{"id":168471,"date":"2019-03-03T06:20:38","date_gmt":"2019-03-02T22:20:38","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=168471"},"modified":"2019-04-26T14:32:39","modified_gmt":"2019-04-26T06:32:39","slug":"%e4%bb%80%e4%b9%88%e6%a0%b7%e7%9a%84%e4%b8%89%e7%bb%b4%e6%89%93%e5%8d%b0%e6%89%8d%e8%83%bd%e5%8f%91%e5%bd%b1%e5%93%8d%e5%9b%a0%e5%ad%9020%e4%bb%a5%e4%b8%8a%e7%9a%84%e6%9d%82%e5%bf%97","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=168471","title":{"rendered":"\u4ec0\u4e48\u6837\u7684\u4e09\u7ef4\u6253\u5370\u624d\u80fd\u53d1\u5f71\u54cd\u56e0\u5b5020\u4ee5\u4e0a\u7684\u6742\u5fd7"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8bed\u3011<\/strong><\/p>\n<p><strong>\u62a5\u544a\u5206\u6790<\/strong><\/p>\n<p><strong>\u6750\u6599\u4eba\u73b0\u5728\u8bbe\u7acb\u5404\u79cd\u6587\u7ae0\u4e13\u680f\uff0c\u6240\u6d89\u53ca\u9886\u57df\u6b63\u5728\u6162\u6162\u5b8c\u5584\uff0c\u7531\u6b64\u4e5f\u9700\u8981\u66f4\u591a\u7684\u4e13\u680f\u4f5c\u8005\uff0c\u671f\u5f85\u4f60\u4eec\u7684\u52a0\u5165\uff0c\u6709\u610f\u5411\u7684\u5c0f\u4f19\u4f34\u76f4\u63a5\u5fae\u4fe1\u8054\u7cfbcailiaorenVIP\u3002\u4e0d\u8981\u518d\u72b9\u8c6b\uff0c\u4e0b\u4e00\u4e2a\u4e13\u680f\u521b\u59cb\u4eba\u5c31\u662f\u4f60\u3002\u8bf7\u8bb0\u4f4f\uff1a\u7eb5\u7136\u4f60\u79bb\u6211\u5343\u91cc\u4e07\u91cc\uff0c\u6211\u90fd\u5728\u6750\u6599\u4eba\u7b49\u4f60\uff01<\/strong><\/p>\n<p>\u4e09\u7ef4\u6253\u5370\u81ea\u4e0a\u4e16\u7eaa80\u5e74\u4ee3\u88ab\u63d0\u51fa\u5f00\u59cb\uff0c\u53d7\u5230\u4e86\u7814\u7a76\u8005\u4eec\u7684\u5e7f\u6cdb\u5173\u6ce8\u3002\u622a\u6b62\u76ee\u524d\uff0c\u6709\u5173\u4e8e3d\u00a0printing\u7684SCI\u8bba\u6587\u6570\u5df2\u9ad8\u8fbe10000\u7bc7\u3002\u4f46\u5176\u4e2d\u5f71\u54cd\u56e0\u5b50\u5927\u4e8e20\u7684\u7bc7\u6570\u4ec5\u4e3a100\u591a\u7bc7\u3002\u4ece\u4ee5\u4e0b3d\u00a0printing\u5728\u5404\u5f71\u54cd\u56e0\u5b50\u53d1\u8868\u6570\u91cf\u7684\u7edf\u8ba1\u56fe\u8868\u4e2d\uff0c\u53ef\u53d1\u73b0\uff0c\u4e09\u7ef4\u6253\u5370\u76f8\u5173\u7814\u7a76\u53d1\u8868\u6700\u591a\u7684\u6742\u5fd7\u662f\u5f71\u54cd\u56e0\u5b505\u5206\u4ee5\u4e0b\u6742\u5fd7\uff0c\u5360\u6bd4\u9ad8\u8fbe70%\u5de6\u53f3\u3002\u6b64\u5916\uff0c\u5f71\u54cd\u56e0\u5b505\u523010\u5206\u7684\u8bba\u6587\u6570\u91cf\u5360\u603b\u6570\u91cf\u768420%\u5de6\u53f3\uff0c\u800c\u5f71\u54cd\u56e0\u5b50\u5927\u4e8e20\u7684\u8bba\u6587\u6570\u91cf\u5360\u6bd4\u4ec5\u4e3a\u767e\u5206\u4e4b\u4e8c\u5de6\u53f3\u3002\u5f53\u7136\uff0c\u8981\u8bf4\u660e\u7684\u662f\uff0c\u5728\u751f\u7269\u6750\u6599\u9886\u57df\u4e2d\u9876\u7ea7\u671f\u520aBiomaterials\u548cActa\u00a0Biomaterialia,\u5f71\u54cd\u56e0\u5b50\u4e5f\u4e0d\u8fc78\u5206\u548c6\u5206\u591a\u3002\u4f46\u8fd9\u4e9b\u6742\u5fd7\u4e0a\u53d1\u8868\u7684\u8bba\u6587\u8d28\u91cf\u5df2\u7ecf\u5904\u4e8e\u76f8\u5f53\u9ad8\u7684\u6c34\u51c6\u4e86\uff01\u00a0\u56e0\u6b64\uff0c\u59d1\u4e14\u4ee5\u5f71\u54cd\u56e0\u5b505\u5206\u4e3a\u5206\u754c\u7ebf\uff0c\u5728\u4e09\u7ef4\u6253\u5370\u7684\u76f8\u5173\u7814\u7a76\u4e2d\u6709\u7ea6\u56db\u5206\u4e4b\u4e00\u7684\u7814\u7a76\u5728\u91cd\u8981\u6027\u548c\u521b\u65b0\u6027\u4e0a\u5747\u662f\u5904\u4e8e\u8f83\u9ad8\u6c34\u51c6\u7684\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-168472 