{"id":174339,"date":"2019-04-29T06:30:26","date_gmt":"2019-04-28T22:30:26","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=174339"},"modified":"2019-04-28T11:53:42","modified_gmt":"2019-04-28T03:53:42","slug":"%e8%82%96%e6%b3%bd%e6%96%87-%e9%84%a2%e7%82%8e%e5%8f%91%e6%95%99%e6%8e%88am%e8%89%af%e5%bf%83%e7%bb%bc%e8%bf%b0%ef%bc%9a%e9%92%99%e9%92%9b%e7%9f%bf%e6%97%a0%e9%93%85%e5%8c%96%e7%9a%84","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=174339","title":{"rendered":"\u8096\u6cfd\u6587\/\u9122\u708e\u53d1\u6559\u6388AM\u826f\u5fc3\u7efc\u8ff0\uff1a\u9499\u949b\u77ff\u65e0\u94c5\u5316\u7684\u201c\u56e0\u201d\u4e0e\u201c\u679c\u201d"},"content":{"rendered":"<p><b>\u3010<strong>\u5f15\u8a00<\/strong>\u3011<\/b><\/p>\n<p>\u94c5\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u56e0\u5176\u4f18\u5f02\u7684\u5149\u7535\u6027\u80fd\u548c\u4f4e\u5236\u4f5c\u6210\u672c\uff08\u4f4e\u95e8\u69db\uff09\u800c\u6210\u4e3a\u5f53\u4eca\u7814\u7a76\u70ed\u70b9\u3002\u7136\u800c\uff0c\u5176\u6b20\u4f73\u7684\u7a33\u5b9a\u6027\u548c\u94c5\u7684\u6bd2\u6027\uff0c\u4f7f\u5176\u5546\u4e1a\u5316\u9762\u4e34\u6311\u6218\u3002\u56e0\u6b64\uff0c\u5bfb\u627e\u65e0\u6bd2\u3001\u7a33\u5b9a\u3001\u9ad8\u6548\u7684\u9499\u949b\u77ff\u578b\u592a\u9633\u80fd\u7535\u6c60\u6750\u6599\u6210\u4e86\u53c8\u4e00\u7814\u7a76\u70ed\u70b9\u3002\u7136\u800c\uff0c\u5728\u592a\u9633\u80fd\u7535\u6c60\u5e94\u7528\u65b9\u9762\uff0c\u76ee\u524d\u6240\u5f97\u7684\u201c\u65e0\u94c5\u201d\u9499\u949b\u77ff\u7686\u65e0\u6cd5\u4e0e\u94c5\u57fa\u9499\u949b\u77ff\u76f8\u5ab2\u7f8e\u3002<\/p>\n<p><b>\u3010<strong>\u6210\u679c\u7b80\u4ecb<\/strong>\u3011<\/b><\/p>\n<p>\u6700\u8fd1\uff0c<strong><b>\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u6b66\u6c49\u5149\u7535\u56fd\u5bb6\u7814\u7a76\u4e2d\u5fc3\u8096\u6cfd\u6587(<\/b><\/strong><strong><b>Zewen Xiao)<\/b><\/strong><strong><b>\u6559\u6388<\/b><\/strong>\u4e0e<strong><b>\u7f8e\u56fdToledo\u5927\u5b66\u7269\u7406\u4e0e\u5929\u6587\u5b66\u7cfb\u5b8b\u8087\u5b81(<\/b><\/strong><strong><b>Zhaoning Song)<\/b><\/strong><strong><b>\u52a9\u7406\u6559\u6388\u548c\u9122\u708e\u53d1(<\/b><\/strong><strong><b>Yanfa Yan)<\/b><\/strong><strong><b>\u6559\u6388<\/b><\/strong>\u5408\u4f5c\uff0c\u5728 <strong><b>Advanced<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Materials<\/b><\/strong><strong><b>\u00a0<\/b><\/strong>\u4e0a\u53d1\u8868\u4e86\u4e00\u7bc7\u540d\u4e3a\u201c<strong><b>From Lead Halide Perovskites to Lead-Free Metal<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Halide Perovskites and Perovskite Derivatives<\/b><\/strong>\u201d\u7684\u7279\u9080\u7efc\u8ff0\u6587\u7ae0\u3002<\/p>\n<p>\u5728\u8fd9\u7bc7\u7efc\u8ff0\u4e2d\uff0c\u4f5c\u8005\u9996\u5148\u5f00\u95e8\u89c1\u5c71\u5730\u603b\u7ed3\u4e86\u201c\u65e0\u94c5\u5316\u201d\u7684\u65b9\u6cd5\u548c\u7ed3\u679c\uff1b\u63a5\u7740\uff0c\u57fa\u7840\u6027\u5730\u9610\u8ff0\u4e86\u94c5\u5364\u5316\u7269\u9499\u949b\u77ff\u7684\u4f18\u5f02\u5149\u4f0f\u7279\u6027\u7684\u6839\u672c\u539f\u56e0\uff1b\u7136\u540e\uff0c\u9010\u4e00\u5206\u6790\u4e86\u5404\u7c7b\u65e0\u94c5\u9499\u949b\u77ff\u7684\u5149\u7535\u6027\u80fd\u6b20\u4f73\u7684\u6839\u672c\u539f\u56e0\uff1b\u6700\u540e\uff0c\u4f5c\u8005\u5bf9\u65e0\u94c5\u9499\u949b\u77ff\u7684\u5e94\u7528\u524d\u666f\u548c\u53d1\u5c55\u65b9\u5411\u505a\u51fa\u4e86\u5c55\u671b\u3002<\/p>\n<p><b>\u3010<strong>\u6838\u5fc3\u89c2\u70b9<\/strong>\u3011<\/b><\/p>\n<p><strong><b>\u94c5\uff08Pb\uff09\u5143\u7d20\u66ff\u6362<\/b><\/strong><strong><b>\u6982\u8ff0<\/b><\/strong><\/p>\n<p>Pb\u7684\u66ff\u6362\u6309\u7167\u4ef7\u6001\u53ef\u5206\u4e3a\u4e24\u7c7b\uff1a\uff08i\uff09\u540c\u4ef7\u66ff\u6362\uff08\u6bd4\u5982Sn(II)\u3001Ge(II)\u7b49\uff09\uff1b\uff08ii\uff09\u5f02\u4ef7\u66ff\u6362\uff08\u6bd4\u5982Bi(III)\u3001Sb(III)\u7b49\uff09\u3002\u540c\u4ef7\u5143\u7d20\u66ff\u6362\u53ef\u4ee5\u4fdd\u6301\u4e09\u7ef4\u9499\u949b\u77ff\u7ed3\u6784\uff0c\u4f46\u7a33\u5b9a\u6027\u6b20\u4f73\u3002\u5bf9\u4e8e\u5f02\u4ef7\u5143\u7d20\u66ff\u6362\uff0c\u4e3a\u4fdd\u6301\u7535\u4e2d\u6027\u6761\u4ef6\uff0c\u53ef\u4ee5\u91c7\u53d6\u4e24\u79cd\u66ff\u6362\u65b9\u5f0f\u3002\u4e00\u79cd\u662f\u201c\u79bb\u5b50\u5288\u88c2\u201d\uff0c\u5373\u901a\u8fc7\u5c06Pb(II)\u5288\u88c2\u6210\u4e00\u4ef7\u548c\u4e09\u4ef7\u9633\u79bb\u5b50\u7684\u7ec4\u5408\u5f62\u6210\u53cc\u9499\u949b\u77ff\u7ed3\u6784\uff0c\u6216\u5728\u5355\u4e00\u5f02\u4ef7\u9633\u79bb\u5b50\u66ff\u6362Pb(II)\u7684\u540c\u65f6\u5f15\u5165\u6df7\u5408\u4ef7\u6001\u9634\u79bb\u5b50\u3002\u9633\u79bb\u5b50\u7684\u5288\u88c2\u867d\u7136\u4fdd\u6301\u4e09\u7ef4\u6676\u4f53\u7ed3\u6784\uff0c\u4f46\u901a\u5e38\u56e0\u5176\u964d\u4f4e\u7684\u7535\u5b50\u7ef4\u5ea6\u800c\u8868\u73b0\u51fa\u6b20\u4f73\u7684\u5149\u7535\u6027\u80fd\uff1b\u9634\u79bb\u5b50\u5288\u88c2\u80fd\u5f97\u5230\u7c7b\u4f3c\u94c5\u57fa\u9499\u949b\u77ff\u7684\u4f18\u5f02\u6027\u80fd\uff0c\u4f46\u5728\u5b9e\u9a8c\u4e0