{"id":162394,"date":"2018-12-24T06:30:26","date_gmt":"2018-12-23T22:30:26","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=162394"},"modified":"2018-12-24T20:56:33","modified_gmt":"2018-12-24T12:56:33","slug":"%e5%a4%a9%e6%b4%a5%e5%a4%a7%e5%ad%a6%e5%b7%a9%e9%87%91%e9%be%99chem-soc-rev-%ef%bc%9a%e6%a0%b8%e5%a3%b3%e7%ba%b3%e7%b1%b3%e7%bb%93%e6%9e%84%e7%9a%84%e6%9e%84%e7%ad%91%e3%80%81%e5%85%89%e5%82%ac","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=162394","title":{"rendered":"\u5929\u6d25\u5927\u5b66\u5de9\u91d1\u9f99Chem. Soc. Rev.\uff1a\u6838\u58f3\u7eb3\u7c73\u7ed3\u6784\u7684\u6784\u7b51\u3001\u5149\u50ac\u5316\u5e94\u7528\u53ca\u5e94\u7528\u524d\u666f"},"content":{"rendered":"<p><strong>\u3010\u7814\u7a76\u80cc\u666f\u3011<\/strong><\/p>\n<p>\u5149\u50ac\u5316\u662f\u5c06\u592a\u9633\u80fd\u76f4\u63a5\u8f6c\u5316\u4e3a\u5316\u5b66\u80fd\u7684\u6709\u524d\u9014\u7684\u9014\u5f84\uff0c\u4e3a\u73af\u5883\u548c\u81ea\u7136\u8d44\u6e90\u95ee\u9898\u63d0\u4f9b\u4e86\u66ff\u4ee3\u89e3\u51b3\u65b9\u6848\u3002\u7406\u8bba\u4e0a\uff0c\u6240\u6709\u5149\u50ac\u5316\u53cd\u5e94\u90fd\u662f\u7531\u7535\u8377\u8f7d\u4f53\u9a71\u52a8\u7684\uff0c\u7535\u8377\u8f7d\u4f53\u7684\u884c\u4e3a\u53ef\u5206\u4e3a\u7535\u8377\u4ea7\u751f\u3001\u5206\u79bb\u3001\u8fc1\u79fb\u548c\u8868\u9762\u53cd\u5e94\u3002\u6bcf\u4e2a\u6b65\u9aa4\u4e2d\u7535\u8377\u5229\u7528\u7684\u6548\u7387\u51b3\u5b9a\u4e86\u5149\u50ac\u5316\u7684\u6574\u4f53\u6027\u80fd\u3002\u6838\u58f3\uff08YS\uff09\u7ed3\u6784\u53ef\u4ee5\u4e3a\u7535\u8377\u8f7d\u4f53\u7684\u6709\u6548\u5229\u7528\u63d0\u4f9b\u7406\u60f3\u7684\u5e73\u53f0\u3002\u901a\u5e38\uff0c\u6838\u58f3\u7ed3\u6784\u7531\u4e2d\u7a7a\u58f3\u548c\u5185\u82af\u6784\u6210\uff0c\u5176\u53ef\u4ee5\u589e\u5f3a\u4e2d\u7a7a\u7a7a\u95f4\u4e2d\u7684\u5149\u6563\u5c04\u5e76\u63d0\u4f9b\u5927\u8868\u9762\u4ee5\u4ea7\u751f\u8db3\u591f\u7684\u6d3b\u6027\u4f4d\u70b9\uff0c\u8fd9\u4e24\u8005\u90fd\u53ef\u4ee5\u663e\u7740\u63d0\u9ad8\u7535\u8377\u5229\u7528\u7684\u6548\u7387\u3002\u53e6\u5916\uff0c\u53ef\u4ee5\u91c7\u7528\u8bb8\u591a\u7b56\u7565\u6765\u6539\u9020\u6838\u58f3\u7ed3\u6784\uff0c\u4ee5\u8fdb\u4e00\u6b65\u589e\u5f3a\u6bcf\u4e2a\u6b65\u9aa4\u4e2d\u7684\u7535\u8377\u884c\u4e3a\u3002\u5173\u4e8e\u6838\u58f3\u7ed3\u6784\u7684\u73b0\u6709\u7efc\u8ff0\u4e3b\u8981\u96c6\u4e2d\u5728\u6838\u58f3\u5e94\u7528\u7684\u666e\u904d\u6027\uff0c\u800c\u57fa\u4e8e\u6838\u58f3\u7684\u6539\u5584\u5149\u50ac\u5316\u6027\u80fd\u7684\u7b56\u7565\u5c1a\u672a\u5f97\u5230\u8be6\u7ec6\u8bf4\u660e\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u5929\u6d25\u5927\u5b66\u5de9\u91d1\u9f99\u6559\u6388<\/strong>\u4ece\u63d0\u9ad8\u5149\u50ac\u5316\u6027\u80fd\u7684\u7b56\u7565\u8be6\u7ec6\u9610\u8ff0\u4e86\u6838\u58f3\u7ed3\u6784\uff0c\u5e76\u6982\u8ff0\u4e86\u6838\u58f3\u7ed3\u6784\u7684\u5206\u7c7b\uff0c\u5408\u6210\uff0c\u5f62\u6210\u673a\u5236\u548c\u5149\u751f\u8f7d\u6d41\u5b50\u884c\u4e3a\u7684\u5408\u7406\u8c03\u63a7\uff0c\u4ee5\u5b9e\u73b0\u975e\u5747\u76f8\u5149\u50ac\u5316\u53cd\u5e94\u4e2d\u6838\u58f3\u7ed3\u6784\u7684\u6709\u6548\u5229\u7528\u3002\u6700\u540e\uff0c\u4f5c\u8005\u63d0\u51fa\u6838\u58f3\u7ed3\u6784\u4ee5\u540e\u7684\u53d1\u5c55\u65b9\u5411\u4f1a\u5728\u5149\u50ac\u5316\u6c34\u5206\u89e3\u3001CRR\u3001\u4e0e\u5355\u539f\u5b50\u50ac\u5316\u7ed3\u5408\u3001\u4ee5\u53ca\u7814\u7a76\u5149\u53cd\u5e94\u8fc7\u7a0b\u4e2d\u5f62\u6210\u6838\u58f3\u7684\u539f\u5b50\u7ea7\u673a\u5236\u548c\u7535\u8377\u4f20\u8f93\u7684\u65f6\u95f4\u5206\u8fa8\u8fc7\u7a0b\u3002\u8be5\u6210\u679c\u8fd1\u65e5\u4ee5\u9898\u4e3a\u201c<strong>Rational