{"id":177544,"date":"2019-06-15T06:30:38","date_gmt":"2019-06-14T22:30:38","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=177544"},"modified":"2019-06-14T09:53:56","modified_gmt":"2019-06-14T01:53:56","slug":"%e3%80%90%e5%b7%b2%e6%a0%a1%e7%a8%bf%e3%80%91%e6%be%b3%e5%a4%a7%e5%88%a9%e4%ba%9a%e5%8d%97%e6%98%86%e5%a3%ab%e5%85%b0%e5%a4%a7%e5%ad%a6%e9%99%88%e5%bf%97%e5%88%9a%e7%bb%bc%e8%bf%b0%ef%bc%9a%e6%9f%94","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=177544","title":{"rendered":"\u6fb3\u5927\u5229\u4e9a\u5357\u6606\u58eb\u5170\u5927\u5b66\u9648\u5fd7\u521a\u7efc\u8ff0\uff1a\u67d4\u6027\u70ed\u7535\u6750\u6599\u548c\u53d1\u7535\u673a\uff1a\u6311\u6218\u548c\u521b\u65b0"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u5982\u4eca\uff0c\u5c0f\u578b\u5316\u7684\u96c6\u6210\u7535\u5b50\u4ea7\u54c1\u8b6c\u5982\u53ef\u7a7f\u6234\u548c\u533b\u7597\u690d\u5165\u8bbe\u5907\u6b63\u5728\u84ec\u52c3\u53d1\u5c55\u3002\u7531\u4e8e\u67d4\u6027\u70ed\u7535\u6750\u6599\u548c\u88c5\u7f6e\u80fd\u591f\u901a\u8fc7\u5c06\u70ed\u91cf\u4e00\u81f4\u5730\u8fde\u63a5\u5230\u70ed\u6e90\u4e0a\u800c\u5c06\u70ed\u91cf\u76f4\u63a5\u8f6c\u6362\u6210\u7535\u80fd\uff0c\u800c\u53d7\u5230\u8d8a\u6765\u8d8a\u591a\u7684\u5173\u6ce8\u3002\u67d4\u6027\u70ed\u7535\u805a\u5408\u7269\u6750\u6599\u7531\u4e8e\u5176\u56fa\u6709\u7684\u67d4\u97e7\u6027\uff0c\u53ef\u8d1f\u62c5\u6027\u548c\u4f4e\u6bd2\u6027\u800c\u5f15\u4eba\u5173\u6ce8\uff0c\u800c\u65e0\u673a\u67d4\u6027\u70ed\u7535\u6750\u6599\u4e5f\u5177\u6709\u9ad8\u80fd\u91cf\u8f6c\u6362\u6548\u7387\uff0c\u5927\u529f\u7387\u8f93\u51fa\u548c\u5728\u76f8\u5bf9\u9ad8\u6e29\u4e0b\u7684\u7a33\u5b9a\u6027\u7b49\u4f18\u70b9\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u671f\uff0c<strong>\u6fb3<\/strong><strong>\u5927\u5229\u4e9a\u5357\u6606\u58eb\u5170\u5927\u5b66\u9648\u5fd7\u521a<\/strong><strong>\u6559\u6388\u4e0e\u6606\u58eb\u5170\u5927\u5b66\u90b9\u8fdb\u6559\u6388\u548c\u4e0a\u6d77\u7845\u9178\u76d0\u6240\u7684\u9648\u7acb\u4e1c\u6559\u6388\u548c\u53f2\u8fc5\u6559\u6388<\/strong>\u5728Advanced Materials\u4e0a\u53d1\u8868\u4e86\u9898\u4e3a\u201cFlexible Thermoelectric Materials and Generators:Challenges and Innovations\u201d \u7684\u7efc\u8ff0\u8bba\u6587\u3002\u672c\u6587\u603b\u7ed3\u4e86\u67d4\u6027\u70ed\u7535\u6750\u6599\u548c\u5668\u4ef6\u53d1\u5c55\u7684\u6700\u65b0\u6280\u672f\uff0c\u5305\u62ec\u901a\u8fc7\u5c06\u6750\u6599\u5316\u5b66\u548c\u7269\u7406\u4e0e\u6027\u80fd\u76f8\u5173\u8054\u6765\u63a2\u7d22\u67d4\u6027\u70ed\u7535\u6750\u6599\u548c\u5668\u4ef6\u6027\u80fd\u80cc\u540e\u7684\u57fa\u672c\u539f\u7406\uff0c\u7a81\u51fa\u4e86\u9ad8\u6027\u80fd\u67d4\u6027\u70ed\u7535\u6750\u6599\u7684\u5c40\u9650\u6027\u4ee5\u53ca\u4e0e\u6bcf\u79cd\u4f18\u5316\u7b56\u7565\u76f8\u5173\u7684\u57fa\u672c\u673a\u5236\u3002\u6700\u540e\uff0c\u603b\u7ed3\u4e86\u67d4\u6027\u70ed\u7535\u6750\u6599\u7684\u5176\u4f59\u6311\u6218\uff0c\u63d0\u51fa\u4e86\u6307\u5bfc\u672a\u6765\u53d1\u5c55\u7684\u5efa\u8bae\u548c\u6846\u67b6\uff0c\u4e3a\u80fd\u6e90\u5e02\u573a\u4e2d\u67d4\u6027\u70ed\u7535\u5668\u4ef6\u7684\u7f8e\u597d\u672a\u6765\u94fa\u5e73\u4e86\u9053\u8def\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe1\u00a0 \u67d4\u6027\u70ed\u7535\uff08FTE\uff09\u88c5\u7f6e\u7684\u5e94\u7528\u548c\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177571 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/1-1.png\" alt=\"\" width=\"700\" height=\"682\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/1-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/1-1-300x292.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>&nbsp;<\/p>\n<p>a\uff09\u53ef\u7a7f\u6234\u548c\/\u6216\u53ef\u690d\u5165\u7535\u5b50\u8bbe\u5907\u7684\u5e94\u7528\u5728\u4eba\u4f53\u4e0a\uff1b<\/p>\n<p>b\uff09\u53ef\u7a7f\u6234\u548c\/\u6216\u53ef\u690d\u5165\u7535\u5b50\u8bbe\u5907\u7684\u7edf\u8ba1\u548c\u4f30\u8ba1\u7684\u5168\u7403\u5e02\u573a\u4ef7\u503c\uff1b<\/p>\n<p>c) FTE\u8bbe\u5907\u7684\u5178\u578b\u6a21\u5757\u793a\u610f\u56fe\uff1b<\/p>\n<p>d\uff09FTE\u88c5\u7f6e\u7684\u53d1\u7535\u6548\u7387\uff08\u03b7p\uff09\u4e0e\u5e73\u5747\u54c1\u8d28\u56e0\u6570\uff08zT\uff09\uff0c\u6750\u6599\u7684zTave\u7684\u51fd\u6570\u5173\u7cfb\u3002<\/p>\n<p><strong>\u56fe2\u00a0 \u4e0d\u540c\u70ed\u7535\u6750\u6599\uff08FTE\uff09\u4f18\u70b9\uff08zT\uff09<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177572 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/2-1.png\" alt=\"\" width=\"700\" height=\"698\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/2-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/2-1-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/2-1-300x300.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>&nbsp;<\/p>\n<p>\u5305\u62ec\u5bfc\u7535\u805a\u5408\u7269\uff0c\u805a\u5408\u7269\u590d\u5408\u6750\u6599\u548c\u65e0\u673a\u8584\u819c<\/p>\n<p><strong>\u56fe3\u00a0 \u5178\u578b\u5bfc\u7535\u805a\u5408\u7269\u7684\u5206\u5b50\u548c\u5316\u5b66\u7ed3\u6784<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177573 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/3-1.png\" alt=\"\" width=\"700\" height=\"694\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/3-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/3-1-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/3-1-300x297.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u4ee3\u8868\u6027\u5bfc\u7535\u805a\u5408\u7269\u7684\u5206\u5b50\u7ed3\u6784\uff0c\u5305\u62ecp\u578b\u805a\u82ef\u80fa\uff08PANI\uff09\uff0c\u805a\uff083-\u5df1\u57fa\u567b\u5429-2,5-\u4e8c\u57fa\uff09\uff08P3HT\uff09\uff0c\u805a\uff083-\u4e01\u57fa\u567b\u5429\uff09\uff08P3BT\uff09\uff0c\u805a\u4e59\u7094\uff08PA\uff09\uff0c\u805a\uff083,4-\u4e9a\u4e59\u4e8c\u6c27\u57fa\u567b\u5429\uff09\uff08PEDOT\uff09\uff0c\u805a\u567b\u5429\uff08PTs\uff09\u548c\u805a\u5421\u54af\uff08PPy\uff09\uff0cn\u578b\u82ef\u5e76\u4e8c\u544b\u5583\u4e8c\u916e\u57fa\u805a\uff08\u5bf9\u4e9a\u82ef\u57fa\u4e9a\u4e59\u70ef\u57fa\uff09\uff08BDPPV\uff09\uff0c\u805a\uff08Cu-\u82ef\u516d\u786b\u9187\uff09\uff08CuBHT\uff09\u805a\u82ef\u5e76\u54aa\u5511\u5e76\u82ef\u5e76\u84bd\uff08BBL\uff09\uff0c\u805a\uff08perinaphthalene\uff09\uff08PPN\uff09 \uff09\u548cpoly [Kx\uff08Ni-ett\uff09]\uff1b<\/p>\n<p>b\uff09\u5bfc\u7535\u805a\u5408\u7269\u4e2dsp<sup>2<\/sup>\u6742\u5316\u548c\u5171\u8f6d\u03c0\u952e\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe4\u00a0 \u5bfc\u7535\u805a\u5408\u7269\u7684\u5fae\u89c2\u7ed3\u6784<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177574 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/4-1.png\" alt=\"\" width=\"700\" height=\"683\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/4-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/4-1-300x293.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5bfc\u7535\u805a\u5408\u7269\u4e2d\u7684\u975e\u5747\u76f8\u5fae\u7ed3\u6784\u7531\u7ed3\u6676\u57df\u548c\u65e0\u5b9a\u5f62\u57df\u968f\u673a\u7ec4\u6210\uff1b<\/p>\n<p>b\uff09\u5bfc\u7535\u805a\u5408\u7269\u4e2d\u5206\u5b50\u94fe\u7684\u591a\u91cd\u8fde\u63a5\u3002<\/p>\n<p><strong>\u56fe5\u63ba\u6742\u5bfc\u7535\u805a\u5408\u7269\u4e2d\uff08\u53cc\uff09\u6781\u5316\u5b50\u7684\u5206\u5b50\u548c\u7535\u5b50\u7ed3\u6784<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177575 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/5.png\" alt=\"\" width=\"700\" height=\"684\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/5.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/5-300x293.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u805a\u82ef\u4e59\u70ef\u78fa\u9178\u76d0\uff08PSS\uff09\u63ba\u6742\u7684\u805a\uff083,4-\u4e9a\u4e59\u4e8c\u6c27\u57fa\u567b\u5429\uff09\uff08PEDOT\uff09\u4ece\u4e2d\u6027\u72b6\u6001\u5230\uff08\u53cc\uff09\u6781\u5316\u5b50\u72b6\u6001\u7684\u5206\u5b50\u7ed3\u6784\uff1b<\/p>\n<p>b\uff09\u5177\u6709\uff08bi\uff09\u6781\u5316\u5b50\u4ea7\u751f\u548c\u63ba\u6742\u6c34\u5e73\u7684\u7535\u5b50\u7ed3\u6784\u6f14\u53d8\uff0c\u5176\u4e2dLUMO\u548cHOMO\u5206\u522b\u4ee3\u8868\u6700\u4f4e\u7684\u672a\u5360\u5206\u5b50\u8f68\u9053\u548c\u6700\u9ad8\u5360\u636e\u5206\u5b50\u8f68\u9053\uff1b<\/p>\n<p>c\uff09\u5728\u9ad8\u63ba\u6742\u6c34\u5e73\u4e0b\u4ea7\u751f\u94fe\u5185\u548c\u94fe\u95f4\uff08\u53cc\uff09\u6781\u5316\u5b50\u5076\u5408\u3002<\/p>\n<p><strong>\u56fe6\u57fa\u4e8e\u6c27\u5316\u8fd8\u539f\u7684\u5bfc\u7535\u805a\u5408\u7269\u901a\u8fc7\u5316\u5b66\u53cd\u5e94\u63ba\u6742<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177576 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/6.png\" alt=\"\" width=\"700\" height=\"601\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/6.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/6-300x258.