a\u96be\u4ee5\u5408\u6210\u3002\u53e6\u4e00\u79cd\u5219\u662f\u901a\u8fc7\u5f62\u6210\u7a7a\u4f4d\u6765\u7ef4\u6301\u7535\u4e2d\u6027\u6761\u4ef6\u3002\u7136\u800c\u7a7a\u4f4d\u7684\u5f62\u6210\u5c06\u539f\u6709\u7684\u4e09\u7ef4\u9499\u949b\u77ff\u7ed3\u6784\u201c\u5207\u5272\u201d\u6210\u4e86\u4f4e\u7ef4\u5ea6\u7684\u6676\u4f53\u7ed3\u6784\uff0c\u4ece\u800c\u964d\u4f4e\u7535\u5b50\u7ef4\u5ea6\uff0c\u201c\u6bc1\u706d\u201d\u4e86\u94c5\u57fa\u9499\u949b\u77ff\u539f\u6709\u7684\u4f18\u5f02\u5149\u7535\u6027\u80fd\u3002<\/p>\n<p><strong><b>\u94c5\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff\u201c\u5f97\u5929\u72ec\u539a\u201d\u7684\u7279\u6027\uff1a\u5e38\u5e38\u88ab\u6a21\u4eff\uff0c\u65e0\u6cd5\u88ab\u8d85\u8d8a<\/b><\/strong><\/p>\n<p>\uff08i\uff09\u9499\u949b\u77ff\u7ed3\u6784\u7684\u9ad8\u5bf9\u79f0\u6027\u3002\u9996\u5148\u8bd5\u60f3\uff1a\u4e8c\u5143PbI<sub>2<\/sub>\u7684\u5e26\u9699\u4e3a2.3eV\uff0c\u4e3a\u4ec0\u4e48\u5f15\u5165\u9ad8\u79bb\u5b50\u6027\u7684CsI\u6216MAI\uff08\u5177\u6709\u66f4\u5bbd\u5e26\u9699\uff09\u5374\u80fd\u5f97\u5230\u5e26\u9699\u4f4e\u81f31.5eV\uff08\u9002\u5408\u4e8e\u5438\u5149\u6750\u6599\uff09\u7684APbI<sub>3<\/sub>\uff1f\u6ca1\u9519\uff0c\u5c31\u662f\u56e0\u4e3a\u5176\u9499\u949b\u77ff\u7ed3\u6784\u7684<em><i>O<\/i><\/em><sub>h<\/sub>\u9ad8\u5bf9\u79f0\u6027\uff0c\u4f7f\u5176Pb\u00a06p\u7ec4\u6210\u7684\u5bfc\u5e26\u5e95\uff08CBM\uff09\u5177\u6709\u4e09\u91cd\u7b80\u5e76\u6027\uff0c\u4ece\u800c\u4f7f\u5bfc\u5e26\u5c55\u5bbd\uff0c\u964d\u4f4e\u5e26\u9699\u3002\u53e6\u4e00\u65b9\u9762\uff0c\u5728<em><i>O<\/i><\/em><sub>h<\/sub>\u5bf9\u79f0\u73af\u5883\u4e0b\uff0c\u5364\u7d20p\u8f68\u9053\u4e0ePb\u00a06s\u8f68\u9053\u7684\u8026\u5408\u4f5c\u7528\u4e5f\u589e\u5f3a\uff0c\u4f7f\u5f97\u4ef7\u5e26\u9876\uff08VBM\uff09\u63d0\u9ad8\u3002\u5728\u6b64\u57fa\u7840\u4e0a\uff0c\u5c31\u4e0d\u96be\u7406\u89e3\u4e3a\u4ec0\u4e48\u5404\u79cd\u975e\u9499\u949b\u77ff\u7ed3\u6784\uff08\u4f4e\u5bf9\u79f0\u6027\uff09\u7684\u884d\u751f\u7269\uff08\u6bd4\u5982CsPbI<sub>3<\/sub>\u7684d\u76f8\uff09\u901a\u5e38\u8868\u73b0\u51fa\u8f83\u5927\u7684\u5e26\u9699\u548c\u6b20\u4f73\u7684\u8f7d\u6d41\u5b50\u4f20\u8f93\u7279\u6027\u3002<\/p>\n<p>\uff08ii\uff09Pb(II)\u72ec\u7279\u76846s<sup>2<\/sup>p<sup>0<\/sup>\u7535\u5b50\u6392\u5e03\u6784\u578b\u3002Pb\u76846s<sup>2<\/sup>\u8f68\u9053\u80fd\u7ea7\u4f4d\u7f6e\u201c\u6070\u5230\u597d\u5904\u201d\uff0c\u65e2\u80fd\u4e0e\u5364\u7d20p\u8f68\u9053\u5f62\u6210\u53cd\u952e\u6001\u63a8\u9ad8\u4ef7\u5e26\u9876\uff08\u51cf\u5c0f\u5e26\u9699\uff09\uff0c\u53c8\u4e0d\u5bb9\u6613\u5931\u53bbs<sup>2<\/sup>\u7535\u5b50\u800c\u6c27\u5316\u6210Pb(IV)\u3002\u5177\u6709\u7c7b\u4f3c\u7535\u5b50\u6392\u5e03\u6784\u578b\u7684In(I)\u3001Tl(I)\u3001Sn(II)\u3001Bi(III)\u3001Sb(III)\u5219\u4e0d\u5177\u6709\u8fd9\u79cd\u201c\u5f97\u5929\u72ec\u539a\u201d\u7684s<sup>2<\/sup>\u80fd\u7ea7\u4f4d\u7f6e\u3002\u5176\u4e2d\uff0cIn(I)\u3001Tl(I)\u548cSn(II)\u7684s<sup>2<\/sup>\u6bd4Pb(II)\u7684s<sup>2<\/sup>\u7684\u80fd\u7ea7\u6d45\uff0c\u5bb9\u6613\u5931\u53bbs<sup>2<\/sup>\u7535\u5b50\u800c\u88ab\u6c27\u5316\u6210In(III)\u3001Tl(III)\u548cSn(IV)\uff0c\u96be\u4ee5\u5f62\u6210\u7a33\u5b9a\u7684\u5364\u5316\u7269\u9499\u949b\u77ff\u3002\u800cBi(III)\u548cSb(III)\u7684s<sup>2<\/sup>\u6bd4Pb(II)\u7684s<sup>2<\/sup>\u7684\u80fd\u7ea7\u6df1\uff0c\u5176\u4f18\u70b9\u662f\u4e0d\u5bb9\u6613\u88ab\u6c27\u5316\u6210Bi(V)\u548cSb(V)\u800c\u8868\u73b0\u51fa\u4e00\u5b9a\u7684\u7a33\u5b9a\u6027\uff0c\u800c\u7f3a\u70b9\u662f\u5373\u4fbf\u80fd\u5f62\u6210\u4e09\u7ef4\u9499\u949b\u77ff\u4e5f\u4e0d\u80fd\u50cfPb(II)\u90a3\u6837\u63a8\u9ad8\u4ef7\u5e26\u9876\u4ece\u800c\u964d\u4f4e\u5e26\u9699\uff0c\u66f4\u4f55\u51b5Bi(III)\u548cSb(III)\u57fa\u9499\u949b\u77ff\u901a\u5e38\u662f\u4f4e\u7ef4\u5ea6\u7684\u7ed3\u6784\uff0c\u4f7f\u5f97\u5e26\u9699\u8fdb\u4e00\u6b65\u53d8\u5927\u3002<\/p>\n<p>\u57fa\u4e8e\u4ee5\u4e0a\u4e24\u4e2a\u4e3b\u8981\u56e0\u7d20\uff0cPb(II)\u57fa\u7898\u5316\u7269\u9499\u949b\u77ff\u8868\u73b0\u51fa\u8f83\u7406\u60f3\u7684\u5149\u7535\u6027\u8d28\uff1a\u8f83\u5408\u9002\u7684\u76f4\u63a5\u5e26\u9699\u3001\u8f83\u4f4e\u7684\u6709\u6548\u8d28\u91cf\u3001\u8f83\u9ad8\u7684\u5149\u5b66\u5438\u6536\u7cfb\u6570\u3001\u8f83\u597d\u7684\u7f3a\u9677\u5bb9\u5fcd\u6027\u548c\u4e0d\u7b97\u592a\u5dee\u7684\u7a33\u5b9a\u6027\u3002\u4efb\u4f55\u964d\u4f4e\u4e09\u7ef4\u9499\u949b\u77ff\u9ad8\u5bf9\u79f0\u6027\u548c\u7ef4\u5ea6\u6216\u66ff\u6362\u201c\u6070\u5230\u597d\u5904\u201d\u7684Pb(II)\u7684\u4e3e\u63aa\u90fd\u5c06\u6216\u591a\u6216\u5c11\u5730\u635f\u5bb3Pb(II)\u57fa\u7898\u5316\u7269\u9499\u949b\u77ff\u201c\u5929\u7136\u201d\u7684\u4f18\u5f02\u6027\u8d28\uff0c\u4f7f\u5f97\u201c\u65e0\u94c5\u5316\u201d\u4e4b\u8def\u5145\u6ee1\u6311\u6218\u3002<\/p>\n<p><b>\u3010<strong>\u5c0f\u7ed3<\/strong>\u3011<\/b><\/p>\n<p>\uff08i\uff09\u94c5\u5364\u5316\u7269\u9499\u949b\u77ff\u7684\u4f18\u5f02\u5149\u7535\u6027\u80fd\u4e3b\u8981\u