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72476-11.png\" alt=\"\" width=\"481\" height=\"289\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72476-11.png 481w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72476-11-300x180.png 300w\" sizes=\"(max-width: 481px) 100vw, 481px\" \/><\/p>\n<p>\u5176\u4e2d\u4e09\u7ef4\u6253\u5370\u6d89\u53ca\u7684\u9886\u57df\u4e3b\u8981\u96c6\u4e2d\u5728\u751f\u7269\u533b\u5b66\u9886\u57df\u4e2d\u7684\u5e94\u7528\uff0c\u5982\u4e09\u7ef4\u6253\u5370\u9aa8\u7ec4\u7ec7\u5de5\u7a0b\u652f\u67b6\uff0c\u4e09\u7ef4\u6253\u5370\u8f6f\u9aa8\u7ec4\u7ec7\uff0c\u4ee5\u53ca\u4e09\u7ef4\u6253\u5370\u5668\u5b98\u7b49\u3002\u6b64\u5916\uff0c\u4e09\u7ef4\u6253\u5370\u867d\u7136\u5728\u822a\u7a7a\u822a\u5929\u548c\u6c7d\u8f66\u5236\u9020\u7b49\u9886\u57df\u867d\u7136\u4e5f\u6709\u5e7f\u6cdb\u7684\u5e94\u7528\uff0c\u4f46\u76f8\u5173\u7684\u7814\u7a76\u8bba\u6587\u5374\u5e76\u4e0d\u5e38\u89c1\u3002\u8fd1\u5e74\u6765\uff0c\u4e09\u7ef4\u6253\u5370\u6253\u5370\u8d85\u7ea7\u7535\u5bb9\u5668\uff0c\u4e09\u7ef4\u6253\u5370\u77f3\u58a8\u70ef\u7b49\u65b0\u6750\u6599\u4e5f\u53d7\u5230\u4e86\u8d8a\u6765\u8d8a\u5e7f\u6cdb\u7684\u91cd\u89c6\u3002\u5c06\u4e09\u7ef4\u6253\u5370\u5e94\u7528\u4e8e\u80fd\u6e90\u9886\u57df\u5df2\u6210\u4e3a\u5f53\u4e0b\u70ed\u95e8\u7684\u7814\u7a76\u8bfe\u9898\u3002<\/p>\n<p>\u8fc7\u53bb\u5341\u5e74\u662f\u4e09\u7ef4\u6253\u5370\u65e9\u671f\u53ca\u6700\u706b\u7684\u5e74\u4ee3\u3002\u968f\u7740\u7814\u7a76\u8005\u4eec\u8d8a\u6765\u8d8a\u591a\uff0c\u5e76\u4e14\u53ef\u4f9b\u6253\u5370\u7684\u6750\u6599\u4e5f\u65e9\u5df2\u88ab\u7814\u7a76\u5f97\u5f88\u5f7b\u5e95\u3002\u8fd1\u5e74\u6765\uff0c\u4e09\u7ef4\u6253\u5370\u4f3c\u4e4e\u4e5f\u9677\u5165\u4e86\u74f6\u9888\u3002\u4f46\u4f9d\u7136\u6709\u4e9b\u5927\u4f6c\u4eec\u7528\u6781\u5177\u521b\u65b0\u7684\u6750\u6599\u6216\u5b9e\u9a8c\u5728\u9876\u7ea7\u671f\u520a\u4e0a\u53d1\u8868\u7740\u4ed6\u4eec\u7684\u7814\u7a76\u6210\u679c\u3002\u8ba9\u6211\u4eec\u6765\u770b\u770b\u51e0\u4e2a\u5177\u4f53\u5b9e\u4f8b\uff0c\u770b\u770b\u4ec0\u4e48\u6837\u7684\u4e09\u7ef4\u6253\u5370\u624d\u80fd\u53d1\u5f71\u54cd\u56e0\u5b5020\u4ee5\u4e0a\u7684\u6742\u5fd7\u3002<\/p>\n<p><strong><b>1.UC\u4f2f\u514b\u5229-Volumetric additive manufacturing via tomographic reconstruction<\/b><\/strong><\/p>\n<p>Brett E. Kelly\u7b49\u4eba1\u6708\u4efd\u5728Science\u6742\u5fd7\u4e0a\u53d1\u8868\u4e86\u5229\u7528\u62d3\u6251\u91cd\u5efa\u7406\u8bba\u548c\u589e\u6750\u5236\u9020\u6280\u672f\u5feb\u901f\u5236\u5907\u601d\u60f3\u8005\u6a21\u578b\u7684\u6587\u7ae0\uff0c\u77ac\u95f4\u5f15\u53d1\u79d1\u7814\u754c\u7684\u5927\u91cf\u5173\u6ce8\u3002\u8be5\u56e2\u961f\u7814\u7a76\u4eba\u5458\u5f00\u53d1\u4e86\u4e00\u79cd\u8ba1\u7b97\u8f74\u5411\u5149\u523b\uff08CAL\uff09\u65b9\u6cd5\uff0c\u8be5\u65b9\u6cd5\u5c06\u5149\u56fa\u5316\u7acb\u4f53\u5370\u5237\u5f0f\u4e09\u7ef4\u6253\u5370\u6280\u672f\u63a8\u5411\u4e86\u65b0\u7684\u9ad8\u5ea6\uff0c\u582a\u79f0\u91cc\u7a0b\u7891\u5f0f\u7684\u521b\u9020\u3002\u4ee5\u201c\u601d\u60f3\u8005\u201d\u4e3a\u4f8b\uff0c\u8be5\u56e2\u961f\u7814\u7a76\u4eba\u5458\u9996\u5148\u5bf9\