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u901a\u8fc7\u5316\u5b66\u53cd\u5e94\u8fdb\u884c\u57fa\u4e8e\u6c27\u5316\u8fd8\u539f\u7684\u63ba\u6742\u7684\u673a\u7406\uff1b<\/p>\n<p>b\uff09\u5e38\u89c1\u7684n\u578b\u63ba\u6742\u5242\u56db\uff08\u4e8c\u7532\u57fa\u6c28\u57fa\uff09\u4e59\u70ef\uff08TDAE\uff09\uff0c\u80bc\u548c\u805a\u4e59\u70ef\u4e9a\u80fa\uff08PEI\uff09\u7684\u5206\u5b50\u7ed3\u6784; p\u578b\u63ba\u6742\u5242\u5305\u62ecI<sub>2<\/sub>\uff0cFeCl<sub>3<\/sub>\u548c\u4e09\u6c1f\u5316\u94c1\uff08Fetf\uff09\u7684\u94c1\u76d0\uff1b<\/p>\n<p>c\uff09TDAE\u63ba\u6742\u7684PEDOT\u7684\u7535\u5bfc\u7387\uff08\u03c3\uff09\uff0c\u585e\u8d1d\u514b\u7cfb\u6570\uff08S\uff09\u548c\u529f\u7387\u56e0\u6570\uff08S2\u03c3\uff09\uff1b<\/p>\n<p>d\uff09TDAE\u63ba\u6742\u7684PEDOT\u7684\u5316\u5b66\u673a\u7406\u3002<\/p>\n<p><strong>\u56fe7 \u57fa\u4e8e\u6c27\u5316\u8fd8\u539f\u7684\u5bfc\u7535\u805a\u5408\u7269\u901a\u8fc7\u7535\u5316\u5b66\u53cd\u5e94\u63ba\u6742<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177577 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/7.png\" alt=\"\" width=\"700\" height=\"576\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/7.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/7-300x247.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u57fa\u4e8e\u6c27\u5316\u8fd8\u539f\u7684\u63ba\u6742\u7684\u673a\u7406\u548c\u7ed3\u6784\u7535\u5316\u5b66\u53cd\u5e94\uff1b<\/p>\n<p>b\uff09\u5177\u6709\u4e0d\u540c\u65bd\u52a0\u7535\u4f4d\u7684\u7535\u5316\u5b66\u63ba\u6742\u7684\u805a\uff083,4-\u4e9a\u4e59\u4e8c\u6c27\u57fa\u567b\u5429\uff09\uff08PEDOT\uff09flm\u7684\u7535\u5bfc\u7387\uff08\u03c3\uff09\u548c\u585e\u8d1d\u514b\u7cfb\u6570\uff08S\uff09\uff1b<\/p>\n<p>c\uff09\u6676\u4f53\u7ba1\u4e2d\u7535\u5316\u5b66\u63ba\u6742\u7684\u805a\uff083,4-\u4e9a\u4e59\u4e8c\u6c27\u57fa\u567b\u5429\uff09\u805a\u82ef\u4e59\u70ef\u78fa\u9178\u76d0\uff08PEDOT\uff1aPSS\uff09\u7684\u03c3\u548cS\uff0c\u5176\u4e2d\u5b9e\u73b0\u4e86\u539f\u4f4d\u8868\u5f81\u3002<\/p>\n<p><strong>\u56fe8 \u57fa\u4e8e\u9178\u7684\u63ba\u6742\u5bfc\u7535\u805a\u5408\u7269<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177578 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/8.png\" alt=\"\" width=\"700\" height=\"660\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/8.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/8-300x283.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5e38\u89c1\u63ba\u6742\u5242\u7684\u5206\u5b50\u7ed3\u6784\uff0c\u5305\u62ec\u9178\u63ba\u6742\u52424-\u4e59\u57fa\u82ef\u78fa\u9178\uff08EBSA\uff09\uff0c\uff08trideca\u6c1f\u4ee3-1,1,2,2-\u56db\u6c22\u8f9b\u57fa\uff09\u4e09\u6c2f\u7845\u70f7\uff08FTS\uff09\uff0c\u6a1f\u8111\u78fa\u9178\uff08CSA\uff09\uff0c\u5341\u4e8c\u70f7\u57fa\u82ef\u78fa\u9178\uff08DBSA\uff09\u548c[6,6] -\u82ef\u57fa-C61-\u4e01\u9178\u7532\u916f\uff08PCBM\uff09\uff1b [35]\u57fa\u7840\u63ba\u6742\u5242\u9690\u8272\u7ed3\u6676\u7d2b\uff08LCV\uff09\uff0c\uff084-\uff081,3-\u4e8c\u7532\u57fa-2,3-\u4e8c\u6c22-1H-\u82ef\u5e76\u54aa\u5511-2-\u57fa\uff09\u82ef\u57fa\uff09\u4e8c\u7532\u80fa\uff08N-DMBI\uff09\u548c4-\uff081,3-\u4e8c\u7532\u57fa-2,3-\u4e8c\u6c22-1H-\u82ef\u5e76\u54aa\u5511-2-\u57fa\uff09-N\uff0cN-\u4e8c\u82ef\u57fa\u82ef\u80fa\uff08N-DPBI\uff09\uff1b<\/p>\n<p>b\uff09\u63ba\u6742\u805a\uff082,5-\u53cc\uff083-\u5341\u56db\u70f7\u57fa\u567b\u5429\uff09\u7684\u793a\u610f\u56fe\uff0c2-\u4e01\u57fa\u567b\u5429\u5e76[3,2-b]\u567b\u5429\uff09\uff08PBTTT\uff09\u5206\u522b\u5177\u6709\u4e0d\u540c\u7684\u52a0\u5de5\u65b9\u6cd5\uff0c\u5373FTS\u84b8\u6c14\u548cEBSA\u6eb6\u6db2\uff1b<\/p>\n<p>c\uff0cd\uff09\u5173\u4e8e\u7535\u5bfc\u7387\uff08\u03c3\uff09\u6d4b\u91cf\u585e\u8d1d\u514b\u7cfb\u6570\uff08S\uff09\u548c\u529f\u7387\u56e0\u6570\uff08S<sup>2<\/sup>\u03c3\uff09\uff0c\u5176\u4e2d\u6a59\u8272\u70b9\u4ee3\u8868EBSA\u63ba\u6742\u7684\u8584\u819c\uff0c\u7d2b\u8272\u70b9\u4ee3\u8868FTS\u63ba\u6742\u7684\u8584\u819c\u3002<\/p>\n<p><strong>\u56fe9 \u901a\u8fc7\u6781\u6027\u6eb6\u5242\u5904\u7406\u5bf9\u5bfc\u7535\u805a\u5408\u7269\u8fdb\u884c\u4e8c\u6b21\u63ba\u6742<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177579 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/9.png\" alt=\"\" width=\"700\" height=\"720\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/9.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/9-292x300.png 292w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u4ece\u76d8\u7ed5\u7ed3\u6784\u5230\u7ebf\u6027\u6216\u5ef6\u4f38\u7ebf\u5708\u7ed3\u6784\u7684\u6784\u8c61\u53d8\u5316\uff0c\u4ece\u82ef\u5e76\u5230\u918c\u578b\u7ed3\u6784\u7684\u5316\u5b66\u7ed3\u6784\u6f14\u53d8\uff0c\u4ee5\u53ca\u6781\u6027\u6eb6\u5242\u5904\u7406\u540e\u4ece\u4f4e\u7ed3\u6676\u5230\u9ad8\u7ed3\u6676\u7684\u5f62\u6001\u53d8\u5316\uff1b<\/p>\n<p>b\uff09\u4e8c\u7532\u57fa\u4e9a\u781c\uff08DMSO\uff09-\u805a\uff08\u73af\u6c27\u4e59\u70f7\uff09\uff08PEO\uff09\u4e8c\u5143\u4e8c\u6b21\u63ba\u6742\u5242\u540c\u65f6\u589e\u52a0\u7535\u5bfc\u7387\uff08\u03c3\uff09\u548c\u585e\u8d1d\u514b\u7cfb\u6570\uff08S\uff09\uff08\u7ea2\u8272\u865a\u7ebf\u7a81\u51fa\u663e\u793a\uff09 PEDOT\uff1aPSS\uff1b<\/p>\n<p>c\uff09DMSO-PEO\u4e8c\u5143\u4e8c\u6b21\u63ba\u6742\u5242\u5904\u7406\u7684PEDOT\uff1aPSS\u4e2d\u529f\u7387\u56e0\u6570\uff08S<sup>2<\/sup>\u03c3\uff09\u7684\u663e\u7740\u589e\u52a0\uff08\u7531\u7ea2\u8272\u865a\u7ebf\u7a81\u51fa\u663e\u793a\uff09\u3002<\/p>\n<p><strong>\u56fe10 \u901a\u8fc7\u540e\u5904\u7406\u5bf9\u5bfc\u7535\u805a\u5408\u7269\u8fdb\u884c\u4e8c\u6b21\u63ba\u6742<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177580 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/10.png\" alt=\"\" width=\"700\" height=\"685\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/10.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/10-300x294.