6765\u6e90\u4e8e\u9499\u949b\u77ff\u7ed3\u6784\u7684\u9ad8\u5bf9\u79f0\u6027\u548c\u9ad8\u7535\u5b50\u7ef4\u5ea6\u3001Pb(II)\u76846s\u8f68\u9053\u5b64\u5bf9\u7535\u5b50\u3001\u975e\u6d3b\u6027\u7684Pb(II)6p\u8f68\u9053\u3001\u5bf9SOC\u7684\u654f\u611f\u6027\u3001\u6781\u6027\u6709\u673a\u9633\u79bb\u5b50\u7684\u6392\u5217\u548c\u5364\u5316\u7269\u7684\u79bb\u5b50\u6027\u8d28\u7b49\u3002<\/p>\n<p>\uff08ii\uff09\u4ee5\u65e0\u6bd2\u7684\u5f02\u4ef7\u5143\u7d20In(I)\u3001Sb(III)\u548cBi(III)\u548c\u540c\u4ef7\u5143\u7d20Ge(II)\u3001Sn(II)\u7b49\u66ff\u4ee3Pb\u53ef\u4ee5\u7ef4\u6301\u5b64\u5bf9s\u7535\u5b50\u548c\u975e\u6d3b\u6027p\u8f68\u9053\u7684\u7535\u5b50\u7279\u6027\u3002In(I)\u7531\u4e8e\u9ad8\u80fd\u91cf\u76845s\u8f68\u9053\u5bfc\u81f4\u5176\u6781\u4e0d\u7a33\u5b9a\uff1bSb(III)\u548cBi(III)\u5219\u4f1a\u5bfc\u81f4\u9499\u949b\u77ff\u5177\u6709\u4f4e\u7ef4\u7ed3\u6784\u6216\u4f4e\u7535\u5b50\u7ef4\u5ea6\uff0c\u8fd9\u6781\u5927\u5730\u9650\u5236\u4e86\u57fa\u4e8e\u5b83\u4eec\u5236\u4f5c\u7684\u592a\u9633\u80fd\u7535\u6c60\u7684\u6027\u80fd\u3002<strong><b>\u4f46\u662f\uff0c\u8fd9\u4e9b\u5316\u5408\u7269\u5728\u5149\u7535\u63a2\u6d4b\u5668\u548c\u53d1\u5149\u5668\u4ef6\u7b49\u5176\u4ed6\u5e94\u7528\u4e2d\u6781\u5177\u6f5c\u529b\u3002<\/b><\/strong><\/p>\n<p>\uff08iii\uff09\u7528Sn(II)\u6216Ge(II)\u66ff\u4ee3Pb(II)\u7684\u9499\u949b\u77ff\u7ed3\u6784\u80fd\u591f\u7ef4\u6301\u4e09\u7ef4\u7ed3\u6784\u548c\u7535\u5b50\u7ef4\u5ea6\u3002\u7531\u4e8e\u5177\u6709\u66f4\u4f4e\u7684\u6210\u672c\u548c\u66f4\u9ad8\u7684\u7a33\u5b9a\u6027\uff0cSn(II)\u662f\u6bd4Ge(II)\u66f4\u597d\u7684\u9009\u62e9\u3002 \u5b9e\u9645\u4e0a\uff0cSn\u57fa\u7535\u6c60\u5df2\u7ecf\u5728\u65e0\u94c5\u5364\u5316\u7269\u9499\u949b\u77ff\u7535\u6c60\u4e2d\u8868\u73b0\u51fa\u4e86\u6700\u597d\u7684\u6548\u679c\u3002\u56e0\u4e3aSn\u76845s\u80fd\u91cf\u9ad8\u4e8ePb\u76846s\uff0c \u5bfc\u81f4\u7a33\u5b9a\u6027\u4e0d\u5982\u94c5\u5364\u5316\u7269\u9499\u949b\u77ff\u3002\u8fdb\u4e00\u6b65\u63d0\u9ad8Sn\u57fa\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u6548\u7387\u7684\u65b9\u6cd5\u5305\u62ec\u4f7f\u7528\u4e8c\u7ef4\u4e09\u7ef4\u6df7\u5408\u7ed3\u6784\u6765\u907f\u514dSn\u7684\u635f\u5931\uff0c\u63ba\u5165\u65bd\u4e3b\u5143\u7d20\u6216\u8005\u6297\u6c27\u5316\u5242\u7b49\u3002<\/p>\n<p>\u867d\u7136\u5bf9\u4e8e\u65e0\u94c5\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u7684\u7814\u7a76\u4ecd\u7136\u9762\u4e34\u6311\u6218\uff0c\u4f46\u662f\u76ee\u524d\u7684\u7814\u7a76\u8fdb\u5c55\u4ecd\u7136\u5bf9\u6b64\u9886\u57df\u4ea7\u751f\u4e86\u91cd\u5927\u5f71\u54cd\uff0c\u8fd9\u4ecd\u5c06\u662f\u4e00\u4e2a\u6781\u5177\u5438\u5f15\u529b\u7684\u7814\u7a76\u65b9\u5411\u3002<\/p>\n<p><b>\u3010<strong>\u56fe\u6587\u5bfc\u8bfb<\/strong>\u3011<\/b><\/p>\n<p><strong><b>\u56fe1\u94c5\uff08Pb\uff09\u5143\u7d20\u66ff\u6362\u5404\u79cd\u65b9\u6cd5\u548c\u7ed3\u679c\u793a\u610f\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174344 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72477-16.png\" alt=\"\" width=\"600\" height=\"488\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72477-16.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72477-16-300x244.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/> \u00a0\u00a0\u00a0<\/p>\n<p><strong><b>\u56fe2<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u94c5\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff\u7684\u9ad8\u5149\u5b66\u5438\u6536\u6548\u7387<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174345 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72478-15.png\" alt=\"\" width=\"600\" height=\"319\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72478-15.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72478-15-300x160.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09Si(\u5de6)\u3001GaAs(\u4e2d)\u548cMAPbI<sub>3<\/sub>\u9499\u949b\u77ff(\u53f3)\u7684\u5149\u5438\u6536\u539f\u7406\u56fe\u3002<\/p>\n<p>\uff08b\uff09MAPbI<sub>3<\/sub>\u548cGaAs\u7684\u6001\u5bc6\u5ea6\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08c\uff09MAPbI<sub>3<\/sub>\u548cGaAs\u7684\u8054\u5408\u6001\u5bc6\u5ea6\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08d\uff09MAPbI<sub>3<\/sub>\u548cGaAs\u7684\u5149\u5b66\u5438\u6536\u8c31\u3002<\/p>\n<p>\uff08e\uff09\u7406\u8bba\u8ba1\u7b97\u5f97\u5230\u7684MAPbI<sub>3<\/sub>\u3001CIS\u3001CZTS\u3001GaAs\u7684\u6700\u5927\u6548\u7387\u968f\u819c\u539a\u7684\u53d8\u5316\u66f2\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe3<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u94c5\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff\u7684\u80fd\u5e26\u7ed3\u6784\uff1a\u4f4e\u8f7d\u6d41\u5b50\u6709\u6548\u8d28\u91cf<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174346 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72479-15.png\" alt=\"\" width=\"600\" height=\"211\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72479-15.