u5176\u8fdb\u884c\u4e09\u7ef4\u6a21\u578b\u7684\u91cd\u5efa\uff0c\u5305\u62ec2D\u7684\u5085\u91cc\u53f6\u53d8\u6362\u3002\u9009\u62e9\u7532\u57fa\u4e19\u70ef\u9178\u916f\u660e\u80f6\u6c34\u51dd\u80f6\u4e3a\u6253\u5370\u6d46\u6599\u3002\u5229\u7528CAL\u5236\u9020\u7cfb\u7edf\u628a\u4e00\u7ec4\u4e8c\u7ef4\u56fe\u50cf\uff0c\u4ece\u4e0d\u540c\u7684\u89d2\u5ea6\u6295\u5c04\u51fa\u6765\uff0c\u8fd9\u79cd\u591a\u89d2\u5ea6\u7684\u66dd\u5149\u53e0\u52a0\uff0c\u53ef\u4ee5\u8ba9\u5149\u654f\u6db2\u4f53\u56fa\u5316\u6210\u6240\u9700\u8981\u7684\u51e0\u4f55\u5f62\u72b6\u3002\u8fd9\u5957\u7cfb\u7edf\u6253\u5370\u901f\u5ea6\u5feb\uff0c\u7cbe\u5ea6\u9ad8\uff0c\u80fd\u5236\u5907\u5404\u79cd\u590d\u6742\u5f62\u72b6\u6a21\u578b\uff0c\u5c06\u5e26\u6765\u6781\u5927\u7684\u79d1\u6280\u5e94\u7528\u4ef7\u503c\u3002<\/p>\n<p>Fig. 1 CAL volumetric fabrication<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-168473 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72477-10.png\" alt=\"\" width=\"600\" height=\"306\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72477-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72477-10-300x153.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u5168\u6587\u94fe\u63a5\uff1a<a href=\"http:\/\/science.sciencemag.org\/content\/early\/2019\/01\/30\/science.aau7114.full\"><u>http:\/\/science.sciencemag.org\/content\/early\/2019\/01\/30\/science.aau7114.full<\/u><\/a><\/p>\n<p><strong><b>2.\u52a0\u5dde\u5927\u5b66\u5723\u5730\u4e9a\u54e5\u5206\u6821-Biomimetic 3D-printed scaffolds for spinal cord injury repair<\/b><\/strong><\/p>\n<p>\u5229\u7528\u4e09\u7ef4\u6253\u5370\u7684\u65b9\u5f0f\u6253\u5370\u7ec4\u7ec7\u5668\u5b98\u662f\u76ee\u524d\u751f\u7269\u6253\u5370\u9886\u57df\u6700\u70ed\u95e8\u6700\u524d\u6cbf\u7684\u7814\u7a76\u65b9\u5411\u3002\u5982\u4f55\u6784\u5efa\u590d\u6742\u7684\u4e09\u7ef4\u5fae\u7ed3\u6784\uff0c\u8fd9\u5bf9\u4e8e\u6307\u5bfc\u7ec6\u80de\u751f\u957f\u548c\u4fc3\u8fdb\u7ec4\u7ec7\u53d1\u80b2\u81f3\u5173\u91cd\u8981\u3002\u8fd9\u5176\u4e2d\uff0c\u7531\u4e8e\u4e2d\u67a2\u795e\u7ecf\u7cfb\u7edf\u7ed3\u6784\u7684\u590d\u6742\u6027\uff0c\u4e09\u7ef4\u6253\u5370\u4e2d\u67a2\u795e\u7ecf\u7cfb\u7edf(CNS)\u7ed3\u6784\u65b9\u9762\u7684\u8bba\u6587\u4f9d\u7136\u7f55\u89c1\u3002\u52a0\u5dde\u5927\u5b66\u5723\u5730\u4e9a\u54e5\u5206\u6821\u7684Jacob\u00a0Koffler\u7b49\u4eba\u4f7f\u7528\u5fae\u5c3a\u5ea6\u8fde\u7eed\u6295\u5f71\u5149\u523b\u65b9\u6cd5(\u03bcCPP)\u6765\u521b\u5efa\u4e00\u4e2a\u590d\u6742\u7684\u4e2d\u67a2\u795e\u7ecf\u7cfb\u7edf\u7ed3\u6784\uff0c\u5e76\u63a2\u7d22\u4e86\u5176\u5728\u810a\u9ad3\u518d\u751f\u533b\u5b66\u65b9\u9762\u7684\u5e94\u7528\u3002\u8be5\u8bba\u6587\u53d1\u8868\u5728Nature Medicine\u4e0a\uff0c\u5f71\u54cd\u56e0\u5b5032.62\u3002\u03bcCPP\u53ef\u4ee5\u5229\u7528\u4eff\u751f\u6c34\u51dd\u80f6\u6253\u5370\u810a\u9ad3\u652f\u67b6\uff0c\u5e76\u4e14\u53ef\u6839\u636e\u4eba\u7c7b\u810a\u9ad3\u75c5\u53d8\u5b9a\u5236\u4e0d\u540c\u5927\u5c0f\u548c\u51e0\u4f55\u56fe\u5f62\u3002\u8be5\u8bfe\u9898\u7ec4\u7814\u53d1\u7684\u810a\u9ad3\u652f\u67b6\u88c5\u8f7d\u795e\u7ecf\u7956\u7ec6\u80de(npc)\u540e\uff0c\u80fd\u591f\u652f\u6301\u8f74\u7a81\u518d\u751f\uff0c\u4fee\u590d\u810a\u9ad3\u635f\u4f24\u3002\u56e0\u6b64\uff0c\u8be5\u4e09\u7ef4\u4eff\u751f\u652f\u67b6\u63d0\u4f9b\u4e86\u4e00\u79cd\u901a\u8fc7\u7cbe\u51c6\u533b\u7597\u4fc3\u8fdb\u4e2d\u67a2\u795e\u7ecf\u7cfb\u7edf\u518d\u751f\u7684\u624b\u6bb5\u3002<\/p>\n<p>Fig. 2 The 3D-printed scaffold mimics the spinal cord architecture.