design of yolk\u2013shell nanostructures for photocatalysis<\/strong>\u201d\u53d1\u8868\u5728\u77e5\u540d\u7efc\u8ff0<strong>Chem. Soc. Rev.<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00\uff1a\u534a\u5bfc\u4f53\u5149\u50ac\u5316\u5242\u7684\u5b8c\u6574\u50ac\u5316\u8fc7\u7a0b\uff08\u4e00\u3001\u5149\u8f90\u5c04\u4ea7\u751f\u8f7d\u6d41\u5b50\uff1b\u4e8c\u3001\u7535\u5b50\u548c\u7a7a\u7a74\u8fc1\u79fb\u5230\u50ac\u5316\u5242\u8868\u9762\uff1b\u4e09\u3001\u8868\u9762\u53cd\u5e94\uff09<\/strong><br \/>\n <img decoding=\"async\" class=\"aligncenter size-full wp-image-162395\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/1.tiff\" alt=\"\" \/><a href=\"http:\/\/www.cailiaoniu.com\" rel=\"attachment wp-att-162398\"><img decoding=\"async\" class=\"aligncenter size-full wp-image-162398\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/1.tiff\" alt=\"\" \/><\/a><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162414\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/1-25.jpg\" alt=\"\" width=\"600\" height=\"228\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/1-25.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/1-25-300x114.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a) \u5149\u50ac\u5316\u534a\u5bfc\u4f53\u7684\u80fd\u5e26\u7ed3\u6784\uff0c\u4ee5\u53ca\u7535\u8377\u4ea7\u751f\u548c\u6c27\u5316\u8fd8\u539f\u53cd\u5e94\u7684\u673a\u7406\uff1b<br \/>\n (b) \u591a\u76f8\u5149\u50ac\u5316\u7684\u5178\u578b\u7ed3\u6784\u548c\u5149\u50ac\u5316\u8fc7\u7a0b\u4e2d\u8f7d\u6d41\u5b50\u884c\u4e3a\u7684\u6b65\u9aa4\u3002<\/p>\n<p><strong>\u56fe\u4e8c\uff1a\u4e2d\u7a7a\u7ed3\u6784\u88ab\u8ba4\u4e3a\u662f\u6700\u7279\u6b8a\u4e00\u79cd\u6838\u58f3\u7ed3\u6784<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162415\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/2-27.jpg\" alt=\"\" width=\"600\" height=\"369\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/2-27.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/2-27-300x185.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u5404\u79cd\u7c7b\u578b\u6838\u58f3\u7ed3\u6784\u6750\u6599\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u4e09\uff1a\u67ef\u80af\u7279\u5c14\u6548\u5e94\u89e3\u91ca\u90e8\u5206\u7a7a\u5fc3\u7ed3\u6784\u4e2d\u7a7a\u9699\u7a7a\u95f4\u7684\u5f62\u6210<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162416\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/3-29.jpg\" alt=\"\" width=\"600\" height=\"416\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/3-29.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/3-29-300x208.