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u72479-15-300x106.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09LDA\u8ba1\u7b97\u7684\u7acb\u65b9CsPbI<sub>3<\/sub>\u9499\u949b\u77ff\u7684\u80fd\u5e26\u7ed3\u6784\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08b\uff09GW+SOC\u8ba1\u7b97\u7684MAPbI<sub>3<\/sub>\u7684\u80fd\u5e26\u7ed3\u6784\u793a\u610f\u56fe<\/p>\n<p><strong><b>\u56fe4<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u94c5\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff\u7684\u9ad8\u7f3a\u9677\u5bb9\u5fcd\u6027<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174347 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724710-16.png\" alt=\"\" width=\"600\" height=\"298\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724710-16.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724710-16-300x149.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09\u5728\u94c5\u5364\u5316\u7269\u9499\u949b\u77ff\u4e2dCBM\u548cCBM\u7f3a\u9677\u5f62\u6210\u793a\u610f\u56fe(\u5de6)\uff0c\u9633\u79bb\u5b50\u548c\u9634\u79bb\u5b50\u5f62\u6210\u7684\u65bd\u4e3b\u548c\u53d7\u4e3b\u7f3a\u9677\u793a\u610f\u56fe(\u4e2d)\uff0c\u9633\u79bb\u5b50-\u9633\u79bb\u5b50\u548c\u9634\u79bb\u5b50-\u9634\u79bb\u5b50\u8bef\u6210\u952e\u7684\u7f3a\u9677\u793a\u610f\u56fe(\u53f3)\u3002<\/p>\n<p>\uff08b\uff09MAPbI<sub>3<\/sub>\u4e2d\u70b9\u7f3a\u9677\u7684\u8fc7\u6e21\u80fd\u7ea7\u56fe\u3002<\/p>\n<p>\uff08c\uff09\u5206\u522b\u5728\u5728\u5bccI\/\u8d2bPb(\u5de6), \u4e2d\u6027(\u4e2d)\u548c\u5bccPb\/\u8d2bI\u7684\u5316\u5b66\u6761\u4ef6\u4e0b\u7684MAPbI<sub>3<\/sub>\u7684\u56fa\u6709\u70b9\u7f3a\u9677\u5f62\u6210\u80fd\u3002<\/p>\n<p>\uff08d\uff09\u6df7\u5408\u94c5\u5364\u5316\u7269\u9499\u949b\u77ff\u4e2d\u7684\u5927\u6781\u5316\u5b50\u793a\u610f\u56fe\u3002<\/p>\n<p><strong><b>\u56fe5 \u4f18\u4e8e\u4f20\u7edf\u7ed3\u6784\u7ef4\u5ea6\u7684\u7535\u5b50\u7ef4\u5ea6\u65b0\u6982\u5ff5<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174348 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724711-15.png\" alt=\"\" width=\"600\" height=\"385\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724711-15.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724711-15-300x193.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09\u4e0d\u540c\u7ef4\u5ea6\u9499\u949b\u77ff\u7ed3\u6784\u7684\u6676\u4f53\u7ed3\u6784\u56fe\uff0c\u4ece\u5de6\u81f3\u53f3\u5206\u522b\u4e3a3D\u30012D\u30011D\u548c0D\u3002<\/p>\n<p>\uff08b\uff09\u4e0d\u540c\u7ef4\u5ea6\u9499\u949b\u77ff\u7ed3\u6784\u7684\u80fd\u5e26\u7ed3\u6784\u56fe\u3002<\/p>\n<p>\uff08c\uff09\u4e0d\u540c\u7ef4\u5ea6\u9499\u949b\u77ff\u7ed3\u6784\u7684\u5149\u5b66\u5438\u6536\u5149\u8c31\u3002<\/p>\n<p>\uff08d\uff09\u4e09\u7ef4\u7ed3\u6784\u7684Cs<sub>2<\/sub>PbPbI<sub>6<\/sub>(\u5de6)\u548cCs<sub>2<\/sub>Sr[PbI<sub>6<\/sub>](\u53f3)\u7684\u6676\u4f53\u7ed3\u6784\u56fe\u3002<\/p>\n<p>\uff08e\uff09Cs<sub>2<\/sub>PbPbI<sub>6<\/sub>(\u5de6)\u548cCs<sub>2<\/sub>Sr[PbI<sub>6<\/sub>](\u53f3)\u7684\u80fd\u5e26\u7ed3\u6784\u56fe\u3002<\/p>\n<p>\uff08f\uff09Cs<sub>2<\/sub>PbPbI<sub>6<\/sub>(\u5de6)\u548cCs<sub>2<\/sub>Sr[PbI<sub>6<\/sub>](\u53f3)\u7684(100)\u9762VBM\u548cCBM\u7684\u7535\u8377\u5bc6\u5ea6\u56fe\u3002<\/p>\n<p><strong><b>\u56fe6<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u540c\u4ef7\u66ff\u6362\uff08\u4e00\uff09\uff1a<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Sn<\/b><\/strong><strong><b>(II)<\/b><\/strong><strong><b>\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174350 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724712-14.png\" alt=\"\" width=\"600\" height=\"700\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724712-14.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724712-14-257x300.png 257w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/> <br \/>\n <\/b><\/strong><\/p>\n<p>\uff08a\uff09GW+SOC\u65b9\u6cd5\u8ba1\u7b97\u5f97\u5230\u7684MASnI<sub>3<\/sub>\u7684\u80fd\u5e26\u7ed3\u6784\u56fe\u3002<\/p>\n<p>\uff08b\uff09GW+SOC\u65b9\u6cd5\u8ba1\u7b97\u5f97\u5230\u7684MASnI<sub>3<\/sub>\u548cMAPbI<sub>3<\/sub>\u7684\u6001\u5bc6\u5ea6\u548c\u5149\u5b66\u5438\u6536\u5149\u8c31\u7684\u5bf9\u6bd4\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08c\uff09\u5728\u5bccSn\u548c\u8d2bSn\u6761\u4ef6\u4e0b\u8ba1\u7b97\u5f97\u5230\u7684\u7f3a\u9677\u5f62\u6210\u80fd\u3002<\/p>\n<p>\uff08d\uff09CsSnI<sub>3<\/sub>\u7684\u5404\u79cd\u56fa\u6709\u70b9\u7f3a\u9677\u7684\u8fc7\u6e21\u80fd\u7ea7\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08e\uff09\u7528\u4e0d\u540c\u65b9\u6cd5\u5236\u9020\u7684\u5149\u4f0f\u5668\u4ef6\u7684J-V\u66f2\u7ebf<\/p>\n<p>\uff08f\uff09\u56fa\u5b9a\u8d39\u7c73\u80fd\u7ea7\u4e0b\uff0cSn\u7684\u7a7a\u4f4d\u5f62\u6210\u80fd\u968f\u5316\u5b66\u52bf\u7684\u51fd\u6570\u53d8\u5316\u793a\u610f\u56fe\u3002<\/p>\n<p><strong><b>\u56fe7<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u540c\u4ef7\u66ff\u6362\uff08\u4e8c\uff09\uff1aGe<\/b><\/strong><strong><b>(II)<\/b><\/strong><strong><b>\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174351 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724713-14.png\" alt=\"\" width=\"600\" height=\"299\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724713-14.