{"id":176374,"date":"2019-06-04T16:46:53","date_gmt":"2019-06-04T08:46:53","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=176374"},"modified":"2019-06-26T16:00:22","modified_gmt":"2019-06-26T08:00:22","slug":"adv-funct-mater-%ef%bc%9a%e9%80%9a%e8%bf%87%e5%8d%8f%e5%90%8c%e7%a3%b7%e5%8c%96%e5%92%8c%e7%83%ad%e8%a7%a3%e5%b0%86rhpx%e5%b5%8c%e5%85%a5n%ef%bc%8cp%e5%85%b1%e6%8e%ba%e6%9d%82%e7%a2%b3%e7%ba%b3","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=176374","title":{"rendered":"Adv. Funct. Mater.\uff1a\u901a\u8fc7\u534f\u540c\u78f7\u5316\u548c\u70ed\u89e3\u5c06RhPx\u5d4c\u5165N\uff0cP\u5171\u63ba\u6742\u78b3\u7eb3\u7c73\u58f3\u4e2d\uff0c\u5b9e\u73b0\u9ad8\u6548\u6790\u6c22\u53cd\u5e94"},"content":{"rendered":"<p><b><\/b><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u867d\u7136\u7535\u5316\u5b66\u6c34\u5206\u89e3\u88ab\u8ba4\u4e3a\u662f\u4e00\u79cd\u73af\u4fdd\u3001\u9ad8\u6548\u7684\u65e0\u6c61\u67d3\u5236\u6c22\u9014\u5f84\uff0c\u4f46\u4ecd\u9700\u8981\u4e00\u79cd\u9ad8\u6548\u7684\u6790\u6c22\u53cd\u5e94\uff08HER\uff09\u7535\u50ac\u5316\u5242\u3002\u76ee\u524d\uff0cPt\u57fa\u6750\u6599\u88ab\u8ba4\u4e3a\u662f\u6700\u5148\u8fdb\u7684\u7535\u50ac\u5316\u5242\uff0c\u5c24\u5176\u662f\u5728\u9178\u6027\u7535\u89e3\u8d28\u4e2d\u3002\u7136\u800c\uff0cPt\u57fa\u50ac\u5316\u5242\u5728\u78b1\u6027\u548c\u4e2d\u6027\u7535\u89e3\u8d28\u4e2d\u5747\u8868\u73b0\u51fa\u8f83\u6162\u7684\u52a8\u529b\u5b66\u3002\u56e0\u6b64\uff0c\u5f00\u53d1\u9002\u7528\u5bbdpH\u8303\u56f4\u7684\u7535\u50ac\u5316\u5242\u4ecd\u7136\u662f\u4e00\u9879\u7d27\u8feb\u800c\u8270\u5de8\u7684\u4efb\u52a1\u3002\u5c06\u50ac\u5316\u5242\u7eb3\u7c73\u7c92\u5b50\uff08NPs\uff09\u5305\u8986\u5728\u78b3\u5c42\u4e2d\u662f\u63d0\u9ad8\u5176\u5728\u4e0d\u540c\u7535\u89e3\u8d28\u4e2d\u7a33\u5b9a\u6027\u7684\u6709\u6548\u7b56\u7565\u3002\u7eb3\u7c73\u7ed3\u6784\u78b3\u8f7d\u4f53\u7684\u53ef\u63a7\u5408\u6210\u662f\u5f00\u53d1\u9ad8\u6548\u7535\u50ac\u5316\u5242\u7684\u57fa\u7840\u3002\u4f18\u5316\u78b3\u8f7d\u4f53\u4ee5\u83b7\u5f97\u9ad8\u6bd4\u8868\u9762\u79ef\u548c\u4e30\u5bcc\u7684\u4ecb\u5b54\u7387\uff0c\u5bf9\u4e8e\u66b4\u9732\u66f4\u591a\u7684\u50ac\u5316\u4f4d\u70b9\u662f\u81f3\u5173\u91cd\u8981\u7684\u3002\u805a\u82ef\u80fa\u3001\u5421\u54af\u7b49\u805a\u5408\u7269\u57fa\u4f53\u5177\u6709\u826f\u597d\u7684\u5bfc\u7535\u6027\u548c\u8f83\u9ad8\u7684\u542b\u6c2e\u91cf\uff0c\u88ab\u8ba4\u4e3a\u662f\u50ac\u5316\u5242\u8f7d\u4f53\u7684\u4f18\u826f\u524d\u9a71\u4f53\u3002\u7136\u800c\uff0c\u8fd9\u79cd\u8f7d\u4f53\u7684\u8868\u9762\u79ef\u548c\u5b54\u9699\u7387\u4ecd\u7136\u4e0d\u7406\u60f3\uff0c\u7ed3\u6784\u5f80\u5f80\u662f\u4e0d\u53ef\u63a7\u5236\u7684\uff0c\u8fd9\u9650\u5236\u4e86\u5b83\u4eec\u7684\u5e94\u7528\u3002\u636e\u62a5\u9053\uff0c\u901a\u8fc7\u78f7\u5316\u8fc7\u7a0b\u5c06\u78f7\u6c27\u5316\u7269\u78b3\u70ed\u8fd8\u539f\u4e3aP\uff0c\u5728\u78b3\u57fa\u8d28\u4e2d\u5f62\u6210\u7