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a-b) \u4e24\u79cd\u4e0d\u540c\u6750\u6599\u6216\u76f8A\u548cB\u4e4b\u95f4\u7684\u67ef\u80af\u7279\u5c14\u6548\u5e94\u793a\u610f\u56fe\uff1b<br \/>\n (c) \u7eb3\u7c73\u5c3a\u5ea6\u67ef\u514b\u5170\u5fb7\u5c14\u6548\u5e94\u5f62\u6210\u7a7a\u5fc3\u7eb3\u7c73\u6676\u4f53\u7684\u793a\u610f\u56fe\uff1b<br \/>\n (d-m) \u4e0d\u540c\u63ba\u6742\u53ca\u4e0d\u540c\u65f6\u95f4\u94b4\u7eb3\u7c73\u6676\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u56db\uff1a\u5965\u65af\u74e6\u5c14\u5fb7\u719f\u5316<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162417\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/4-25.jpg\" alt=\"\" width=\"600\" height=\"1217\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/4-25.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/4-25-148x300.jpg 148w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/4-25-505x1024.jpg 505w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a) \u5965\u65af\u7279\u74e6\u5c14\u5fb7\u719f\u5316\u7684\u4e00\u822c\u8fc7\u7a0b\uff1b<br \/>\n (b-e) \u5404\u79cd\u7403\u5f62\u80f6\u88c5\u805a\u96c6\u4f53\u7684\u5965\u65af\u7279\u74e6\u5c14\u5fb7\u719f\u5316\u793a\u610f\u56fe\uff1b<br \/>\n (f) \u65cb\u8f6c\u7684\u6838\uff1b<br \/>\n (g) \u534a\u7a7a\u5fc3\u6838\u58f3\u7ed3\u6784\u7684\u8d28\u91cf\u4e2d\u5fc3\uff1b<br \/>\n (h) \u56fe\uff08c\uff09\u4e2d\u53ef\u80fd\u7684\u6a21\u578b\u7528\u4e8e\u5728\u6838\u548c\u58f3\u4e4b\u95f4\u5f62\u6210\u7a7a\u9699\u7a7a\u95f4\uff1b<br \/>\n (i-k) \u5965\u65af\u7279\u74e6\u5c14\u5fb7\u719f\u5316\u4e0d\u540c\u65f6\u95f4\u7684ZnS\u6838\u58f3\u7ed3\u6784TEM\u56fe\u50cf\uff1b<br \/>\n (l-n) \u5965\u65af\u7279\u74e6\u5c14\u5fb7\u719f\u531624h\u540e\u7684Co<sub>3<\/sub>O<sub>4<\/sub>\u6838\u58f3\u7ed3\u6784TEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u4e94\uff1a\u786c\u6a21\u677f\u6cd5\u5408\u6210\u6838\u58f3\u7ed3\u6784<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162418\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/5-22.jpg\" alt=\"\" width=\"600\" height=\"388\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/5-22.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/5-22-300x194.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u4e0d\u540c\u7c7b\u578b\u7684\u786c\u6a21\u677f\u6cd5\u5408\u6210\u6838\u58f3\u7ed3\u6784\u6750\u6599\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u516d\uff1a\u786c\u6a21\u677f\u6cd5\u5408\u6210\u6838\u58f3\u7ed3\u6784<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162419\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/6-10.jpg\" alt=\"\" width=\"600\" height=\"998\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/6-10.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/6-10-180x300.jpg 180w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a-f) \u7b2c\u4e00\u7c7b\u578b\u7684\u786c\u6a21\u677f\u6cd5\u5408\u6210\u8fc7\u7a0b\u53ca\u6750\u6599TEM\u56fe\u50cf\uff1b<br \/>\n (g-l) \u7b2c\u4e8c\u7c7b\u578b\u7684\u786c\u6a21\u677f\u6cd5\u5408\u6210\u8fc7\u7a0b\u53ca\u6750\u6599TEM\u56fe\u50cf\uff1b<br \/>\n (m-t) \u7b2c\u4e09\u7c7b\u578b\u7684\u786c\u6a21\u677f\u6cd5\u5408\u6210\u8fc7\u7a0b\u53ca\u6750\u6599TEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u4e03\uff1a\u8f6f\u6a21\u677f\u6cd5\u5408\u6210\u6838\u58f3\u7ed3\u6784<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162420\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/7-6.jpg\" alt=\"\" width=\"600\" height=\"213\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/7-6.