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724713-14-300x150.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09CsGeI<sub>3<\/sub>\u7684\u6676\u4f53\u7ed3\u6784\u56fe\u3002<\/p>\n<p>\uff08b\uff09MAGeI<sub>3<\/sub>\u7684\u6676\u4f53\u7ed3\u6784\u56fe\u3002<\/p>\n<p>\uff08c\uff09CsGeI<sub>3<\/sub>\u3001MAGeI<sub>3<\/sub>\u3001FAGeI<sub>3<\/sub>\u548cCsSnI<sub>3<\/sub>\u7684\u5149\u5b66\u5438\u6536\u8c31\u5bf9\u6bd4\u56fe\u3002<\/p>\n<p>\uff08d\uff09CsGeI<sub>3<\/sub>\u7684\u80fd\u5e26\u7ed3\u6784\u548c\u6295\u5f71\u6001\u5bc6\u5ea6\u56fe\u3002<\/p>\n<p>\uff08e\uff09CsGeI<sub>3<\/sub>\u3001MAGeI<sub>3<\/sub>\u548cFAGeI<sub>3<\/sub>\u7684\u80fd\u7ea7\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08f\uff09\u7528CsGeI<sub>3<\/sub>\u548cMAGeI<sub>3<\/sub>\u5236\u9020\u7684\u5149\u4f0f\u5668\u4ef6\u7684J-V\u66f2\u7ebf<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>8 <\/b><\/strong><strong><b>\u540c\u4ef7\u66ff\u6362\uff08\u4e09\uff09\uff1a\u8fc7\u6e21\u91d1\u5c5e\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174352 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724714-12.png\" alt=\"\" width=\"600\" height=\"200\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724714-12.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724714-12-300x100.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09MA<sub>2<\/sub>CuCl<sub>2<\/sub>Br<sub>2<\/sub>\u7684\u6676\u4f53\u7ed3\u6784\u56fe\u3002<\/p>\n<p>\uff08b\uff09MA<sub>2<\/sub>CuCl<sub>2<\/sub>Br<sub>2<\/sub>\u7684\u80fd\u5e26\u7ed3\u6784\u56fe\u3002<\/p>\n<p>\uff08c\uff09\u7528MA<sub>2<\/sub>CuCl<sub>2<\/sub>Br<sub>2<\/sub>\u548cMA<sub>2<\/sub>CuCl<sub>0.5<\/sub>Br<sub>3.5<\/sub>\u5236\u9020\u7684\u592a\u9633\u80fd\u7535\u6c60\u7684I-V\u66f2\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe9\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u4e00\uff09\uff1a\u201c\u96f6\u7ef4\u201d\u9499\u949b\u77ff\u884d\u751f\u7269A<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>BX<\/b><\/strong><strong><sub><b>6<\/b><\/sub><\/strong><strong><b>\u7684\u7535\u5b50\u7ed3\u6784<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174353 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724715-11.png\" alt=\"\" width=\"600\" height=\"462\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724715-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724715-11-300x231.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09HSE\u8ba1\u7b97\u7684Cs<sub>2<\/sub>SnI<sub>6<\/sub>\u80fd\u5e26\u7ed3\u6784\u548c\u6001\u5bc6\u5ea6\u3002<\/p>\n<p>\uff08b\uff09HSE\u8ba1\u7b97\u7684Cs<sub>2<\/sub>PdBr<sub>6<\/sub>\u80fd\u5e26\u7ed3\u6784\u548c\u6001\u5bc6\u5ea6\u3002<\/p>\n<p>\uff08c\uff09PBE\u8ba1\u7b97\u7684Cs<sub>2<\/sub>TiBr<sub>6<\/sub>\u80fd\u5e26\u7ed3\u6784\u548cHSE\u8ba1\u7b97\u7684\u6001\u5bc6\u5ea6\u3002<\/p>\n<p>\uff08d\uff09Cs<sub>2<\/sub>SnI<sub>6<\/sub>\u4e2d\u56fa\u6709\u7f3a\u9677\u7684\u8f6c\u53d8\u80fd\u7ea7\u3002<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>0 <\/b><\/strong><strong><b>\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u4e00\uff09\uff1a\u201c\u96f6\u7ef4\u201d\u9499\u949b\u77ff\u884d\u751f\u7269A<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>BX<\/b><\/strong><strong><sub><b>6<\/b><\/sub><\/strong><strong><b>\u7684\u5149\u7535\u6027\u80fd<\/b><\/strong><\/p>\n<p><strong><sub><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174354 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724716-11.png\" alt=\"\" width=\"600\" height=\"291\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724716-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724716-11-300x146.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/sub><\/strong><\/p>\n<p>\uff08a\uff09Cs<sub>2<\/sub>SnI<sub>6<\/sub>\u8584\u819c\u7684\u5438\u6536\u5149\u8c31\u548cPL\u5149\u8c31\u3002<\/p>\n<p>\uff08b\uff09Cs<sub>2<\/sub>PdBr<sub>6<\/sub>\u7c89\u672b\u548c\u8584\u819c\u7684\u5438\u6536\u5149\u8c31\u548cPL\u5149\u8c31\u3002<\/p>\n<p>\uff08c\uff09Cs<sub>2<\/sub>TiBr<sub>6<\/sub>\u8584\u819c\u7684Tauc\u66f2\u7ebf\u548cPL\u5149\u8c31\u3002<\/p>\n<p>\uff08d\uff09\u4e00\u7cfb\u5217\u5177\u6709\u4e0d\u540c\u7ec4\u6210\u7684Cs<sub>2<\/sub>SnI<sub>6-x<\/sub>Br<sub>x<\/sub>\u7684J-V\u7279\u6027\u66f2\u7ebf\u3002<\/p>\n<p>\uff08e\uff09\u57fa\u4e8eCs<sub>2<\/sub>TiBr<sub>6<\/sub>\u7684\u592a\u9633\u80fd\u7535\u6c60\u4e2d\u80fd\u7ea7\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08f\uff09\u6b63\u5411\u548c\u53cd\u5411\u626b\u63cf\u7684\u6709\/\u65e0C<sub>60<\/sub>\u754c\u9762\u5c42\u592a\u9633\u80fd\u7535\u6c60\u7684J-V\u7279\u6027\u66f2\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>1 <\/b><\/strong><strong><b>\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u4e8c\uff09\uff1a\u201c\u96f6\u7ef4\u201d\u9499\u949b\u77ff\u884d\u751f\u7269A<\/b><\/strong><strong><sub><b>3<\/b><\/sub><\/strong><strong><b>B<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>X<\/b><\/strong><strong><sub><b>9<\/b><\/sub><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174362 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724717-10.png\" alt=\"\" width=\"600\" height=\"469\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724717-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724717-10-300x235.