a7a\u9699\u3002\u56e0\u6b64\uff0cP\u7684\u5f15\u5165\u6709\u671b\u5b9e\u73b0\u53ef\u63a7\u7684\u4ecb\u5b54\u7ed3\u6784\uff0c\u5e76\u6709\u53ef\u80fd\u63d0\u9ad8\u5176\u50ac\u5316\u4f4d\u70b9\u7684\u5229\u7528\u7387\u3002\u53e6\u4e00\u65b9\u9762\uff0c\u91d1\u5c5e\u78f7\u5316\u7269\uff08MPs\uff09\u4f5c\u4e3a\u586b\u9699\u5f0f\u5408\u91d1\u88ab\u8ba4\u4e3a\u662f\u52a0\u6c22\u8131\u786b\uff08HDS\uff09\u53cd\u5e94\u7684\u6709\u6548\u50ac\u5316\u5242\u3002\u9274\u4e8eHDS\u53cd\u5e94\u548cHER\u90fd\u4f9d\u8d56\u4e8e\u6c22\u7684\u53ef\u9006\u7ed3\u5408\u548c\u89e3\u79bb\uff0c\u91d1\u5c5e\u78f7\u5316\u7269\u4f5c\u4e3a\u50ac\u5316\u5242\u503c\u5f97\u7814\u7a76\uff0c\u6700\u8fd1\u7684\u4e00\u4e9b\u7814\u7a76\u7ed3\u679c\u652f\u6301\u4e86\u8fd9\u4e00\u89c2\u70b9\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u5728<strong><b>\u4e2d\u56fd\u77f3\u6cb9\u5927\u5b66\uff08\u534e\u4e1c\uff09<\/b><\/strong><strong><b>\u8463\u658c<\/b><\/strong><strong><b>\u526f<\/b><\/strong><strong><b>\u6559\u6388<\/b><\/strong>\u548c<strong><b>\u52a0\u5dde\u5927\u5b66\u6cb3\u6ee8\u5206\u6821<\/b><\/strong><strong><b>\u6bb7\u4e9a\u4e1c<\/b><\/strong><strong><b>\u6559\u6388<\/b><\/strong><strong><b>\u56e2\u961f\uff08<\/b><\/strong><strong><b>\u5171\u540c<\/b><\/strong><strong><b>\u901a\u8baf\u4f5c\u8005\uff09<\/b><\/strong>\u5e26\u9886\u4e0b\uff0c\u4e0e<strong><b>\u5317\u4eac\u822a\u7a7a\u822a\u5929<\/b><\/strong><strong><b>\u5927\u5b66<\/b><\/strong>\u5408\u4f5c\uff0c\u62a5\u544a\u4e86\u4e00\u79cd\u6709\u673a-\u65e0\u673a\u70ed\u89e3\u7b56\u7565\uff0c\u4ee5\u5b9e\u73b0\u7531\u8d85\u8584\u78b3\u5c42\u5305\u88f9\u7684\u9ad8\u5ea6\u5206\u6563\u7684RhP<sub>x<\/sub>\u00a0NPs\u3002\u8be5\u7b56\u7565\u7684\u8bbe\u8ba1\u5229\u7528\u4e86\u7a7a\u95f4\u9650\u5236\u7684\u78f7\u5316\u8fc7\u7a0b\uff0c\u5f53\u5728\u70ed\u89e3\u6761\u4ef6\u4e0b\u5728\u542bRh\/P\u7684\u805a\u5408\u7269\u524d\u4f53\u4e2d\u53d1\u751f\u65f6\uff0c\u8bf1\u5bfc\u5f62\u6210\u542b\u6709\u826f\u597d\u5206\u6563\u7684\u8d85\u7ec6RhP<sub>x<\/sub>\u7eb3\u7c73\u9897\u7c92\u7684\u8d85\u8584\u78b3\u7eb3\u7c73\u58f3\u3002\u78b3\u7eb3\u7c73\u58f3\u662f\u826f\u597d\u7684\u50ac\u5316\u5242\u8f7d\u4f53\uff0c\u5177\u6709\u9ad8\u8868\u9762\u79ef\u3001\u4e30\u5bcc\u7684\u4e2d\u5b54\u6027\u548c\u53ef\u63a7\u7684N\uff0cP\u5171\u63ba\u6742\u3002\u5f97\u76ca\u4e8e\u5206\u6563\u826f\u597d\u7684\u8d85\u7ec6RhP<sub>x<\/sub>\u00a0NPs\uff0c\u5f3a\u50ac\u5316\u5242-\u8f7d\u4f53\u76f8\u4e92\u4f5c\u7528\u3001\u9ad8\u8868\u9762\u79ef\u548c\u6742\u539f\u5b50\u63ba\u6742\u7684\u78b3\u8f7d\u4f53\uff0c\u5236\u5907\u7684RhP<sub>x<\/sub>@NPC\u7eb3\u7c73\u58f3\u5728\u9178\u6027\u3001\u78b1\u6027\u548c\u4e2d\u6027\u6761\u4ef6\u4e0b\u8868\u73b0\u51fa\u4e0ePt\u76f8\u5f53\u7684HER\u50ac\u5316\u6d3b\u6027\uff0c\u4ee5\u53ca\u4f4e\u8fc7\u7535\u4f4d\u548c\u957f\u671f\u8010\u4e45\u6027\u3002\u76f8\u5173\u6210\u679c\u4ee5\u9898\u4e3a<strong><b>\u201c<\/b><\/strong><strong><b>Embedding RhP<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>\u00a0in N, P Co-Doped Carbon Nanoshells Through Synergetic Phosphorization and Pyrolysis for Efficient Hydrogen Evolution<\/b><\/strong><strong><b>\u201d<\/b><\/strong>\u53d1\u8868\u5728\u4e86<strong><b>Adv. Funct. Mater.