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/7-6-300x107.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u4f7f\u7528\u8868\u9762\u6d3b\u6027\u5242\u4f5c\u4e3a\u6a21\u677f\u7684\u5178\u578b\u8f6f\u6a21\u677f\u7684\u793a\u610f\u56fe\u53ca\u4e0d\u540cSiO<sub>2<\/sub>\u58f3\u7ed3\u6784\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u516b\uff1a\u8f6f\u6a21\u677f\u6cd5\u5408\u6210\u591a\u58f3\u7ed3\u6784<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162425\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/8-5.jpg\" alt=\"\" width=\"600\" height=\"371\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/8-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/8-5-300x186.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u57fa\u4e8e\u8868\u9762\u6d3b\u6027\u5242\u7684\u8f6f\u6a21\u677f\u65b9\u6cd5\u5408\u6210\u5177\u6709\u591a\u58f3\u7684\u6838\u58f3\u7ed3\u6784\u6750\u6599\u53ca\u5176TEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u4e5d\uff1a\u4e73\u6db2\u4e3a\u6a21\u677f\u7684\u8f6f\u6a21\u677f\u6cd5<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162426\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/9-5.jpg\" alt=\"\" width=\"600\" height=\"340\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/9-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/9-5-300x170.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u4f7f\u7528\u4e73\u6db2\u4f5c\u4e3a\u6a21\u677f\u7684\u8f6f\u6a21\u677f\u6cd5\u5408\u6210TiO<sub>2<\/sub>@SiO<sub>2<\/sub>\u6838\u58f3\u7ed3\u6784\u6750\u6599\uff0cAu@SiO<sub>2<\/sub>\u6838\u58f3\u7ed3\u6784\u6750\u6599\u53ca\u5176TEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u5341\uff1a\u8d85\u58f0\u6ce2\u55b7\u96fe\u70ed\u89e3\u8f6f\u6a21\u677f\u6cd5<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162427\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/10-4.jpg\" alt=\"\" width=\"600\" height=\"491\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/10-4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/10-4-300x246.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u57fa\u4e8e\u6c14\u6eb6\u80f6\u7684\u55b7\u96fe\u70ed\u89e3\u65b9\u6cd5\u7684\u793a\u610f\u56fe\u53ca\u5236\u5907\u7684Fe<sub>2<\/sub>O<sub>3<\/sub>@Fe<sub>2<\/sub>O<sub>3<\/sub>\u6750\u6599\u7684\u8868\u5f81\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e00\uff1a\u201c\u74f6\u4e2d\u9020\u8239\u201d\u6cd5\u5408\u6210\u591a\u58f3\u7ed3\u6784<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162428\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/11-3.jpg\" alt=\"\" width=\"600\" height=\"799\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/11-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/11-3-225x300.jpg 225w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u201c\u74f6\u4e2d\u9020\u8239\u201d\u6cd5\u539f\u4f4d\u5408\u6210\u793a\u610f\u56fe\u53ca\u5176\u8868\u5f81\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e8c\uff1a\u57fa\u672c\u65b9\u6cd5\u7684\u7ed3\u5408<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162429\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/12-4.jpg\" alt=\"\" width=\"600\" height=\"194\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/12-4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/12-4-300x97.