{"id":163885,"date":"2019-01-07T06:23:27","date_gmt":"2019-01-06T22:23:27","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=163885"},"modified":"2019-01-07T09:48:02","modified_gmt":"2019-01-07T01:48:02","slug":"%e3%80%90%e5%b7%b2%e6%a0%a1%e7%a8%bf%e3%80%91%e5%85%b0%e5%b7%9e%e5%a4%a7%e5%ad%a6%e5%b8%ad%e8%81%98%e8%b4%a4%e5%9b%a2%e9%98%9f%e5%b8%83%e6%9c%97%e5%a4%a7%e5%ad%a6%e5%ad%99%e5%ae%88%e6%81%92nano-e","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=163885","title":{"rendered":"\u5170\u5dde\u5927\u5b66\u5e2d\u8058\u8d24\u56e2\u961f&amp;\u5e03\u6717\u5927\u5b66\u5b59\u5b88\u6052Nano Energy\uff1a\u7528Co\u66ff\u4ee3\u53ef\u63a7\u8c03\u8282Fe-N\u7eb3\u7c73\u7247\u589e\u5f3a\u6790\u6c27\u53cd\u5e94"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u6790\u6c27\u53cd\u5e94\uff08OER\uff09\u548c\u6c27\u8fd8\u539f\u53cd\u5e94\uff08ORR\uff09\u662f\u4e24\u4e2a\u91cd\u8981\u7684\u534a\u7535\u6c60\u53cd\u5e94\u3002OER\u548cORR\u90fd\u9700\u8981\u50ac\u5316\u5242\u6765\u964d\u4f4e\u53cd\u5e94\u8fc7\u7535\u4f4d\uff0c\u6539\u5584\u56db\u7535\u5b50\u53cd\u5e94\u52a8\u529b\u5b66\u3002\u7531\u4e8e\u5e38\u7528\u7684OER\u50ac\u5316\u5242\u94f1\uff08Ir\uff09\u6216\u948c\uff08Ru\uff09\u548cORR\u50ac\u5316\u5242\u94c2\uff08Pt\uff09\u7a00\u6709\u4e14\u6602\u8d35\u3002\u50ac\u5316\u5242\u7684\u5927\u89c4\u6a21\u4f7f\u7528\u7684\u9700\u6c42\u8fdb\u4e00\u6b65\u63a8\u52a8\u4e86\u975e\u8d35\u91d1\u5c5e\u50ac\u5316\u5242\u7684\u5e7f\u6cdb\u7814\u7a76\u3002\u7136\u800c\uff0c\u7531\u4e8eOH<sup>&#8211;<\/sup>\u6c27\u5316\uff08OER\uff09\u548cO<sub>2<\/sub>\u8fd8\u539f\uff08ORR\uff09\u4e4b\u95f4\u7684\u673a\u7406\u4e0d\u540c\uff0c\u5f00\u53d1\u5177\u6709\u6210\u672c\u6548\u76ca\u7684\u975e\u8d35\u91d1\u5c5e\u53cc\u529f\u80fdOER\/ORR\u50ac\u5316\u5242\u4e00\u76f4\u662f\u4e00\u9879\u6311\u6218\u3002\u8fc7\u6e21\u91d1\u5c5e\u6c2e\u5316\u7269\uff08TMNs\uff09\uff0c\u7531\u4e8e\u5176\u9ad8\u5bfc\u7535\u6027\uff0c\u72ec\u7279\u7684\u4e0e\u6c27\u7269\u8d28\u53cd\u5e94\u7684\u80fd\u529b\u4ee5\u53ca\u5728\u6c27\u5316\u7269\u4e2d\u7684\u4f18\u5f02\u5316\u5b66\u7a33\u5b9a\u6027\u800c\u5907\u53d7\u5173\u6ce8\u3002\u7136\u800c\uff0c\u5230\u76ee\u524d\u4e3a\u6b62\u62a5\u9053\u7684\u5927\u591a\u6570TMNs\u50ac\u5316\u5242\u9002\u7528\u4e8eORR\uff0c\u5bf9\u4e8eOER\u5219\u4e0d\u7136\u3002\u56e0\u6b64\uff0c\u5728\u4e0d\u635f\u5bb3\u5176ORR\u50ac\u5316\u6027\u80fd\u7684\u60c5\u51b5\u4e0b\u589e\u5f3aOER\u50ac\u5316\u662f\u975e\u5e38\u5fc5\u8981\u7684\u3002\u6700\u8fd1\u7684\u7814\u7a76\u8868\u660e\uff0c\u5408\u91d1\u5316\u662f\u63d0\u9ad8OER\u7535\u50ac\u5316\u6027\u80fd\u7684\u91cd\u8981\u9014\u5f84\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u5728<strong><b>\u5170\u5dde\u5927\u5b66\u5e2d\u8058\u8d24<\/b><\/strong><strong><b>\u6559\u6388\u56e2\u961f<\/b><\/strong>\u548c<