<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-168474 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72478-10.png\" alt=\"\" width=\"334\" height=\"508\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72478-10.png 334w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72478-10-197x300.png 197w\" sizes=\"(max-width: 334px) 100vw, 334px\" \/><\/p>\n<p>\u6587\u7ae0\u94fe\u63a5\uff1a<a href=\"https:\/\/www.nature.com\/articles\/s41591-018-0296-z\">https:\/\/www.nature.com\/articles\/s41591-018-0296-z<\/a><\/p>\n<p><strong><b>3.\u4e1c\u534e\u5927\u5b66-3D Printing\u00a0of Tunable Energy Storage Devices with Both High Areal and Volumetric Energy Densities<\/b><\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\u7531\u4e8e\u4eba\u7c7b\u5bf9\u80fd\u6e90\u5371\u673a\u7684\u9ad8\u5ea6\u91cd\u89c6\uff0c\u5f00\u53d1\u5177\u6709\u9ad8\u9762\u79ef\u548c\u9ad8\u5bb9\u91cf\u7684\u5148\u8fdb\u8d85\u7ea7\u7535\u5bb9\u5668\u4e00\u76f4\u4ee5\u6765\u662f\u7814\u7a76\u7684\u70ed\u70b9\u3002\u5f53\u8d85\u7ea7\u7535\u5bb9\u5668\u4e0e\u4e09\u7ef4\u6253\u5370\u4e24\u5927\u70ed\u95e8\u7814\u7a76\u65b9\u5411\u78b0\u649e\u5230\u4e00\u8d77\uff0c\u90a3\u5f15\u8d77\u7684\u53cd\u54cd\u5fc5\u7136\u662f\u6781\u5927\u7684\u3002\u4e1c\u534e\u5927\u5b66Tingting Gao\u7b49\u4eba\u91c7\u7528\u4e09\u7ef4\u6253\u5370\u6280\u672f\u5236\u5907\u51fa\u5177\u6709\u9ad8\u5bc6\u5ea6\u80fd\u91cf\u7684\u78b3\u590d\u5408\u6750\u6599\u8d85\u7ea7\u7535\u5bb9\u5668\uff0c\u8be5\u7814\u7a76\u6210\u679c\u53d1\u8868\u5728Advanced energy materials\u4e0a\uff0c\u5f71\u54cd\u56e0\u5b5021.88\u5206\u3002\u8be5\u7814\u7a76\u56e2\u961f\u9009\u53d6\u4e86\u78b3\/\u78b3\u7eb3\u7c73\u7ba1\/\u8fd8\u539f\u6c27\u5316\u77f3\u58a8\u70ef(AC\/CNT\/rGO)\u590d\u5408\u6750\u6599\u4f5c\u4e3a\u6253\u5370\u6d46\u6599\uff0c\u5229\u7528\u6324\u51fa\u5f0f\u76f4\u63a5\u4e66\u5199\u6253\u5370\u7684\u65b9\u5f0f\uff0c\u5236\u5907\u7d27\u5bc6\u5806\u53e0\u3001\u7ed3\u6784\u6574\u9f50\u7684\u7535\u5bb9\u5668\u3002\u503c\u5f97\u63d0\u51fa\u7684\u662f\uff0c\u5f53\u524d\u5e38\u6e29\u6324\u51fa\u5f0f\u4e09\u7ef4\u6253\u5370\u6280\u672f\u5e38\u91c7\u7528\u805a\u5408\u7269\u4f5c\u4e3a\u7c98\u7ed3\u5242\uff0c\u4ee5\u8d4b\u4e88\u6d46\u6599\u826f\u597d\u7684\u9002\u5408\u6253\u5370\u7684\u6d41\u53d8\u6027\u80fd\u3002\u4f46\u805a\u5408\u7269\u7684\u6dfb\u52a0\u4f1a\u6781\u5927\u5730\u964d\u4f4e\u7535\u5bb9\u5668\u7684\u80fd\u91cf\u50a8\u5907\u3002\u4e3a\u6700\u5927\u9650\u5ea6\u5730\u5f00\u53d1\u9ad8\u5bb9\u91cf\u5bc6\u5ea6\u7684\u8d85\u7ea7\u7535\u5bb9\u5668\uff0c\u8be5\u56e2\u961f\u81f4\u529b\u4e8e\u5bfb\u627e\u5f00\u53d1\u4e0d\u4f7f\u7528\u805a\u5408\u7269\u7684\u6253\u5370\u6d46\u6599\uff0c\u663e\u7136\u4ed6\u4eec\u6210\u529f\u4e86\uff0c\u4e3a\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7535\u5316\u5b66\u50a8\u80fd\u88c5\u7f6e\u63d0\u4f9b\u4e86\u5d2d\u65b0\u7684\u601d\u8def\u3002<\/p>\n<p>Figure 3. 