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u7ed3\u5408\u4e86\u786c\u6a21\u677f\uff0c\u8f6f\u6a21\u677f\uff0c\u6c34\u70ed\u6cd5\u548c\u201c\u74f6\u4e2d\u9020\u8239\u201d\u6cd5\u5408\u6210TiO<sub>2<\/sub>@TiO<sub>2<\/sub>\u53cc\u58f3\u7ed3\u6784\u53caTEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e09\uff1a\u6563\u5c04\u589e\u5f3a\u589e\u5f3a\u7535\u8377\u4ea7\u751f<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162430\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/13-3.jpg\" alt=\"\" width=\"600\" height=\"425\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/13-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/13-3-300x213.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a-d) \u56fa\u4f53\u9897\u7c92\uff0c\u5355\u6838\u6838-\u58f3\u7ed3\u6784\uff0c\u53cc\u58f3\u7ed3\u6784\u548c\u591a\u58f3\u7ed3\u6784\u7684\u5149\u6563\u5c04\u5f62\u5f0f\u7684\u793a\u610f\u56fe\uff1b<br \/>\n (e-h) \u4e0d\u540c\u7ed3\u6784\u4e0d\u540c\u6fc0\u6d3b\u7684\u6838\u58f3\u7ed3\u6784\u53ca\u5176\u534f\u540c\u4fc3\u8fdb\u5149\u50ac\u5316\u4f5c\u7528\u3002<\/p>\n<p><strong>\u56fe\u5341\u56db\uff1a\u5c40\u57df\u8868\u9762\u7b49\u79bb\u5b50\u4f53\u5171\u632f\u589e\u5f3a\u7535\u8377\u4ea7\u751f<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162431\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/14-2.jpg\" alt=\"\" width=\"600\" height=\"392\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/14-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/14-2-300x196.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a) \u7b49\u79bb\u5b50\u4f53\u7c92\u5b50\u4e0a\u7684\u7b49\u79bb\u5b50\u4f53\u632f\u8361\u793a\u610f\u56fe\uff1b<br \/>\n (b) \u589e\u5f3a\u7b49\u79bb\u5b50\u4f53\u6750\u6599\u5149\u50ac\u5316\u4f5c\u7528\u7684\u4e09\u79cd\u673a\u5236\u793a\u610f\u56fe\uff1b<br \/>\n (c-e) \u70ed\u7535\u5b50\u6ce8\u5165\u7684\u5f71\u54cd\u7684\u7cbe\u7ec6\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e94\uff1a\u63ba\u6742\u589e\u5f3a\u7535\u8377\u4ea7\u751f<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162432\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/15.jpg\" alt=\"\" width=\"600\" height=\"1382\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/15.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/15-130x300.jpg 130w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/15-445x1024.jpg 445w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a) \u63ba\u6742N\u548cFe\u4e4b\u540e\u7684TiO<sub>2<\/sub>\u80fd\u5e26\u7ed3\u6784\u53d8\u5316\uff1b<br \/>\n (b) \u63ba\u6742Ti<sup>3+<\/sup>\u540e\u6c27\u7a7a\u4f4d\u7684\u53d8\u5316\u5bfc\u81f4Eg\u53d8\u7a84\uff1b<br \/>\n (c) \u5728Eg\u4e2d\u521b\u5efa\u7a7a\u4f4d\u7ed9\u7535\u5b50\u63d0\u4f9b\u8df3\u677f\u3002<\/p>\n<p><strong>\u56fe\u5341\u516d\uff1a\u4e0a\u8f6c\u6362\u7eb3\u7c73\u7c92\u5b50\u6838\u58f3\u7ed3\u6784\u7528\u4e8e\u5149\u50ac\u5316\u53cd\u5e94<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162433\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/16.jpg\" alt=\"\" width=\"600\" height=\"525\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/16.