strong><b>\u7f8e\u56fd\u5e03\u6717\u5927\u5b66\u5b59\u5b88\u6052\u6559\u6388<\/b><\/strong>\u548c<strong><b>\uff08<\/b><\/strong><strong><b>\u5171\u540c<\/b><\/strong><strong><b>\u901a\u8baf\u4f5c\u8005\uff09<\/b><\/strong>\u5e26\u9886\u4e0b\uff0c\u4e0e<strong><b>\u5357\u5f00\u5927\u5b66<\/b><\/strong>\u548c<strong><b>\u4e2d\u56fd\u79d1\u5b66\u9662\u4e0a\u6d77\u5e94\u7528\u7269\u7406\u7814\u7a76\u6240<\/b><\/strong>\u5408\u4f5c\uff0c\u62a5\u9053\u4e86\u4e00\u79cd\u5c06ORR\u5355\u529f\u80fd\u50ac\u5316\u5242Fe-N\u8f6c\u5316\u4e3aOER\/ORR\u53cc\u529f\u80fd\u50ac\u5316\u5242Co-Fe-N\u7684\u65b0\u5de5\u827a\uff0c\u5e76\u63d0\u51fa\u4e86Co\u5728\u50ac\u5316\u8f6c\u5316\u4e2d\u53d1\u6325\u4f5c\u7528\u7684\u539f\u5b50\u673a\u7406\u3002\u5728\u8fd9\u9879\u7814\u7a76\u4e2d\uff0c\u56e2\u961f\u9996\u5148\u901a\u8fc7\u6eb6\u6db2\u76f8\u5265\u79bb\u65b9\u6cd5\u5236\u5907\u8d85\u8584\uff081.1nm\u539a\uff09Fe-N\u548c\u591a\u79cdCo-Fe-N\u7eb3\u7c73\u7247\uff08NSs\uff09\u3002\u8be51.1nm\u539a\u5ea6\u662f\u6cbf\u5176\u6676\u4f53b\u8f74\u65b9\u5411\u7684\u6b63\u4ea4Co-Fe-N\u7ed3\u6784\u7684\u4e24\u4e2a\u6676\u80de\u7684\u957f\u5ea6\u5c3a\u5ea6\u3002\u8fd9\u4e9b\u8d85\u8584\u7eb3\u7c73\u7247\u4f7fCo\u6700\u5927\u7684\u66b4\u9732\u4e8e\u53cd\u5e94\u73af\u5883\uff0c\u662f\u4e00\u7c7b\u4f18\u5f02OER\u50ac\u5316\u5242\u3002\u5728\u7cfb\u5217Co\u63ba\u6742Fe-N\u7eb3\u7c73\u7247\u4e2d\uff0c\u63ba\u6742\u91cf\u4e3a15%\u65f6\uff0c\u6027\u80fd\u6700\u4f18\u3002Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684OER\u8fc7\u7535\u4f4d\u03b7\u572810 mA cm<sup>-2<\/sup>\u65f6\u4ec5\u4e3a266 mV\uff0cTafel\u659c\u7387\u4e3a~30 mV dec<sup>-1<\/sup>\uff0c\u800c\u4e14\u7a33\u5b9a\u6027\u5f88\u597d\uff0c\u572890\u5c0f\u65f6\u7a33\u5b9a\u6027\u8bd5\u9a8c\u540e\u6ca1\u6709\u660e\u663e\u7684\u6d3b\u6027\u53d8\u5316\u3002\u5bc6\u5ea6\u6cdb\u51fd\u7406\u8bba\uff08DFT\uff09\u8ba1\u7b97\u8868\u660e\uff0c\u5728Co<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7ed3\u6784\u4e2d\u5b58\u5728\u9002\u5f53\u6bd4\u4f8b\u7684Co-Fe\uff0c\u5176\u6539\u5584O\u204e\u5438\u9644\u548c\u53cd\u5e94\u9014\u5f84\u7684\u5173\u952e\uff0c\u4fc3\u8fdbO\u204e-O\u204e\u8026\u5408\u548cOER\u8fc7\u7a0b\u4e2d\u5f62\u6210O<sub>2<\/sub>\u3002\u76f8\u5173\u6210\u679c\u4ee5\u9898\u4e3a<strong><b>\u201cControllable Tuning of Fe-N Nanosheets by Co Substitution for Enhanced Oxygen Evolution Reaction\u201d<\/b><\/strong>\u53d1\u8868\u5728\u4e86<strong><b>Nano Energy<\/b><\/strong>\u4e0a\uff0c\u7b2c\u4e00\u4f5c\u8005\u4e3a\u5170\u5dde\u5927\u5b66\u5b89\u4e3d\u535a\u58eb\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Co<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>Fe<\/b><\/strong><strong><sub><b>1-x<\/b><\/sub><\/strong><strong><b>N<\/b><\/strong><strong><sub><b>0.5<\/b><\/sub><\/strong><strong><b>\u00a0NS<\/b><\/strong><strong><b>s\u7684\u7269\u7406\u6027\u80fd\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-163886\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/1-3.jpg\" alt=\"\" width=\"600\" height=\"757\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/1-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/1-3-238x300.jpg 