<\/b><\/strong>\u4e0a\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>RhP<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>@NPC\u7eb3\u7c73\u58f3\u5408\u6210\u65b9\u6cd5\u7684\u793a\u610f\u56fe<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-176376\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/1-16.jpg\" alt=\"\" width=\"600\" height=\"204\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/1-16.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/1-16-300x102.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe2<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>TEM\u56fe\u50cf<\/b><\/strong><strong><b>\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-176377\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/2-13.jpg\" alt=\"\" width=\"600\" height=\"343\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/2-13.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/2-13-300x172.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a-d\uff09a\uff09NC\uff0cb\uff09NPC\uff0cc\uff09Rh@ NC\u548cd\uff09RhP<sub>x<\/sub>@NPC\u7eb3\u7c73\u58f3\u7684TEM\u56fe\u50cf\u3002<\/p>\n<p>e,f\uff09\u5206\u522b\u901a\u8fc7\u6539\u53d8e\uff09NaH<sub>2<\/sub>PO<sub>2<\/sub>\u00b7H<sub>2<\/sub>O\u91cf\u548cf\uff09\u78f7\u5316\u65f6\u95f4\u6765\u8ba1\u7b97TEM\u56fe\u50cf\u4e2d\u7684\u7c92\u5ea6\u76f8\u5e94\u7684\u5916\u5f84\u548c\u5185\u5f84\u5206\u5e03\u56fe\u3002<\/p>\n<p><strong><b>\u56fe3<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>RhP<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>@NPC\u7eb3\u7c73\u58f3<\/b><\/strong><strong><b>\u7684\u7269\u7406\u6027\u80fd\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-176378\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/3-13.jpg\" alt=\"\" width=\"600\" height=\"351\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/3-13.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/3-13-300x176.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a-f\uff09RhP<sub>x<\/sub>@NPC\u7eb3\u7c73\u58f3\u7684a\uff09SEM\uff0cb,c\uff09TEM\uff0cd\uff09HRTEM\uff0ce\uff09\u5143\u7d20\u5206\u5e03\u56fe\u50cf\uff0cf\uff09N<sub>2<\/sub>\u5438\u9644-\u89e3\u5438\u7b49\u6e29\u7ebf\u548c\u5b54\u5f84\u5206\u5e03\u56fe\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4 <\/b><\/strong><strong><b>RhP<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>@NPC\u7eb3\u7c73\u58f3<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>XRD<\/b><\/strong><strong><b>\u548c<\/b><\/strong><strong><b>XPS\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-176379\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/4-12.jpg\" alt=\"\" width=\"600\" height=\"718\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/4-12.