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/> \u00a0\u00a0\u00a0\u00a0\u00a0<\/b><\/strong><\/p>\n<p>\uff08a\uff09\u7531\u5206\u79bb\u7684[Bi<sub>2<\/sub>I<sub>9<\/sub>]\u516b\u9762\u4f53\u7ec4\u6210\u7684Cs<sub>3<\/sub>Bi<sub>2<\/sub>I<sub>9<\/sub>\u6676\u4f53\u7ed3\u6784\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08b\uff09Cs<sub>3<\/sub>Bi<sub>2<\/sub>I<sub>9<\/sub>\u80fd\u5e26\u7ed3\u6784\u548c\u6001\u5bc6\u5ea6\u3002<\/p>\n<p>\uff08c\uff09Cs<sub>3<\/sub>Bi<sub>2<\/sub>I<sub>9<\/sub>\u572810K\u65f6\u7684Tauc\u56fe\u3002<\/p>\n<p>\uff08d\uff09\u57fa\u4e8eCs<sub>3<\/sub>Bi<sub>2<\/sub>I<sub>9<\/sub>\u592a\u9633\u80fd\u7535\u6c60\u7684J-V\u66f2\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>2 <\/b><\/strong><strong><b>\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u4e09\uff09\uff1a\u5c42\u72b6\u9499\u949b\u77ffA<\/b><\/strong><strong><sub><b>3<\/b><\/sub><\/strong><strong><b>B<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>X<\/b><\/strong><strong><sub><b>9<\/b><\/sub><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174363 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724718-11.png\" alt=\"\" width=\"600\" height=\"376\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724718-11.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724718-11-300x188.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09\u5c42\u72b6\u9499\u949b\u77ffA<sub>3<\/sub>B<sub>2<\/sub>X<sub>9<\/sub>\u7684\u6676\u4f53\u7ed3\u6784\u3002<\/p>\n<p>\uff08b\uff09\u5c42\u72b6\u548c\u4e8c\u805a\u7269A<sub>3<\/sub>B<sub>2<\/sub>X<sub>9<\/sub>\u7684\u80fd\u5e26\u7ed3\u6784\u3002<\/p>\n<p>\uff08c\uff09\u9633\u79bb\u5b50A\u7684\u5927\u5c0f\u5bf9\u5c42\u72b6A<sub>3<\/sub>B<sub>2<\/sub>X<sub>9<\/sub>\u6676\u4f53\u7ed3\u6784\u5f71\u54cd\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08d\uff09\u4eceA<sub>3<\/sub>Sb<sub>2<\/sub>X<sub>9<\/sub>\u7684\u96f6\u7ef4\u4e8c\u805a\u4f53\u5230A<sub>3<\/sub>Sb<sub>2<\/sub>Cl<sub>x<\/sub>I<sub>9<\/sub><sub>-x<\/sub>\u5c42\u72b6\u76f8\u7684Cl\u52a0\u6210\u8bf1\u5bfc\u8f6c\u5316\u793a\u610f\u56fe\u3002<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>3 <\/b><\/strong><strong><b>\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u56db\uff09\uff1a\u6df7\u5408\u9634\u79bb\u5b50\u4e09\u7ef4\u9499\u949b\u77ffABX(<\/b><\/strong><strong><b>Ch,X)<\/b><\/strong><strong><sub><b>3<\/b><\/sub><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174364 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724719-10.png\" alt=\"\" width=\"600\" height=\"628\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724719-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724719-10-287x300.png 287w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09\u9634\u79bb\u5b50\u6df7\u5408\u65b9\u6cd5\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08b\uff09MAPbI<sub>3<\/sub>\u548cMABiSI<sub>2<\/sub>\u7684\u80fd\u5e26\u7ed3\u6784\u3002<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>4 <\/b><\/strong><strong><b>\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u56db\uff09\uff1a\u53cc\u9499\u949b\u77ffA<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>B(<\/b><\/strong><strong><b>I)<\/b><\/strong><strong><b>B<\/b><\/strong><strong><b>(I<\/b><\/strong><strong><b>I<\/b><\/strong><strong><b>I)X<\/b><\/strong><strong><sub><b>6<\/b><\/sub><\/strong><strong><b>\uff081\uff09<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174365 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724720-10.png\" alt=\"\" width=\"600\" height=\"479\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724720-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724720-10-300x240.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u80fd\u591f\u5f62\u6210\u53cc\u9499\u949b\u77ff\u7ed3\u6784\u7684\u5143\u7d20\u548c\u6676\u4f53\u4e2d\u53ef\u80fd\u7684\u4f4d\u7f6e\u793a\u610f\u56fe<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>5<\/b><\/strong><strong><b>\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u56db\uff09\uff1a\u53cc\u9499\u949b\u77ffA<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>B(<\/b><\/strong><strong><b>I)<\/b><\/strong><strong><b>B<\/b><\/strong><strong><b>(I<\/b><\/strong><strong><b>I<\/b><\/strong><strong><b>I)X<\/b><\/strong><strong><sub><b>6<\/b><\/sub><\/strong><strong><b>\uff08<\/b><\/strong><strong><b>2<\/b><\/strong><strong><b>\uff09<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174366 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724721-10.png\" alt=\"\" width=\"600\" height=\"345\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724721-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724721-10-300x173.