238w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Co<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub>\u00a0NSs\uff08\u5de6\uff09\u53ca\u76f8\u5e94\u7684\uff08121\uff09\u5cf0\uff08\u53f3\uff09\u7684XRD\u56fe\u3002<\/p>\n<p>\uff08b-d\uff09Co<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684\uff08b\uff09TEM\uff0c\uff08c\uff09TEM-EDS\u5143\u7d20\u5206\u5e03\u56fe\u548c\uff08d\uff09HRTEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08e\uff09Co<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684AFM\u56fe\u50cf\u3002<\/p>\n<p>\uff08f\uff09Co<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684\u9ad8\u5ea6\u5206\u5e03\u3002 \u00a0<\/p>\n<p>\uff08g\uff09Co<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684\u53cc\u5355\u5143\u6a21\u578b\u3002<\/p>\n<p><strong><b>\u56fe2<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Co<\/b><\/strong><strong><sub><b>0.15<\/b><\/sub><\/strong><strong><b>Fe<\/b><\/strong><strong><sub><b>0.85<\/b><\/sub><\/strong><strong><b>N<\/b><\/strong><strong><sub><b>0.5<\/b><\/sub><\/strong><strong><b>\u00a0NSs<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>XPS\u5149\u8c31<\/b><\/strong><strong><b>\u548c<\/b><\/strong><strong><b>EXAFS\u5149\u8c31<\/b><\/strong><strong><b>\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-163887\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/2-3.jpg\" alt=\"\" width=\"600\" height=\"739\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/2-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/2-3-244x300.jpg 244w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684Fe 2p XPS\u5149\u8c31\u3002<\/p>\n<p>\uff08b\uff09Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684Co 2p XPS\u5149\u8c31\u3002<\/p>\n<p>\uff08c\uff09Fe<sub>1.0<\/sub>N<sub>0.5<\/sub><sub>\u00a0<\/sub>NSs\u548cCo<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684Fe 2p XPS\u5149\u8c31\u6bd4\u8f83\u3002<\/p>\n<p>\uff08d\uff09Fe<sub>1.0<\/sub>N<sub>0.5<\/sub><sub>\u00a0<\/sub>NSs\u548cCo<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684N 1s XPS\u5149\u8c31\u3002<\/p>\n<p>\uff08e\uff09Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u548cFe<sub>1.0<\/sub>N<sub>0.5<\/sub><sub>\u00a0<\/sub>NSs\u7684Fe K\u8fb9\u7684R\u7a7a\u95f4\u7684EXAFS\u5149\u8c31\u3002<\/p>\n<p>\uff08f\uff09Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684Co