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/4-12-251x300.jpg 251w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a\uff09RhP<sub>x<\/sub>@NPC\u7684XRD\u56fe\u8c31\u3002<\/p>\n<p>b\uff09Rh@NC\u548cRhP<sub>x<\/sub>@NPC\u7684Rh 3d XPS\u5149\u8c31\u3002<\/p>\n<p>c\uff09NPC\u548cRhP<sub>x<\/sub>@NPC\u7684P 2p XPS\u5149\u8c31\u3002<\/p>\n<p>d,e\uff09RhP<sub>x<\/sub>@NPC\u7684C 1s\u548cN 1s XPS\u5149\u8c31\u3002<\/p>\n<p>f\uff09RhP<sub>x<\/sub>@NPC\u7684\u62c9\u66fc\u5149\u8c31\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>5<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u7145\u70e7<\/b><\/strong><strong><b>\u540e\u7684<\/b><\/strong><strong><b>RhP<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>@NPC<\/b><\/strong><strong><b>\u7684\u7269\u7406\u6027\u80fd\u8868\u5f81<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-176385\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/5-9.jpg\" alt=\"\" width=\"600\" height=\"526\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/5-9.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/5-9-300x263.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a-c\uff09800\u2103\u4e0b\u7145\u70e7\u7684RhP<sub>x<\/sub>@NPC\u7684a\uff09SEM\uff0cb\uff09TEM\u548cc\uff09\u7684HRTEM\u56fe\u50cf\u3002<\/p>\n<p>d-f\uff091000\u2103\u4e0b\u7145\u70e7\u7684RhP<sub>x<\/sub>@NPC\u7684d\uff09SEM\uff0ce\uff09TEM\u548cf\uff09\u7684HRTEM\u56fe\u50cf\u3002<\/p>\n<p>g-i\uff09\u5206\u522b\u5728800\u3001900 \u548c1000\u2103\u4e0b\u7145\u70e7\u7684RhP<sub>x<\/sub>@NPC\u7684g\uff09XRD\u56fe\uff0ch\uff09\u62c9\u66fc\u5149\u8c31\uff0ci\uff09N<sub>2<\/sub>\u5438\u9644-\u89e3\u5438\u7b49\u6e29\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>6<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>RhP<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>@NPC<\/b><\/strong><strong><b>\u5728\u9178\u6027\u7535\u89e3\u6db2\u4e2d\u7684\u6781\u5316\u66f2\u7ebf<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-176384\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/6-5.jpg\" alt=\"\" width=\"600\" height=\"677\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/6-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/6-5-266x300.jpg 266w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a\uff09\u88f8GCE\uff0cNC\uff0cNPC\uff0cRh@NC\uff0cRhP<sub>x<\/sub>\u00a0NPs\uff0cRhP<sub>x<\/sub>@NPC\u548cPt\/C\u7535\u6781\u57280.5\u00a0M\u00a0H<sub>2<\/sub>SO<sub>4<\/sub>\uff0c\u626b\u63cf\u901f\u7387\u4e3a5mV s<sup>-1<\/sup>\u7684\u6781\u5316\u66f2\u7ebf\u3002<\/p>\n<p>b\uff09\u5bf9\u5e94\u7684Tafel\u56fe\u3002<\/p>\n<p>c\uff09\u4e0d\u540c\u626b\u63cf\u901f\u7387\u4e0bRhP<sub>x<\/sub>@NPC\u53cc\u5c42\u7535\u5bb9\u6d4b\u91cf\u7684CV\u626b\u63cf\u3002<\/p>\n<p>d,e\uff09\u6240\u6709\u6837\u54c1\u7684d\uff09\u53cc\u5c42\u7535\u5bb9\u548ce\uff09\u5948\u594e\u65af\u7279\u56fe\u3002<\/p>\n<p>f\uff09\u57281000\u4e2aCV\u5faa\u73af\u524d\u540eRhP<sub>x<\/sub>@NPC\u5728-0.2~0.1V\uff08vs