u5230\u4e86\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1(51772017, 51372012, 51432003, 11704019)\u548c\u6709\u673a-\u65e0\u673a\u590d\u5408\u6750\u6599\u56fd\u5bb6\u91cd\u70b9\u5b9e\u9a8c\u5ba4(oic-201701011)\u7684\u652f\u6301\u3002\u76f8\u5173\u8ba1\u7b97\u5de5\u4f5c\u5728\u56fd\u5bb6\u8d85\u7ea7\u8ba1\u7b97\u5929\u6d25\u4e2d\u5fc3(TianHe-1(A)) \u5b8c\u6210\u3002<\/p>\n<p>\u672c\u6587\u7531<strong>\u5317\u4eac\u5316\u5de5\u5927\u5b66\u6768\u5112\u6559\u6388<\/strong><strong><b>\u56e2\u961f<\/b><\/strong>\u4f9b\u7a3f\uff0c\u7f16\u8f91\u90e8\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p><strong><b>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP<\/b><\/strong><\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u53ef\u5145\u7535\u7535\u6c60\u5728\u7535\u5b50\u4ea7\u54c1\u548c\u5927\u89c4\u6a21\u7684\u7535\u80fd\u50a8\u5b58\u65b9\u9762\u626e\u6f14\u7740\u91cd\u8981\u89d2\u8272\uff0c\u4f46\u5728\u5173\u4e8e\u6210\u672c\u548c\u7a33\u5b9a\u6027\u65b9\u9762\u7684\u8bb8\u591a\u95ee\u9898\u4ecd\u672a\u89e3\u51b3\u3002\u5728\u4f17\u591a\u7684\u9502\u79bb\u5b50\u7535\u6c60\u66ff\u4ee3\u8005\u4e2d\uff0c\u7531\u4e8e\u94be(K)\u7684\u4f4e\u6210\u672c&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-162174","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/162174"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=162174"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/162174\/revisions"}],"predecessor-version":[{"id":162202,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/162174\/revisions\/162202"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=162174"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=162174"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=162174"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}