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u540e\u5904\u7406\u540ePEDOT\uff1aPSS flm\u7684\u7535\u5bfc\u7387\uff08\u03c3\uff09\uff0c\u8fc7\u4e0d\u540c\u79cd\u7c7b\u7684\u63ba\u6742\u5242\uff0c\u5305\u62ec\u7532\u9187\uff0cCuCl<sub>2<\/sub>\u548cZnCl<sub>2<\/sub>\u7684N\uff0cN-\u4e8c\u7532\u57fa\u7532\u9170\u80fa\uff08DMF\uff09\u6eb6\u6db2\uff0c\u7532\u9178\u548c\u786b\u9178\uff1b<\/p>\n<p>b\uff09\u901a\u8fc7\u6d53\u786b\u9178\u7684\u540e\u5904\u7406\u8bf1\u5bfc\u7684\u5e26\u7535PEDOT\u548cPSS\u4e4b\u95f4\u7684\u76f8\u5206\u79bb\uff1b<\/p>\n<p>c\uff09\u5728PEDOT\uff1aPSS\u4e2d\u53bb\u9664\u65e0\u6548PSS\u7684\u6548\u679c\u7684\u793a\u610f\u56fe\uff0c\u5176\u4e2d\u8f7d\u4f53\u7ecf\u5386\u4e0d\u53d7\u963b\u788d\u7684\u8fd0\u8f93\u5e76\u4e14\u8868\u73b0\u51fa\u9ad8\u79fb\u52a8\u6027\u3002<\/p>\n<p>d\uff09\u53bb\u9664\u4f4e\u6548PSS\u540eEG \/ DMSO\u6df7\u5408PEDOT\uff1aPSS flm\u7684\u529f\u7387\u56e0\u6570\uff08S<sup>2<\/sup>\u03c3\uff09\u548czT\u3002<\/p>\n<p><strong>\u56fe11 \u5bfc\u7535\u805a\u5408\u7269\u7684\u6709\u673a\u5c0f\u5206\u5b50\u5916\u5ef6<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177581 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/11.png\" alt=\"\" width=\"700\" height=\"711\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/11.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/11-295x300.png 295w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5177\u6709\u5c0f\u7684P3HT\u94fe\u7684\u53d6\u5411\u8fc7\u7a0b\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>b\uff09P3HT\u548cTCB\u5206\u5b50\u4e4b\u95f4\u53ef\u5ffd\u7565\u4e0d\u8ba1\u7684\u6676\u683c\u5931\u914d\u548c\u03c0-\u03c0\u76f8\u4e92\u4f5c\u7528\uff1b<\/p>\n<p>c\uff09\u53d6\u5411\u7684P3HT\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>d\uff09\u6d4b\u91cf\u5177\u6709\u548c\u4e0d\u5177\u6709TCB\u5904\u7406\u7684P3HT\u819c\u7684S<sup>2<\/sup>\u03c3\uff0c\u5176\u4e2d\u5728TCB\u5904\u7406\u540e\u663e\u793a\u51fa\u5f3a\u7684\u5404\u5411\u5f02\u6027\u548c\u63d0\u9ad8\u7684\u7535\u6027\u80fd\u3002<\/p>\n<p><strong>\u56fe12 <span class=\"tlid-translation translation\" lang=\"zh-CN\"><span class=\"\" title=\"\">\u5728\u5bfc\u7535\u805a\u5408\u7269\u548c\u586b\u6599\u4e4b\u95f4\u7684\u754c\u9762\u5904\u7684\u80fd\u91cf\u8fc7\u6ee4\u6548\u5e94\u7684\u793a\u610f\u56fe<\/span><\/span><\/strong><\/p>\n<p><strong>\u00a0<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177582 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/12.png\" alt=\"\" width=\"700\" height=\"536\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/12.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/12-300x230.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p><strong>\u56fe13 \u539f\u4f4d\u805a\u5408\u6cd5\u7684\u754c\u9762\u6709\u5e8f\u6548\u5e94<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177583 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/13.png\" alt=\"\" width=\"700\" height=\"661\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/13.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/13-300x283.