RHE\uff09\u7684\u6781\u5316\u66f2\u7ebf\u3002\u63d2\u56fe\uff1a\u572825 mV\u7684\u56fa\u5b9a\u8fc7\u7535\u4f4d\u4e0b\u6d4b\u8bd510\u5c0f\u65f6\u7684\u8ba1\u65f6\u5b89\u57f9\u66f2\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>7<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>RhP<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>@NPC<\/b><\/strong><strong><b>\u5728\u78b1\u6027\u7535\u89e3\u6db2\u7684\u6781\u5316\u66f2\u7ebf<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-176381\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/7-2.jpg\" alt=\"\" width=\"600\" height=\"301\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/7-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/7-2-300x151.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a,d\uff09\u88f8GCE\u3001NC\u3001NPC\u3001Rh@NC\u3001RhP<sub>x<\/sub>\u00a0NPs\u3001RhP<sub>x<\/sub>@NPC\u548cPt\/C\u7535\u6781\u57281.0 M\u00a0KOH\u548c1.0 M\u00a0PBS\u4e2d\u626b\u63cf\u901f\u7387\u4e3a5 mV s<sup>\u22121<\/sup>\u65f6\u7684\u6781\u5316\u66f2\u7ebf\u3002<\/p>\n<p>b,e\uff09\u5bf9\u5e94\u7684\u5854\u83f2\u5c14\u56fe\u3002<\/p>\n<p>c,f\uff091000\u4e2aCV \u5faa\u73af\u524d\u540eRhP<sub>x<\/sub>@NPC\u5728-0.2~0.1V\uff08vs RHE\uff09\u7684\u6781\u5316\u66f2\u7ebf\u3002\u63d2\u56fe\uff1a\u5206\u522b\u57281.0 M\u00a0KOH\u548c1.0 M\u00a0PBS\u4e2d\uff0c\u9759\u6001\u8fc7\u7535\u4f4d\u4e3a80 mV\u548c40 mV\u65f6\u7684\u8ba1\u65f6\u7535\u6d41\u6cd5\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>8<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>RhP<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>@NPC<\/b><\/strong><strong><b>\u5728\u4e0d\u540c\u7684\u7535\u89e3\u6db2\u7684\u6781\u5316\u66f2\u7ebf<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-176382\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/8-2.jpg\" alt=\"\" width=\"600\" height=\"670\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/8-2.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/05\/8-2-269x300.jpg 269w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>a-f\uff09\u5206\u522b\u5728\u4e0d\u540c\u7535\u89e3\u8d28\u4e2d\u5728800\u3001900\u548c1000\u2103\u4e0b\u7145\u70e7\u7684RhP<sub>x<\/sub>@NPC\u7684a,c,e\uff09\u6781\u5316\u66f2\u7ebf\u548cb,d,f\uff09\u7684\u5854\u83f2\u5c14\u56fe\u3002<\/p>\n<p>\u3010<strong><b>\u5c0f\u7ed3<\/b><\/strong>\u3011<\/p>\n<p>\u603b\u4e4b\uff0c\u56e2\u961f\u5df2\u7ecf\u5f00\u53d1\u51fa\u4e00\u79cd\u534f\u540c\u70ed\u89e3\u548c\u78f7\u5316\u7b56\u7565\uff0c\u5c06RhPx\u5d4c\u5165N\uff0cP\u5171\u63ba\u6742\u78b3\u7eb3\u7c73\u58f3\u4e2d\uff0c\u4ee5\u5b9e\u73b0\u9ad8\u6548\u7684\u901a\u7528pH\u6790\u6c22\u3002\u78f7\u5316\u8fc7\u7a0b\u8bf1\u5bfc\u78b3\u7eb3\u7c73\u58f3\u7684\u81ea\u53d1\u7ec6