K\u8fb9\u7684R\u7a7a\u95f4\u4e2d\u7684EXAFS\u5149\u8c31\u3002<\/p>\n<p><strong><b>\u56fe3<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Co<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>Fe<\/b><\/strong><strong><sub><b>1-x<\/b><\/sub><\/strong><strong><b>N<\/b><\/strong><strong><sub><b>0.5<\/b><\/sub><\/strong><strong><sub><b>\u00a0<\/b><\/sub><\/strong><strong><b>NS<\/b><\/strong><strong><b>s\u7684OER\u7535\u5316\u5b66\u8868\u5f81<\/b><\/strong><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-163888\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/3-3.jpg\" alt=\"\" width=\"600\" height=\"613\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/3-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/3-3-294x300.jpg 294w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09Co<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub><sub>\u00a0<\/sub>NSs\uff08x = 0\uff0c0.05\uff0c0.1\uff0c0.15\u548c0.2\uff09\u7684OER\u6781\u5316\u66f2\u7ebf\u3002<\/p>\n<p>\uff08b\uff09Co<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub><sub>\u00a0<\/sub>NSs\uff08x = 0\uff0c0.05\uff0c0.1\uff0c0.15\u548c0.2\uff09\u7684\u8fc7\u7535\u4f4d\u3002<\/p>\n<p>\uff08c\uff09\u57281.0 M KOH\u4e2dCo<sub>x<\/sub>Fe<sub>1-x<\/sub>N<sub>0.5<\/sub><sub>\u00a0<\/sub>NSs\uff08x = 0\uff0c0.05\uff0c0.1\uff0c0.15\u548c0.2\uff09\u7684Tafel\u56fe\uff08\u626b\u63cf\u901f\u7387\u4e3a2 mV\u00a0s<sup>-1<\/sup>\uff09\u3002<\/p>\n<p>\uff08d\uff09\u4e0e\u6700\u5148\u8fdb\u7684OER\u7535\u50ac\u5316\u5242\u8fdb\u884c\u6bd4\u8f83\u3002<\/p>\n<p>\uff08e\uff09\u4e00\u7cfb\u5217\u6052\u5b9a\u7535\u4f4d\u7684Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7684\u8ba1\u65f6\u7535\u6d41\u66f2\u7ebf\u3002<\/p>\n<p>\uff08f\uff09Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7535\u50ac\u5316\u5242\u572810000\u4e2aCV\u5faa\u73af\u4e4b\u524d\u548c\u4e4b\u540e\u7684\u6781\u5316\u66f2\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Co<\/b><\/strong><strong><sub><b>0.15<\/b><\/sub><\/strong><strong><b>Fe<\/b><\/strong><strong><sub><b>0.85<\/b><\/sub><\/strong><strong><b>N<\/b><\/strong><strong><sub><b>0.5<\/b><\/sub><\/strong><strong><sub><b>\u00a0<\/b><\/sub><\/strong><strong><b>NSs<\/b><\/strong><strong><b>\u6a21\u578b\u7684<\/b><\/strong><strong><b>OER<\/b><\/strong><strong><b>\u7406\u8bba\u8ba1\u7b97<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-163890\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/4-3.jpg\" alt=\"\" width=\"600\" height=\"795\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/4-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/4-3-226x300.jpg 226w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u57281.0M KOH\u4e2dCo<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub><sub>\u00a0<\/sub>NSs\uff0cFe<sub>1.0<\/sub>N<sub>0.5<\/sub><sub>\u00a0<\/sub>NSs\u548cCo<sub>5.47<\/sub>N