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/16-300x263.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n UCNP@Zn<sub>x<\/sub>Cd<sub>1-x<\/sub>S\u5728NIR\u5149\u7167\u5c04\u4e0b\u4fc3\u8fdb\u5149\u50ac\u5316\u53cd\u5e94\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e03\uff1a\u5f02\u8d28\u7ed3\u4fc3\u8fdb\u7535\u8377\u5206\u79bb\u548c\u8fc1\u79fb<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162434\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/17.jpg\" alt=\"\" width=\"600\" height=\"427\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/17.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/17-300x214.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u4e0d\u540c\u6750\u6599\u4e4b\u95f4\u7684\u5f02\u8d28\u7ed3\uff0cp-n\u7ed3\uff0c\u540c\u8d28\u7ed3\u80fd\u5e26\u7ed3\u6784\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u5341\u516b\uff1a \u4e0d\u540c\u6838\u58f3\u6750\u6599\u5f02\u8d28\u7ed3\u7684\u6784\u7b51<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162435\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/18.jpg\" alt=\"\" width=\"600\" height=\"728\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/18.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/18-247x300.jpg 247w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u4e0d\u540c\u7c7b\u578b\u5f02\u8d28\u7ed3\u7684\u6838\u58f3\u7ed3\u6784\uff08\u8868\u5f81\u53ca\u80fd\u5e26\u7ed3\u6784\uff09\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e5d\uff1a\u5171\u50ac\u5316\u5242\u7684\u8d1f\u8f7d\u548c\u7a7a\u95f4\u5206\u79bb<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162437\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/19.jpg\" alt=\"\" width=\"600\" height=\"423\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/19.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/19-300x212.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \uff08\u4e0a\uff09\u52a9\u50ac\u5316\u5242\u5206\u79bb\u7684\u6838\u58f3\u7ed3\u6784\u50ac\u5316\u5242\uff1aPt@TiO<sub>2<\/sub>@MnO<sub>x<\/sub><br \/>\n \uff08\u4e0b\uff09\u542b\u8584\u58f3\u5f02\u8d28\u7ed3\u7684\u52a9\u50ac\u5316\u5242\u5206\u79bb\u7684\u6838\u58f3\u7ed3\u6784\u50ac\u5316\u5242\uff1aPt@TiO<sub>2<\/sub>@In<sub>2<\/sub>O<sub>3<\/sub>@MnO<sub>x<\/sub><\/p>\n<p><strong>\u56fe\u4e8c\u5341\uff1a\u6d3b\u6027\u4f4d\u70b9\u7684\u7a7a\u95f4\u5206\u79bb<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162438\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/20.jpg\" alt=\"\" width=\"600\" height=\"190\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/20.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/20-300x95.