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09Cs<sub>2<\/sub>AgBiBr<sub>6<\/sub>\u7c89\u672b\u7684\u5438\u6536\u5149\u8c31\u548c\u95f4\u63a5\u5e26\u9699\u578bTauc\u56fe\u3002<\/p>\n<p>\uff08b\uff09Cs<sub>2<\/sub>AgBiBr<sub>6<\/sub>\u7684\u80fd\u5e26\u7ed3\u6784\u3002<\/p>\n<p>\uff08c\uff09Cs<sub>2<\/sub>AgBiBr<sub>6<\/sub>\u7c89\u672b\u548c\u5355\u6676\u6837\u54c1\u5728\u5ba4\u6e29\u4e0b\u7684\u65f6\u95f4\u5206\u8fa8PL\u8c31\u3002<\/p>\n<p>\uff08d\uff09\u57fa\u4e8eCs<sub>2<\/sub>AgBiBr<sub>6<\/sub>\u53cc\u9499\u949b\u77ff\u7684\u592a\u9633\u80fd\u7535\u6c60\u7684J-V\u66f2\u7ebf\u3002<\/p>\n<p>\uff08e\uff09Cs<sub>2<\/sub>AgBiBr<sub>6<\/sub>\u7eb3\u7c73\u6676\u4f53\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08f\uff09Cs<sub>2<\/sub>AgBiX<sub>6<\/sub>\u7eb3\u7c73\u6676\u4f53\u7684\u5438\u6536\u5149\u8c31\u3002<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>6<\/b><\/strong><strong><b>\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u56db\uff09\uff1a\u53cc\u9499\u949b\u77ffA<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>B(<\/b><\/strong><strong><b>I)<\/b><\/strong><strong><b>B<\/b><\/strong><strong><b>(I<\/b><\/strong><strong><b>I<\/b><\/strong><strong><b>I)X<\/b><\/strong><strong><sub><b>6<\/b><\/sub><\/strong><strong><b>\uff08<\/b><\/strong><strong><b>3<\/b><\/strong><strong><b>\uff09<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174367 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724722-10.png\" alt=\"\" width=\"600\" height=\"322\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724722-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724722-10-300x161.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09Cs<sub>2<\/sub>AgInCl<sub>6<\/sub>\u7684\u80fd\u5e26\u7ed3\u6784\u3002<\/p>\n<p>\uff08b\uff09\u5728Cs<sub>2<\/sub>AgInCl<sub>6<\/sub>\u7684CBM\u548cVBM\u5904\u7684\u7535\u5b50\u6ce2\u51fd\u6570\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08c\uff09Cs<sub>2<\/sub>AgInCl<sub>6<\/sub>\u7684\u5355\u6676\u5438\u6536\u5149\u8c31\u548cTauc\u56fe\u3002<\/p>\n<p>\uff08d\uff09Cs<sub>2<\/sub>AgInCl<sub>6<\/sub>\u5728350-800nm\u8303\u56f4\u5185\u7684PL\u5149\u8c31\u3002<\/p>\n<p>\uff08e\uff09Cs<sub>2<\/sub>(Ag<sub>1<\/sub><sub>-a<\/sub>Bi<sub>1<\/sub><sub>-b<\/sub>)Tl<sub>x<\/sub>Br<sub>6<\/sub>\u7684\u5438\u6536\u5149\u8c31<\/p>\n<p>\uff08f\uff09Cs<sub>2<\/sub>(Ag<sub>1<\/sub><sub>-a<\/sub>Bi<sub>1<\/sub><sub>-b<\/sub>)Tl<sub>x<\/sub>Br<sub>6<\/sub>\u5728x=0.06\u65f6\u7684\u80fd\u5e26\u7ed3\u6784\u3002<\/p>\n<p>\uff08g\uff09Cs<sub>2<\/sub>Ag(Bi<sub>1-x<\/sub>Sb<sub>x<\/sub>)Br<sub>6<\/sub>\u7684\u95f4\u63a5Tauc\u56fe\u3002<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>7<\/b><\/strong><strong><b>\u5f02<\/b><\/strong><strong><b>\u4ef7\u66ff\u6362<\/b><\/strong><strong><b>\uff08\u56db\uff09\uff1a\u53cc\u9499\u949b\u77ffA<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>B(<\/b><\/strong><strong><b>I)<\/b><\/strong><strong><b>B<\/b><\/strong><strong><b>(I<\/b><\/strong><strong><b>I<\/b><\/strong><strong><b>I)X<\/b><\/strong><strong><sub><b>6<\/b><\/sub><\/strong><strong><b>\uff08<\/b><\/strong><strong><b>4<\/b><\/strong><strong><b>\uff09<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-174368 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724723-10.png\" alt=\"\" width=\"600\" height=\"405\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724723-10.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/04\/\u56fe\u724723-10-300x203.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\uff08a\uff09Cs<sub>2<\/sub>PbPbBr<sub>6<\/sub>(\u5de6)\u3001Cs<sub>2<\/sub>TlBiBr<sub>6<\/sub>(\u4e2d)\u548cFr<sub>2<\/sub>TlBiBr<sub>6<\/sub>(\u53f3)\u7684\u80fd\u5e26\u7ed3\u6784\u3002<\/p>\n<p>\uff08b\uff09A<sub>2<\/sub>B(I)B(III)X<sub>6<\/sub>\u00a0(B(I)=Tl, In; B(III)= Bi, Sb)\u7684CBM(\u7ea2\u8272)\u548cVBM(\u84dd\u8272)\u5904\u7684\u5178\u578b\u7535\u5b50\u6ce2\u51fd\u6570\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08c\uff09\u8ba1\u7b97\u5f97\u5230\u7684\u6240\u9009\u53cc\u9499\u949b\u77ff\u7ed3\u6784\u7684\u5438\u6536\u5149\u8c31\u3002<\/p>\n<p>\uff08d\uff09Cs<sub>2<\/sub>InBiX<sub>6<\/sub>(X = I, Br, Cl)\u6cbf\u4e09\u79cd\u5178\u578b\u5206\u89e3\u8def\u5f84\u7684\u5206\u89e3\u7113(\u0394Hd)<\/p>\n<p>\uff08e\uff09Cs<sub>2<\/sub>TlBiBr<sub>6<\/sub>(\u5de6)\u548cFr<sub>2<\/sub>TlBiBr<sub>6<\/sub>(\u53f3)\u7684\u65e0\u7f3a\u9677\uff0cB(I)<sub>B(III)<\/sub>\u53cd\u4f4d\u548cB(III)<sub>B(I)<\/sub>\u53cd\u4f4d\u7f3a\u9677\u65f6\u7684\u80fd\u5e26\u7ed3\u6784\u3002<\/p>\n<p>&nbsp;<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong>From Lead Halide Perovskites to Lead\u2010Free Metal Halide Perovskites and Perovskite Derivatives. Advanced Materials, 2019: 1803792.