NSs\u7684OER\u6781\u5316\u66f2\u7ebf\u3002<\/p>\n<p>\uff08b\uff09Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u548cFe<sub>1.0<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u6a21\u578b\u7684\u9884\u6d4b\u6001\u5bc6\u5ea6\u3002<\/p>\n<p>\uff08c-e\uff09\u5728Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u8868\u9762\u7684\uff08c\uff09OH *\uff0c\uff08d\uff09O *\u548c\uff08e\uff09OOH *\u7684\u4f18\u5316\u5438\u9644\u7ed3\u6784\u3002<\/p>\n<p>\uff08f\uff09Co<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u548cFe<sub>1.0<\/sub>N<sub>0.5<\/sub>\u6a21\u578b\u7684OER\u7684\u80fd\u91cf\u5206\u5e03\u56fe\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>5<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>OER<\/b><\/strong><strong><b>\u8fc7\u7a0b\u4e2d\u4e0d\u540c<\/b><\/strong><strong><b>\u6d3b\u6027\u4f4d\u70b9<\/b><\/strong><strong><b>\u7684\u7406\u8bba\u8ba1\u7b97<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-163889\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/5-1.jpg\" alt=\"\" width=\"600\" height=\"608\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/5-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/01\/5-1-296x300.jpg 296w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5728Fe-Fe\uff0cCo-Fe\u548cCo-Co\u6a21\u578b\u4e0aOER\u8fc7\u7a0b\u7684\u81ea\u7531\u80fd\u56fe\uff0c\u5176\u4e2dM1\u548cM2\u4ee3\u8868Fe\u6216Co\u3002<\/p>\n<p>\uff08b\uff09Co-Fe\u6a21\u578b\u7684\u4f18\u5316\u5438\u9644\u7ed3\u6784\uff0c\u663e\u793a\u6c27\u91cd\u7ec4\u6b65\u9aa4\u7684\u521d\u6001\uff0c\u8fc7\u6e21\u6001\u548c\u7ec8\u6001\u3002<\/p>\n<p>\uff08c\uff09DFT\u8ba1\u7b97Fe-Fe\uff0cCo-Fe\u548cCo-Co\u6a21\u578b\u7684\u8fc7\u7535\u4f4d\u3002\u63d2\u56fe\uff1aFe-Fe\uff0cCo-Fe\u548cCo-Co\u6a21\u578b\u7684OER\u6d3b\u6027\u4f4d\u70b9\u6570\u3002<\/p>\n<p>\u3010<strong><b>\u5c0f\u7ed3<\/b><\/strong>\u3011<\/p>\n<p>\u603b\u4e4b\uff0c\u5f00\u53d1\u57fa\u4e8eTMNs\u7ed3\u6784\u7684\u65b0\u578b\u53cc\u529f\u80fd\u975e\u8d35\u91d1\u5c5e\u50ac\u5316\u5242\uff0c\u56e2\u961f\u901a\u8fc7\u6eb6\u6db2\u76f8\u5265\u79bb\u65b9\u6cd5\u5408\u6210\u539f\u5b50\u7ea7\u8584\uff081.1nm\uff09Co-Fe-N NSs\u3002\u8d85\u8584\u6027\u4fdd\u8bc1\u4e86Co\/Fe\u6700\u5927\u7a0b\u5ea6\u5730\u66b4\u9732\u4e8e\u53cd\u5e94\u73af\u5883\uff0c\u5e76\u80fd\u8be6\u7ec6\u7814\u7a76Co\u5728\u6539\u53d8Fe-N\u7ed3\u6784\u4e2d\u7684\u4f5c\u7528\uff0c\u4ee5\u663e\u793a\u53cc\u529f\u80fdORR\/OER\u50ac\u5316\u3002\u7814\u7a76\u8868\u660e\uff0c\u5728Co-Fe-N\u7ed3\u6784\u4e2d\uff0cCo\u7684\u5b58\u5728\u524a\u5f31\u4e86Fe-N\/Fe-Fe\u952e\u5e76\u589e\u52a0\u4e86\u6574\u4f53\u91d1\u5c5e\u6c27\u5316\u6001\uff0c\u6539\u53d8\u4e86\u7535\u5b50\u7ed3\u6784\u5e76\u6539\u5584\u4e86Fe\u7684\u50ac\u5316\u6027\u80fd\u3002\u7ed3\u679c\uff0cCo<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u572810mA