3D printing process and rheological properties of inks<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-168475 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72479-10.png\" alt=\"\" width=\"405\" height=\"296\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72479-10.png 405w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u72479-10-300x219.png 300w\" sizes=\"(max-width: 405px) 100vw, 405px\" \/><\/p>\n<p>\u6587\u7ae0\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/abs\/10.1002\/aenm.201802578\"><u>https:\/\/onlinelibrary.wiley.com\/doi\/abs\/10.1002\/aenm.201802578<\/u><\/a><\/p>\n<p><strong><b>4.\u4e0a\u6d77\u7845\u9178\u76d0\u7814\u7a76\u6240-3D-printed scaffolds support cartilage and bone growth<\/b><\/strong><\/p>\n<p>\u7531\u4e8e\u8f6f\u9aa8\u7684\u81ea\u6108\u80fd\u529b\u8f83\u5dee\uff0c\u8fd9\u7c7b\u5173\u8282\u8f6f\u9aa8\u635f\u4f24\u5bf9\u9aa8\u79d1\u548c\u8fd0\u52a8\u533b\u5b66\u5c24\u5176\u5177\u6709\u6311\u6218\u6027\uff0c\u56e0\u6b64\u76f8\u5173\u65b9\u9762\u7a81\u7834\u6027\u7684\u7814\u7a76\u4e5f\u662f\u6750\u6599\u5b66\u754c\u548c\u533b\u5b66\u754c\u5173\u6ce8\u7684\u91cd\u70b9\u3002\u5f71\u54cd\u56e0\u5b5024.54\u7684Materials Today\u4e0a\u62a5\u9053\u4e86Chen et al\u53d1\u8868\u5728biomaterials\u4e0a\u7684\u4e00\u7bc7\u6587\u7ae0\uff08Chen et al., Biomaterials (2018),<a href=\"https:\/\/doi.org\/10.1016\/j.biomaterials.2018.04.005\">https:\/\/doi.org\/10.1016\/j.biomaterials.2018.04.005<\/a>\uff09\u3002\u8be5\u6587\u7ae0\u4ecb\u7ecd\u4e86\u4e2d\u56fd\u79d1\u5b66\u9662\u4e0a\u6d77\u7845\u9178\u76d0\u7814\u7a76\u6240\u5434\u8001\u5e08\u8bfe\u9898\u7ec4\u5236\u5907\u7684\u7eaf\u76f8\u7845\u9178\u9502\u9499(\u7b80\u79f0Li2Ca4Si4O13\u6216L2C4S4)\u6750\u6599\u53ca\u5176\u5728\u8f6f\u9aa8\u4fee\u590d\u65b9\u9762\u7684\u5e94\u7528\u524d\u666f\u3002\u8be5\u5c0f\u7ec4\u8bbe\u8ba1\u4e86\u4e00\u79cd\u7b80\u5355\u7684\u6e7f\u5316\u5b66\u6eb6\u80f6-\u51dd\u80f6\u6cd5\u6765\u751f\u4ea7\u9ad8\u8d28\u91cf\u7684\u751f\u7269\u9676\u74f7L2C4S4\u7c89\u4f53\uff0c\u5229\u7528\u4e09\u7ef4\u6253\u5370\u7684\u65b9\u5f0f\u5236\u5907\u5f62\u72b6\u53ef\u63a7\u7684\u652f\u67b6\u3002\u4e09\u7ef4\u6253\u5370\u7684\u65b9\u5f0f\u4f7f\u5f97\u652f\u67b6\u7684\u5b54\u9699\u5ea6\u548c\u5b54\u5f84\u53ef\u4ee5\u5f97\u5230\u9ad8\u5ea6\u7684\u63a7\u5236\uff0c\u7814\u7a76\u4eba\u5458\u5c06\u652f\u67b6\u7684\u5b54\u5f84\u8bbe\u7f6e\u4e3a170\u5fae\u7c73\u5230400\u5fae\u7c73\u4e0d\u7b49\uff0c\u6240\u5f97\u5230\u7684\u652f\u67b6\u5f3a\u5ea6\u662f\u5176\u5b833d\u6253\u5370\u751f\u7269\u9676\u74f7\u652f\u67b6\u76842-3\u500d\uff0c\u529b\u5b66\u6027\u80fd\u4e0e\u5929\u7136\u9aa8\u9abc\u76f8\u5f53\u3002\u652f\u67b6\u7684\u5f3a\u5ea6\u548c\u7a33\u5b9a\u6027\u8db3\u4ee5\u4e3a\u521d\u59cb\u9aa8\u7ec4\u7ec7\u7684\u5f62\u6210\u63d0\u4f9b\u826f\u597d\u7684\u652f\u6491\uff0c\u800c\u6c14\u5b54\u5219\u4e3a\u7ec6\u80de\u7684\u8fc1\u79fb\u6216\u8fd0\u8f93\u63d0\u4f9b\u4e86\u4e00\u6761\u4fbf\u6377\u7684\u8def\u5f84\uff0c\u4e5f\u4e3a\u9aa8\u7684\u751f\u957f\u63d0\u4f9b\u4e86\u8db3\u591f\u7684\u7a7a\u95f4\u3002L2C4S4\u652f\u67b6\u5728\u4f53\u5185\u8868\u73b0\u51fa\u660e\u663e\u7684\u78f7\u7070\u77f3\u77ff\u5316\u548c\u8f6f\u9aa8\u4e0b\u9aa8\u751f\u957f\uff0c\u4f46\u4e00\u65e6\u5b8c\u6210\u5176\u5de5\u4f5c\uff0c\u4fbf\u53ef\u8fdb\u884c\u751f\u7269\u964d\u89e3\u3002\u53cc\u6d3b\u6027\u751f\u7269\u9676\u74f7L2C4S4\u652f\u67b6\u4e3a\u9aa8\u8f6f\u9aa8\u7f3a\u635f\u7684\u518d\u751f\u63d0\u4f9b\u4e86\u4e00\u79cd\u667a\u80fd\u7684\u89e3\u51b3\u65b9\u6848\u3002<\/p>\n<p>Figure 