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n (a) \u4ee5\u5bfc\u7535SiO<sub>2<\/sub>\u7a7a\u5fc3\u58f3\u4e3a\u5e73\u53f0\u5206\u79bb\u4e0d\u540c\u53cd\u5e94\u4f4d\u70b9\uff0c\u6291\u5236\u6574\u4f53\u5149\u50ac\u5316CO<sub>2<\/sub>\u8fd8\u539f\u7684\u4ea4\u53c9\u53cd\u5e94\uff1b<br \/>\n (b) \u4e0d\u540c\u7684\u53cd\u5e94\u4f4d\u70b9\u5b8c\u5168\u5206\u79bbCO<sub>2<\/sub>\u5149\u8fd8\u539f\u751f\u6210CH<sub>3<\/sub>OH\u7684\u7406\u60f3\u5e73\u53f0\u3002<\/p>\n<p><strong>\u56fe\u4e8c\u5341\u4e00\uff1a\u50ac\u5316\u5242\u5206\u79bb\u548c\u5faa\u73af\u5229\u7528<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-162440\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/21.jpg\" alt=\"\" width=\"600\" height=\"416\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/21.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2018\/12\/21-300x208.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><br \/>\n \u7531\u78c1\u6027\u6750\u6599\u6784\u7b51\u7684\u6613\u4e8e\u5206\u79bb\u7684\u6838\u58f3\u7eb3\u7c73\u7c92\u5b50\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u4f5c\u8005\u901a\u8fc7\u6df1\u5165\u4e86\u89e3\u7535\u8377\u8f7d\u4f53\u5408\u7406\u8c03\u8282\u7684\u6709\u6548\u5149\u50ac\u5316\u5f62\u6210\u673a\u7406\u548c\u5236\u5907\u65b9\u6cd5\uff0c\u7efc\u8ff0\u4e86\u5408\u6210\u6838\u58f3\u7ed3\u6784\u7684\u7b56\u7565\u3002\u6211\u4eec\u5c06\u5149\u50ac\u5316\u53cd\u5e94\u4e2d\u7684\u7535\u8377\u884c\u4e3a\u5206\u89e3\u4e3a\u4e09\u4e2a\u90e8\u5206\uff0c\u4ee5\u9610\u660e\u57fa\u4e8e\u6838\u58f3\u7684\u5404\u90e8\u5206\u6240\u91c7\u7528\u7684\u7b56\u7565\uff0c\u8fd9\u53ef\u4e3a\u672a\u6765\u5149\u50ac\u5316\u5242\u7684\u8bbe\u8ba1\u548c\u5236\u9020\u63d0\u4f9b\u6709\u7528\u7684\u6307\u5bfc\u3002\u51e0\u4e4e\u6bcf\u79cd\u4e0a\u8ff0\u6539\u8fdb\u7684\u6838\u58f3\u90fd\u91c7\u7528\u4e86\u4e00\u79cd\u4ee5\u4e0a\u7684\u4fc3\u8fdb\u5149\u50ac\u5316\u53cd\u5e94\u7684\u52a8\u673a\u6548\u5e94\u3002<br \/>\n \u672a\u6765\uff0c\u6838\u58f3\u7ed3\u6784\u5728\u6574\u4f53\u975e\u5747\u76f8\u5149\u50ac\u5316\u7684\u53d1\u5c55\u4e2d\u5177\u6709\u5f88\u5927\u7684\u524d\u666f\uff0c\u4f8b\u5982\u6c34\u5206\u89e3\u548cCRR\u3002\u4e0e\u901a\u5e38\u4f7f\u7528\u727a\u7272\u5242\u52a0\u901f\u5149\u53cd\u5e94\u7684\u4e00\u822c\u5149\u50ac\u5316\u4e0d\u540c\uff0c\u6574\u4f53\u5149\u50ac\u5316\u4ec5\u4f7f\u7528\u7eaf\u6c34\uff08\u6216\u6c34\u548c\u4e8c\u6c27\u5316\u78b3\uff09\u4f5c\u4e3a\u539f\u6599\u6765\u751f\u4ea7H<sub>2<\/sub>\uff0cO<sub>2<\/sub>\u6216\u542b\u78b3\u5316\u5408\u7269\uff0c\u4ee3\u8868\u4ece\u592a\u9633\u80fd\u5230\u5316\u5b66\u80fd\u7684\u6709\u6548\u8f6c\u5316\uff0c\u8fd9\u66f4\u6709\u5229\u4e8e\u73af\u5883\u548c\u8d44\u6e90\u7684\u9700\u6c42\u3002<br \/>\n \u53e6\u4e00\u4e2a\u6539\u5584\u6838\u58f3\u5149\u50ac\u5316\u6d3b\u6027\u7684\u6709\u5e0c\u671b\u7684\u65b9\u5411\u662f\u4e0e\u5355\u539f\u5b50\u50ac\u5316\u7684\u7ed3\u5408\u3002\u5355\u539f\u5b50\u53ef\u4ee5\u4f5c\u4e3a\u5355\u539f\u5b50\u6838\u6216\u52a9\u50ac\u5316\u5242\u52a0\u8f7d\u5728\u5185\u90e8\u6216\u5916\u90e8\u7a7a\u5fc3\u58f3\u4e0a\uff0c\u8fd9\u53ef\u4ee5\u63d0\u4f9b\u663e\u7740\u7684\u6027\u80fd\u6539\u5584\uff0c\u5305\u62ec\u6d3b\u6027\uff0c\u7535\u8377\u6355\u83b7\uff0c\u539f\u5b50\u5229\u7528\u548c\u8868\u9762\u53cd\u5e94\u7b49\u3002\u901a\u5e38\uff0c\u50ac\u5316\u5242\u7528\u4e8e\u5355\u539f\u5b50\u50ac\u5316\u5b9a\u4e49\u4e3a\u4ec5\u542b\u6709\u5206\u79bb\u7684\u5355\u4e2a\u91d1\u5c5e\u539f\u5b50\u4f5c\u4e3a\u4e3b\u8981\u6d3b\u6027\u4e2d\u5fc3\u7684\u8d1f\u8f7d\u578b\u91d1\u5c5e\u50ac\u5316\u5242\u3002\u4e0e\u4ec5\u4f9d\u8d56\u90e8\u5206\u8868\u9762\u539f\u5b50\u50ac\u5316\u53cd\u5e94\u7684\u5927\u578b\u91d1\u5c5e\u7eb3\u7c73\u7c92\u5b50\u4e0d\u540c\uff0c\u5355\u539f\u5b50\u50ac\u5316\u5242\uff08SAC\uff09\u4e2d\u7684\u6bcf\u4e2a\u539f\u5b50\u90fd\u53ef\u4ee5\u4f5c\u4e3a\u6d3b\u6027\u4e2d\u5fc3\uff0c\u56e0\u6b64\u539f\u5b50\u53ef\u7528\u6027\u5728\u7406\u8bba\u4e0a\u662f100\uff05\u3002<br \/>\n \u5728DFT\u548c\u52a8\u529b\u5b66\u5b9e\u9a8c\u7684\u5e2e\u52a9\u4e0b\uff0c\u8fd8\u5e94\u8fdb\u4e00\u6b65\u7814\u7a76\u5728\u5149\u53cd\u5e94\u8fc7\u7a0b\u4e2d\u5f62\u6210\u6838\u58f3\u7684\u539f\u5b50\u7ea7\u673a\u5236\u548c\u7535\u8377\u4f20\u8f93\u7684\u65f6\u95f4\u5206\u8fa8\u8fc7\u7a0b\u3002\u4f5c\u8005\u8ba4\u4e3a\u6838\u58f3\u7ed3\u6784\u53ef\u4ee5\u63d0\u4f9b\u53ef\u6269\u5c55\u7684\u5e73\u53f0\uff0c\u8be5\u5e73\u53f0\u4e0e\u7528\u4e8e\u6539\u8fdb\u5149\u50ac\u5316\u5242\u7684\u65b0\u6982\u5ff5\u548c\u7b56\u7565\u517c\u5bb9\uff0c\u5e76\u4e14\u8fd8\u53ef\u4ee5\u4fee\u6539\u4e3a\u7528\u4e8e\u592a\u9633\u80fd\u8f6c\u6362\u7684\u5176\u4ed6\u7cfb\u7edf\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/pubs.rsc.org\/en\/Content\/ArticleLanding\/2019\/CS\/C8CS00711J#!divAbstract\" target=\"_blank\" rel=\"noopener\">Rational design of yolk\u2013shell nanostructures for photocatalysis<\/a> (<em>Chem. Soc. Rev.<\/em> <strong>2018<\/strong>, DOI: 10.1039\/c8cs00711j)<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7535\u5b50\u7ec4\u5927\u5175\u54e5\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1\uff1a<a href=\"mailto:tougao@cailiaoren.com\" target=\"_blank\" rel=\"noopener\">tougao@cailiaoren.com<\/a>\u3002<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaokefu<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u7814\u7a76\u80cc\u666f\u3011 \u5149\u50ac\u5316\u662f\u5c06\u592a\u9633\u80fd\u76f4\u63a5\u8f6c\u5316\u4e3a\u5316\u5b66\u80fd\u7684\u6709\u524d\u9014\u7684\u9014\u5f84\uff0c\u4e3a\u73af\u5883\u548c\u81ea\u7136\u8d44\u6e90\u95ee\u9898\u63d0\u4f9b\u4e86\u66ff\u4ee3\u89e3\u51b3\u65b9\u6848\u3002\u7406\u8bba\u4e0a\uff0c\u6240\u6709\u5149\u50ac\u5316\u53cd\u5e94\u90fd\u662f\u7531\u7535\u8377\u8f7d\u4f53\u9a71\u52a8\u7684\uff0c\u7535\u8377\u8f7d\u4f53\u7684\u884c\u4e3a&#8230;<\/p>\n","protected":false},"author":1004,"featured_media":162915,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[533],"tags":[3772],"class_list":["post-162394","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zongshu","tag-3772"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/162394"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/1004"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=162394"}],"version-history":[{"count":8,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/162394\/revisions"}],"predecessor-version":[{"id":162747,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/162394\/revisions\/162747"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/162915"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=162394"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=162394"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=162394"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}