\u5316\uff0c\u8fd9\u4f7f\u5f97\u6240\u5f97\u7684RhPx@NPC\u7eb3\u7c73\u58f3\u5c42\u5177\u6709\u53ef\u63a7\u7684\u8584\u78b3\u7eb3\u7c73\u58f3\u5c42\u3001\u9ad8\u8868\u9762\u79ef\u3001\u4e30\u5bcc\u7684\u4ecb\u5b54\u7387\u548cN\uff0cP\u5171\u63ba\u6742\u7b49\u4f18\u70b9\u3002RhPx@NPC\u7eb3\u7c73\u58f3\u5c42\u57280-14\u7684\u5bbdpH\u8303\u56f4\u5185\u8868\u73b0\u51fa\u4f18\u5f02\u7684HER\u7535\u50ac\u5316\u6d3b\u6027\u548c\u8010\u4e45\u6027\u3002\u6b64\u5916\uff0c\u8d85\u8584\u78b3\u5c42\u5728\u4fdd\u62a4RhPx\u00a0NPs\u514d\u53d7\u8150\u8680\u65b9\u9762\u8d77\u7740\u81f3\u5173\u91cd\u8981\u7684\u4f5c\u7528\uff0c\u4ece\u800c\u5728\u53cd\u5e94\u8fc7\u7a0b\u4e2d\u4fdd\u6301\u4e86RhPx@NPC\u50ac\u5316\u5242\u7684\u8010\u4e45\u6027\u3002\u8fd9\u9879\u5de5\u4f5c\u4e3a\u8bbe\u8ba1\u5177\u6709\u9ad8\u50ac\u5316\u6d3b\u6027\u548c\u7a33\u5b9a\u6027\u7684\u5f02\u8d28\u7ed3\u6784\u7535\u50ac\u5316\u5242\u63d0\u4f9b\u4e86\u4e00\u79cd\u6709\u6548\u7684\u7b56\u7565\u3002<\/p>\n<p><strong><b>\u00a0<\/b><\/strong><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/full\/10.1002\/adfm.201901790\"><u>Embedding RhP<\/u><u><sub>x<\/sub><\/u><u>\u00a0in N, P Co<\/u><u>&#8211;<\/u><u>Doped Carbon Nanoshells Through Synergetic Phosphorization and Pyrolysis for Efficient Hydrogen Evolution<\/u><\/a>\uff08Adv. Funct. Mater., 2019, DOI:10.1002\/adfm.201901790\uff09<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u5b66\u672f\u7ec4<strong><b>\u6728\u6587\u97ec<\/b><\/strong>\u7ffb\u8bd1\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u867d\u7136\u7535\u5316\u5b66\u6c34\u5206\u89e3\u88ab\u8ba4\u4e3a\u662f\u4e00\u79cd\u73af\u4fdd\u3001\u9ad8\u6548\u7684\u65e0\u6c61\u67d3\u5236\u6c22\u9014\u5f84\uff0c\u4f46\u4ecd\u9700\u8981\u4e00\u79cd\u9ad8\u6548\u7684\u6790\u6c22\u53cd\u5e94\uff08HER\uff09\u7535\u50ac\u5316\u5242\u3002\u76ee\u524d\uff0cPt\u57fa\u6750\u6599\u88ab\u8ba4\u4e3a\u662f\u6700\u5148\u8fdb\u7684\u7535\u50ac\u5316\u5242\uff0c\u5c24\u5176\u662f&#8230;<\/p>\n","protected":false},"author":2109,"featured_media":176376,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[116,2639,4032,4031],"class_list":["post-176374","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-catalyst","tag-2639","tag-4032","tag-4031"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/176374"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2109"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=176374"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/176374\/revisions"}],"predecessor-version":[{"id":179008,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/176374\/revisions\/179008"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/176376"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=176374"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=176374"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=176374"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}