4. Abstract picture of article<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-168476 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u724710-9.png\" alt=\"\" width=\"293\" height=\"210\" \/><\/p>\n<p><strong><b>\u5168\u6587\u94fe\u63a5\uff1a<a href=\"https:\/\/www.sciencedirect.com\/science\/article\/pii\/S1369702118310423?via%3Dihub\">https:\/\/www.sciencedirect.com\/science\/article\/pii\/S1369702118310423?via%3Dihub<\/a><\/b><\/strong><\/p>\n<p><strong><b>5.\u82cf\u9ece\u4e16\u8054\u90a6\u7406\u5de5\u5b66\u9662-Three-dimensional printing of hierarchical liquid-crystal-polymer structures<\/b><\/strong><\/p>\n<p>Silvan Gantenbein\u7b49\u4eba\u4e8e2018\u5e74\u5728Nature\u4e0a\uff0c\u53d1\u8868\u4e86\u4e09\u7ef4\u6253\u5370\u591a\u7ea7\u5206\u5c42\u6db2\u6676\u805a\u5408\u7269\u7684\u7814\u7a76\u3002\u98de\u673a\u3001\u8f66\u8f86\u548c\u751f\u7269\u533b\u5b66\u690d\u5165\u7269\u7b49\u5747\u9700\u8981\u9ad8\u5f3a\u5ea6\uff0c\u4f46\u53c8\u4e0d\u80fd\u592a\u8fc7\u6c89\u91cd\uff0c\u56e0\u6b64\u5177\u6709\u7406\u60f3\u529b\u5b66\u5f3a\u5ea6\u4f46\u540c\u65f6\u8d28\u91cf\u8f7b\u4fbf\u7684\u6750\u6599\u4e00\u76f4\u662f\u5404\u9886\u57df\u4e89\u5148\u7814\u7a76\u7684\u91cd\u70b9\u3002\u7ea4\u7ef4\u589e\u5f3a\u805a\u5408\u7269\u7ed3\u6784\u5177\u6709\u5f88\u9ad8\u7684\u521a\u5ea6\u548c\u5f3a\u5ea6\uff0c\u4f46\u5b83\u9700\u8981\u8017\u8d39\u5927\u91cf\u7684\u80fd\u6e90\u548c\u52b3\u529b\u6765\u5236\u9020\uff0c\u800c\u4e14\u6613\u53d1\u751f\u8106\u6027\u65ad\u88c2\uff0c\u96be\u4ee5\u6210\u5f62\u548c\u56de\u6536\u3002\u8fd9\u4e0e\u9aa8\u9abc\u3001\u4e1d\u7ef8\u548c\u6728\u6750\u7b49\u8f7b\u8d28\u751f\u7269\u6750\u6599\u5f62\u6210\u4e86\u9c9c\u660e\u7684\u5bf9\u6bd4\uff0c\u8fd9\u4e9b\u6750\u6599\u901a\u8fc7\u5b9a\u5411\u81ea\u7ec4\u88c5\u5f62\u6210\u590d\u6742\u7684\u5c42\u6b21\u5316\u5f62\u72b6\uff0c\u5177\u6709\u4f18\u5f02\u7684\u673a\u68b0\u6027\u80fd\uff0c\u5e76\u80fd\u591f\u5faa\u73af\u96c6\u6210\u5230\u73af\u5883\u4e2d\u3002\u8be5\u7814\u7a76\u56e2\u961f\u50cf\u6211\u4eec\u5c55\u793a\u4e86\u4e00\u79cd\u4e09\u7ef4(3D)\u6253\u5370\u65b9\u6cd5\uff0c\u4ee5\u751f\u6210\u5177\u6709\u5c42\u6b21\u7ed3\u6784\u3001\u590d\u6742\u51e0\u4f55\u5f62\u72b6\u548c\u524d\u6240\u672a\u6709\u7684\u521a\u5ea6\u548c\u97e7\u6027\u7684\u53ef\u56de\u6536\u8f7b\u91cf\u7ea7\u7ed3\u6784\u3002\u5b83\u4eec\u7684\u7279\u70b9\u662f\u5728\u7194\u878d\u539f\u6599\u6324\u538b\u8fc7\u7a0b\u4e2d\uff0c\u6db2\u6676\u805a\u5408\u7269\u5206\u5b50\u81ea\u7ec4\u88c5\u6210\u9ad8\u5ea6\u5b9a\u5411\u7684\u7ed3\u6784\u57df\u3002\u901a\u8fc7\u5c06\u5206\u5b50\u533a\u57df\u5b9a\u4f4d\u5728\u6253\u5370\u8def\u5f84\u4e0a\uff0c\u80fd\u591f\u6839\u636e\u9884\u671f\u7684\u673a\u68b0\u5e94\u529b\u6765\u589e\u5f3a\u805a\u5408\u7269\u7ed3\u6784\uff0c\u4ece\u800c\u4f7f\u5176\u521a\u5ea6\u3001\u5f3a\u5ea6\u548c\u97e7\u6027\u5728\u6570\u91cf\u7ea7\u4e0a\u8d85\u8fc7\u6700\u5148\u8fdb\u76843d\u6253\u5370\u805a\u5408\u7269\uff0c\u5e76\u53ef\u4e0e\u6027\u80fd\u6700\u9ad8\u7684\u8f7b\u8d28\u5316\u5408\u7269\u5ab2\u7f8e\u3002<\/p>\n<p>Fig. 5: Printing hierarchical, thermotropic LCPs using fused deposition modelling.