cm<sup>-2<\/sup>\u5904\u663e\u793a\u51fa\u6700\u4f4e\u7684\u03b7\u4e3a266 mV\uff0c\u6700\u5c0f\u7684Tafel\u659c\u7387\u4e3a~30mV dec<sup>-1<\/sup>\u5e76\u4e14\u5177\u6709\u6700\u9ad8\u7684\u957f\u671f\u7a33\u5b9a\u6027\u3002\u6b64\u5916\uff0cDFT\u8ba1\u7b97\u8868\u660eCo<sub>0.15<\/sub>Fe<sub>0.85<\/sub>N<sub>0.5<\/sub>\u00a0NSs\u7ed3\u6784\u4e2d\u7684Co-Fe\u4f4d\u70b9\u88ab\u4f18\u5316\uff0c\u4fc3\u8fdbOH\u204e\u5411O\u204e\u8f6c\u5316\uff0cO\u204e-O\u204e\u8026\u5408\u548cO<sub>2<\/sub>\u5f62\u6210\uff0c\u8868\u660eCo-Fe\u4f4d\u70b9\u5728\u589e\u5f3aOER\u50ac\u5316\u65b9\u9762\u786e\u5b9e\u8868\u73b0\u51fa\u975e\u5e38\u7406\u60f3\u7684\u534f\u540c\u4f5c\u7528\u3002\u8be5\u7814\u7a76\u7684\u5408\u6210\u65b9\u6cd5\u4e0d\u4ec5\u9650\u4e8eCo-Fe-N\u7684\u5236\u5907\uff0c\u8fd8\u53ef\u4ee5\u63a8\u5e7f\u5230M<sub>x<\/sub>M<sub>1-x<\/sub>N<sub>y<\/sub>\uff0c\u4e3a\u5236\u5907\u91cd\u8981\u7535\u5316\u5b66\u53cd\u5e94\u7684\u975e\u8d35\u91d1\u5c5e\u50ac\u5316\u5242\u53cc\u91d1\u5c5e\u6c2e\u5316\u7269\u63d0\u4f9b\u4e86\u4e00\u79cd\u901a\u7528\u7684\u65b9\u6cd5\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><a href=\"#!\" target=\"_blank\" rel=\"noopener\"><u>Controllable Tuning of Fe-N Nanosheets by Co Substitution for Enhanced Oxygen Evolution Reaction<\/u><\/a>\uff08Nano Energy, 2018, DOI:10.1016\/j.nanoen.2018.12.094\uff09<\/p>\n<p>\u3010<strong><b>\u56e2\u961f\u4ecb\u7ecd<\/b><\/strong>\u3011<\/p>\n<p>\u7814\u7a76\u56e2\u961f\u76f8\u5173\u53c2\u8003\u6587\u732e\uff1a<\/p>\n<ol>\n<li>Heterostructure-Promoted Oxygen Electrocatalysis Enables Rechargeable Zinc-Air Battery with Neutral Aqueous Electrolyte, J. Am. Chem. Soc. 2018, 140, 17624.<\/li>\n<li>Ni-C-N Nanosheets as Catalyst for Hydrogen Evolution Reaction, J. Am. Chem. Soc. 2016, 138,14546.<\/li>\n<li>Oxygen Vacancies Dominated NiS<sub>2<\/sub>\/CoS<sub>2<\/sub>Interface Porous Nanowires for Portable Zn-Air Batteries Driven Water Splitting Devices, Adv. Mater. 2017, 29, 1704681.<\/li>\n<li>4. Epitaxial Heterogeneous Interfaces on N-NiMoO<sub>4<\/sub>\/NiS<sub>2<\/sub>Nanowires\/Nanosheets to Boost Hydrogen and OxygenProduction for Overall Water Splitting, Adv. Funct. Mater. 2019, 29, 1805298<\/li>\n<li>Atomic-level Coupled Interface and Lattice Distortion on Cu-Ni-S Nanocrystals Boost Oxygen Catalysis for Flexible Zn-Air Batteries, Adv. Funct. Mater. 2017, 27, 1703779.<\/li>\n<li>NiO\/CoN Porous Nanowires as Efficient Bifunctional Catalysts for Zn-Air Batteries, ACS. Nano. 2017, 11, 2275.<\/li>\n<li>FeS<sub>2<\/sub>\/CoS<sub>2<\/sub>Interface Nanosheets as Efficient Bifunctional Electrocatalyst for Overall Water Splitting, Small 2018, 14, 1801070.<\/li>\n<li>Activation of defective nickel molybdate nanowires for enhanced alkaline electrochemical hydrogen evolution, Nanoscale, 2018, 10, 16539.