<\/p>\n<p><a href=\"https:\/\/doi.org\/10.1002\/adma.201803792\"><strong><u><b>https:\/\/doi.org\/10.1002\/adma.201803792<\/b><\/u><\/strong><\/a><\/p>\n<p><strong><b>\u8096\u6cfd\u6587\u6559\u6388\u7b80\u4ecb\u53ca\u535a\u58eb\u540e\u62db\u8058\u4fe1\u606f\uff1a<\/b><\/strong><\/p>\n<p>\u8096\u6cfd\u6587\uff0c\u535a\u58eb\uff0c\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u6b66\u6c49\u5149\u7535\u56fd\u5bb6\u7814\u7a76\u4e2d\u5fc3\u6559\u6388\uff0c\u535a\u58eb\u751f\u5bfc\u5e08\u3002\u672c\u7855\u6bd5\u4e1a\u4e8e\u897f\u5b89\u4ea4\u901a\u5927\u5b66\uff082006-2012\uff09\u3001\u535a\u58eb\u6bd5\u4e1a\u4e8e\u65e5\u672c\u4e1c\u4eac\u5de5\u4e1a\u5927\u5b66\uff082012-2015\uff09\uff08\u5e08\u4eceHideo\u00a0Hosono\u6559\u6388\u548cToshio\u00a0Kamiya\u6559\u6388\uff09\u3002\u5728\u7f8e\u56fd\u6258\u83b1\u591a\u5927\u5b66\uff08\u5408\u4f5c\u5bfc\u5e08\u9122\u708e\u53d1\u6559\u6388\uff09\u4ece\u4e8b\u4e00\u5e74\u535a\u58eb\u540e\u7814\u7a76\u5de5\u4f5c\u540e\uff0c\u53d7\u8058\u4e8e\u65e5\u672c\u4e1c\u4eac\u5de5\u4e1a\u5927\u5b66\uff0c\u62c5\u4efb\u52a9\u7406\u6559\u6388\u3002\u8096\u6cfd\u6587\u535a\u58eb\u4e8e2018\u5e749\u6708\u56de\u56fd\u5de5\u4f5c\uff0c\u5176\u8bfe\u9898\u7ec4\u4e3b\u8981\u4ece\u4e8b\u65b0\u578b\u534a\u5bfc\u4f53\u5149\u7535\u6750\u6599\u7406\u6027\u8bbe\u8ba1\u3001\u5408\u6210\u548c\u5149\u7535\u6027\u80fd\u7814\u7a76\uff0c\u5728\u7406\u8bba\u8ba1\u7b97\u4e0e\u5b9e\u9a8c\u7684\u7ed3\u5408\u65b9\u9762\u5177\u6709\u4e30\u5bcc\u548c\u72ec\u7279\u7684\u7ecf\u9a8c\uff08\u201c\u7406\u8bba+\u5b9e\u9a8c\u201d\u4e5f\u662f\u5927\u52bf\u6240\u8d8b\uff01\uff09\u3002\u56de\u56fd\u524d\uff0c\u8096\u6cfd\u6587\u535a\u58eb\u4ee5\u7b2c\u4e00\u4f5c\u8005\u6216\u901a\u8baf\u4f5c\u8005\u5728Joule\u3001Adv. Mater.\u3001Adv. Energy Mater.\u3001J. Am. Chem. Soc.\u3001Adv. Funct. Mater.\u3001Angew. Chem. Int. Ed.\u3001Mater. Horiz.\u3001ACS Energy Lett.\u7b49\u56fd\u9645\u77e5\u540d\u671f\u520a\u4e0a\u53d1\u8868SCI\u8bba\u658730\u7bc7\u3002\u56de\u56fd\u540e\uff0c\u5176\u8bfe\u9898\u7ec4\u7684\u7814\u7a76\u5de5\u4f5c\u5df2\u5f00\u59cb\u5728Adv. Mater.\u3001ACS Energy Lett.\u7b49\u671f\u520a\u53d1\u8868\uff0c\u6216\u6b63\u6295\u7a3f\u4e8eNature\u5b50\u520a\uff08\u4fee\u6539\uff09\u7b49\u3002\u8096\u6cfd\u6587\u6559\u6388\u8bfe\u9898\u7ec4\u62df\u5728\u9002\u5ea6\u5730\u8ffd\u8e2a\u70ed\u70b9\uff08\u7edd\u4e0d\u6c89\u6eba\uff09\u4ee5\u786e\u4fdd\u201c\u751f\u5b58\u201d\u7684\u57fa\u7840\u4e0a\uff0c\u5c06\u96c6\u4e2d\u7cbe\u529b\u8fdb\u884c\u5177\u6709\u9ad8\u5ea6\u539f\u521b\u6027\u7684\u7814\u7a76\u3002\u76ee\u524d\u56e0\u8bfe\u9898\u7ec4\u53d1\u5c55\u9700\u8981\u62df\u62db\u8058\u4ece\u4e8b\u6750\u6599\u76f8\u5173\u7684\u7406\u8bba\u8ba1\u7b97\u6216\u5b9e\u9a8c\u7814\u7a76\u7684\u535a\u58eb\u540e\uff08\u6750\u6599\u3001\u7269\u7406\u3001\u5316\u5b66\u3001\u5149\u7535\u7b49\u4e13\u4e1a\u80cc\u666f\uff092-3\u540d\u3002<\/p>\n<p>\u8be6\u7ec6\u4fe1\u606f\u8bf7\u89c1\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u535a\u58eb\u540e\u6d41\u52a8\u7ad9\u7f51\u9875\uff1a<a href=\"http:\/\/postdoctor.hust.edu.cn\/info\/1007\/1801.htm\"><u>http:\/\/postdoctor.hust.edu.cn\/info\/1007\/1801.htm<\/u><\/a><\/p>\n<p>\u672c\u6587\u7531<strong><b>\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u6b66\u6c49\u5149\u7535\u56fd\u5bb6\u7814\u7a76\u4e2d\u5fc3\u8096\u6cfd\u6587(<\/b><\/strong><strong><b>Zewen Xiao)<\/b><\/strong><strong><b>\u6559\u6388\u56e2\u961f<\/b><\/strong><strong><b>\u4f9b\u7a3f<\/b><\/strong>\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u94c5\u57fa\u5364\u5316\u7269\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u56e0\u5176\u4f18\u5f02\u7684\u5149\u7535\u6027\u80fd\u548c\u4f4e\u5236\u4f5c\u6210\u672c\uff08\u4f4e\u95e8\u69db\uff09\u800c\u6210\u4e3a\u5f53\u4eca\u7814\u7a76\u70ed\u70b9\u3002\u7136\u800c\uff0c\u5176\u6b20\u4f73\u7684\u7a33\u5b9a\u6027\u548c\u94c5\u7684\u6bd2\u6027\uff0c\u4f7f\u5176\u5546\u4e1a\u5316\u9762\u4e34\u6311\u6218\u3002\u56e0\u6b64\uff0c\u5bfb\u627e\u65e0&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[533],"tags":[],"class_list":["post-174339","post","type-post","status-publish","format-standard","hentry","category-zongshu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/174339"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=174339"}],"version-history":[{"count":8,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/174339\/revisions"}],"predecessor-version":[{"id":174374,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/174339\/revisions\/174374"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=174339"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=174339"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=174339"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}