<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-168477 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u724711-9.png\" alt=\"\" width=\"553\" height=\"294\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u724711-9.png 553w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/02\/\u56fe\u724711-9-300x159.png 300w\" sizes=\"(max-width: 553px) 100vw, 553px\" \/><\/p>\n<p>\u5168\u6587\u94fe\u63a5\uff1a<a href=\"https:\/\/www.nature.com\/articles\/s41586-018-0474-7\"><u>https:\/\/www.nature.com\/articles\/s41586-018-0474-7<\/u><\/a><\/p>\n<p>\u5355\u7eaf\u5730\u4ee5\u4e09\u7ef4\u6253\u5370\u4e3a\u521b\u65b0\u70b9\u6253\u5370\u6750\u6599\u5df2\u4e0d\u518d\u662f\u53d1\u8bba\u6587\u7684\u901a\u884c\u8bc1\u3002\u4e09\u7ef4\u6253\u5370\u6280\u672f\u5df2\u53d1\u5c55\u76f8\u5bf9\u6210\u719f\uff0c\u548c\u6a21\u5177\u6210\u578b\u3001\u51b7\u51bb\u5e72\u71e5\u3001\u9759\u7535\u7eba\u4e1d\u7b49\u65b9\u6cd5\u4e00\u6837\uff0c\u4e09\u7ef4\u6253\u5370\u53ea\u662f\u4e00\u79cd\u52a0\u5de5\u5236\u9020\u7684\u6280\u672f\u3002\u672a\u6765\u7684\u521b\u65b0\u70b9\uff0c\u4e00\u662f\u5728\u4e8e\u6280\u672f\u65b9\u9762\u7684\u521b\u65b0\u3002\u50cf\u4e0a\u6587Science\u4e0a\u53d1\u8868\u7684\u8f74\u5411\u5149\u523b\u6253\u5370\u4e00\u6837\uff0c\u80fd\u5426\u6539\u8fdb\u4e09\u7ef4\u6253\u5370\u6210\u578b\u6280\u672f\uff0c\u4f7f\u5176\u901f\u5ea6\u66f4\u5feb\u3001\u7cbe\u5ea6\u66f4\u9ad8\uff0c\u662f\u4e00\u4e2a\u91cd\u8981\u7684\u7a81\u7834\u70b9\u3002\u53e6\u4e00\u65b9\u9762\uff0c\u5982\u4f55\u5bfb\u627e\u6216\u5236\u5907\u66f4\u591a\u80fd\u9002\u7528\u4e8e\u4e09\u7ef4\u6253\u5370\u7684\u6750\u6599\uff0c\u4f9d\u7136\u662f\u7814\u7a76\u7684\u91cd\u70b9\u548c\u70ed\u70b9\u3002<\/p>\n<p>\u751f\u7269\u533b\u5b66\u9886\u57df\u65b9\u9762\uff0c\u5982\u4f55\u8bbe\u8ba1\u4e0d\u540c\u7684\u7ed3\u6784\u5c3a\u5bf8\u3001\u4e09\u7ef4\u6253\u5370\u51fa\u7279\u5b9a\u5f62\u72b6\u7684\u652f\u67b6\uff0c\u5e76\u7cfb\u7edf\u7814\u7a76\u652f\u67b6\u6750\u6599\u529b\u5b66\u4e0e\u7ed3\u6784\u529b\u5b66\uff0c\u89e3\u51b3\u4e09\u7ef4\u6253\u5370\u652f\u67b6\u5f62\u72b6\u6613\u6536\u7f29\u95ee\u9898\u4e5f\u662f\u4e0d\u9519\u7684\u7814\u7a76\u65b9\u5411\uff0cScience\u4e0a\u4e5f\u7740\u91cd\u63d0\u51fa\u8fc7Shrinking\u00a0problem in 3d printing\u3002\u6b64\u5916\uff0c\u5c06\u4e09\u7ef4\u6253\u5370\u5236\u5907\u5f97\u5230\u7684\u652f\u67b6\u8fdb\u884c\u66f4\u5168\u9762\u7cfb\u7edf\u7684\u4f53\u5916\u53ca\u4f53\u5185\u5b9e\u9a8c\uff0c\u589e\u52a0\u5b9e\u9a8c\u7684\u6df1\u5ea6\uff0c\u4e5f\u5bb9\u6613\u8ba9\u4f60\u7684\u7814\u7a76\u53d1\u8868\u5728\u9876\u7ea7\u671f\u520a\u4e0a\u3002\u80fd\u6e90\u9886\u57df\uff0c\u7531\u4e8e\u80fd\u6e90\u6700\u8fd1\u662f\u5927\u70ed\u7684\u7814\u7a76\u65b9\u5411\uff0c\u56e0\u6b64\u5c06\u4e09\u7ef4\u6253\u5370\u4e0e\u65b0\u80fd\u6e90\u6750\u6599\u7ed3\u5408\u8d77\u6765\uff0c\u5bfb\u6c42\u5176\u5728\u50a8\u80fd\u3001\u50a8\u7535\u65b9\u9762\u7684\u5e94\u7528\uff0c\u5c06\u5177\u6709\u6781\u5927\u7684\u7814\u7a76\u53ca\u5e94\u7528\u4ef7\u503c\u3002\u8fd1\u4e24\u5e74Advanced