<\/li>\n<li>High-Index Faceted CuFeS<sub>2 <\/sub>Nanosheets with Enhanced Behavior for Boosting Hydrogen Evolution Reaction, Nanoscale, 2017, 9, 9230.<\/li>\n<li>Self-supported nanoporous NiCo<sub>2<\/sub>O<sub>4 <\/sub>nanowires with cobalt-nickel layered oxide nanosheets for overall water splitting, Nanoscale, 2016, 8, 1390.<\/li>\n<li>A Self-Standing High-Performance Hydrogen Evolution Electrode with Nanostructured NiCo<sub>2<\/sub>O<sub>4<\/sub>\/CuS Heterostructures, Adv. Funct. Mater., 2015, 25, 6814.<\/li>\n<li>Phase Transformation Fabrication of a Cu<sub>2<\/sub>S Nanoplate as an Efficient Catalyst for Water Oxidation with Glycine, Inorg. Chem.,2015, 54, 3281.<\/li>\n<li>High-Quality Copper Sulfide Nanocrystals with Diverse Shapes and Their Catalysis for Electrochemical Reduction of H<sub>2<\/sub>O<sub>2<\/sub>, Part. Part. Syst. Charact. 2015, 32, 536.<\/li>\n<li>Ultrafast Hole Trapping and Relaxation Dynamics in p-Type CuS Nanodisks, J. Phys. Chem. Lett. 2015, 6, 2671.<\/li>\n<li>Self-supported nanoporous NiCo<sub>2<\/sub>O<sub>4<\/sub>nanowires with cobalt-nickel layered oxide nanosheets for overall water splitting. Nanoscale, 2016, 8, 1390.<\/li>\n<\/ol>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u5b66\u672f\u7ec4<strong><b>\u6728\u6587\u97ec<\/b><\/strong>\u7ffb\u8bd1\uff0c<strong>\u5170\u5dde\u5927\u5b66\u5e2d\u8058\u8d24\u6559\u6388<\/strong>\u4fee\u6b63\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u6790\u6c27\u53cd\u5e94\uff08OER\uff09\u548c\u6c27\u8fd8\u539f\u53cd\u5e94\uff08ORR\uff09\u662f\u4e24\u4e2a\u91cd\u8981\u7684\u534a\u7535\u6c60\u53cd\u5e94\u3002OER\u548cORR\u90fd\u9700\u8981\u50ac\u5316\u5242\u6765\u964d\u4f4e\u53cd\u5e94\u8fc7\u7535\u4f4d\uff0c\u6539\u5584\u56db\u7535\u5b50\u53cd\u5e94\u52a8\u529b\u5b66\u3002\u7531\u4e8e\u5e38\u7528\u7684OER\u50ac\u5316&#8230;<\/p>\n","protected":false},"author":2109,"featured_media":163891,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[3804,3353,2444,3471],"class_list":["post-163885","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-3804","tag-3353","tag-2444","tag-3471"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/163885"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2109"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=163885"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/163885\/revisions"}],"predecessor-version":[{"id":164067,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/163885\/revisions\/164067"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/163891"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=163885"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=163885"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=163885"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}