materials \u548cAdvanced energy materials\u53d1\u8868\u7684\u4e09\u7ef4\u6253\u5370\u76f8\u5173\u8bba\u6587\u5927\u90e8\u5206\u90fd\u662f\u9488\u5bf9\u4e8e\u80fd\u6e90\u9886\u57df\u7684\u3002<\/p>\n<p><strong><b>\u770b\u5230\u79d1\u7814\u5927\u4f6c\u4eec\u7684\u8bba\u6587\uff0c\u6709\u6ca1\u6709\u53d7\u5230\u542f\u53d1\u5462\uff0c\u671f\u5f85\u4f60\u7684\u6587\u7ae0\u4e5f\u51fa\u73b0\u5728<\/b><\/strong><strong><b>top<\/b><\/strong><strong><b>\u6742\u5fd7\u4e0a\uff01<\/b><\/strong><\/p>\n<p>\u5f80\u671f\u56de\u987e\uff1a<\/p>\n<p><a class=\"title info_flow_news_title\" href=\"http:\/\/www.cailiaoniu.com\/164101.html\" target=\"_blank\" rel=\"noopener\">\u76d8\u70b9\u56fd\u5916\u751f\u72693D\u6253\u5370\u7684\u5341\u4f4d\u5927\u725b\uff08\u4e8c\uff09<\/a><\/p>\n<p><a class=\"title info_flow_news_title\" href=\"http:\/\/www.cailiaoniu.com\/162255.html\" target=\"_blank\" rel=\"noopener\">\u60f3\u4e86\u89e33D\u6253\u5370\uff0c\u4ece\u8fd9\u5341\u7bc7\u7efc\u8ff0\u5f00\u59cb<\/a><\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/162091.html\">\u76d8\u70b9\u56fd\u5185\u751f\u72693D\u6253\u5370\u9886\u57df\u7684\u5341\u4f4d\u5927\u725b<\/a><\/p>\n<p><a class=\"title info_flow_news_title\" href=\"http:\/\/www.cailiaoniu.com\/159304.html\" target=\"_blank\" rel=\"noopener\">\u5e26\u4f60\u8d70\u8fdb\u751f\u72693D\u6253\u5370\u7684\u4e16\u754c<\/a><\/p>\n<p><a class=\"title info_flow_news_title\" href=\"http:\/\/www.cailiaoniu.com\/112629.html\" target=\"_blank\" rel=\"noopener\">\u75283D\u6253\u5370\u623f\u5b50\u5df2\u7ecf\u4e0d\u662f\u4e8b\u513f\uff0c\u4f46\u4f60\u6562\u4f4f\u5417\uff1f<\/a><\/p>\n<p>\u672c\u6587\u7531<strong>\u6750\u6599\u4eba\u4e13\u680f\u4f5c\u8005\u675c\u8001\u5e08<\/strong><strong><b>\u4f9b\u7a3f\uff0c<\/b><\/strong>\u6750\u6599\u4eba\u7f16\u8f91\u90e8Alisa\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8bed\u3011 \u62a5\u544a\u5206\u6790 \u6750\u6599\u4eba\u73b0\u5728\u8bbe\u7acb\u5404\u79cd\u6587\u7ae0\u4e13\u680f\uff0c\u6240\u6d89\u53ca\u9886\u57df\u6b63\u5728\u6162\u6162\u5b8c\u5584\uff0c\u7531\u6b64\u4e5f\u9700\u8981\u66f4\u591a\u7684\u4e13\u680f\u4f5c\u8005\uff0c\u671f\u5f85\u4f60\u4eec\u7684\u52a0\u5165\uff0c\u6709\u610f\u5411\u7684\u5c0f\u4f19\u4f34\u76f4\u63a5\u5fae\u4fe1\u8054\u7cfbcailiaoren&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":174190,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-168471","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/168471"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=168471"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/168471\/revisions"}],"predecessor-version":[{"id":168984,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/168471\/revisions\/168984"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/174190"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=168471"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=168471"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=168471"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}