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u754c\u9762\u6709\u5e8f\u6548\u5e94\u673a\u7406\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>b\uff09\u5728\u805a\u82ef\u80fa\uff08PANI\uff09\u57fa\u8d28\u4e2d\u63ba\u5165\u5355\u58c1\u78b3\u7eb3\u7c73\u7ba1\uff08SWCNT\uff09\u586b\u6599\u540e\u6539\u5584\u8f7d\u6d41\u5b50\u8fc1\u79fb\u7387\uff08\u03bc\uff09\uff1b<\/p>\n<p>c\uff09SWCNT \/ PANI\u590d\u5408\u6750\u6599\u7684TEM\u56fe\u50cf\uff0c\u5176\u4e2dPANI\u94fe\u7d27\u5bc6\u9644\u7740\u5728SWCNT\u8868\u9762\u4e0a\uff1b<\/p>\n<p>d\uff09\u5177\u6709\u754c\u9762\u6709\u5e8f\u6548\u5e94\u7684\u4e8c\u6b21\u63ba\u6742\u5242\u5904\u7406\u7684\u793a\u610f\u6027\u6548\u679c\uff1b<\/p>\n<p>e\uff09\u6d4b\u91cf\u539f\u4f4d\u805a\u5408\u7684SWCNT \/ PANI\u590d\u5408\u6750\u6599\u7684\u585e\u8d1d\u514b\u7cfb\u6570\uff08S\uff09\u548c\u7535\u5bfc\u7387\uff08\u03c3\uff09\uff0c\u5176\u4e2d\u7531\u4e8e\u663e\u7740\u6539\u5584\u7684\u03bc\uff0c\u89c2\u5bdf\u5230S\u548c\u03c3\u7684\u540c\u65f6\u589e\u52a0\u3002<\/p>\n<p><strong>\u56fe14 \u9010\u5c42\uff08LbL\uff09\u5236\u9020\u7684\u754c\u9762\u6709\u5e8f\u6548\u5e94<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177584 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/14.png\" alt=\"\" width=\"700\" height=\"689\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/14.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/14-300x295.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5236\u9020\u805a\u82ef\u80fa\uff08PANI\uff09\/\u77f3\u58a8\u70ef &#8211; \u805a\uff083,4-\uff09\u7684\u5178\u578b\u7a0b\u5e8f\u4e59\u4e8c\u6c27\u57fa\u567b\u5429\uff09\u805a\u82ef\u4e59\u70ef\u78fa\u9178\u76d0\uff08PEDOT\uff1aPSS\uff09\/ PANI \/\u53cc\u58c1\u78b3\u7eb3\u7c73\u7ba1\uff08DWCNT\uff09-PEDOT\uff1b<\/p>\n<p>b\uff09\u6865\u63a5\u77f3\u58a8\u70ef\u677f\u7684DWCNT\u7f51\u7edc\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>c\uff09\u6d4b\u91cfPANI \/\u77f3\u58a8\u70efPEDOT\u7684S<sup>2<\/sup>\u03c3\u3002<\/p>\n<p><strong>\u56fe15 \u5bfc\u7535\u805a\u5408\u7269\u590d\u5408\u6750\u6599\u4e2d\u8868\u9762\u72b6\u6001\u7684\u5f71\u54cd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177585 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/15.png\" alt=\"\" width=\"700\" height=\"567\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/15.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/15-300x243.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09Bi<sub>2<\/sub>Te<sub>3<\/sub> \/ PEDOT\uff1aPSS\u8584\u819c\u7684\u6a2a\u622a\u9762\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>b\uff09\u901a\u8fc7\u9178\u6d17\u9664\u53bb\u8868\u9762\u4e0a\u7684\u6c27\u5316\u5c42\u540e\uff0c\u529f\u7387\u56e0\u6570\uff08S<sup>2<\/sup>\u03c3\uff09\u7684\u663e\u7740\u589e\u5f3a\uff1b<\/p>\n<p>c\uff0cd\uff09\u5177\u6709\u4e0d\u540cAu\u7eb3\u7c73\u9897\u7c92\u8868\u9762\u72b6\u6001\u7684Au \/ PANI\u590d\u5408\u6750\u6599\u7684\u7535\u5bfc\u7387\uff08\u03c3\uff09\u548c\u585e\u8d1d\u514b\u7cfb\u6570\uff08S\uff09\u3002<\/p>\n<p><strong>\u56fe16 \u6c1f\u5316\u7269\u5f62\u6001\u5bf9\u5bfc\u7535\u805a\u5408\u7269\u590d\u5408\u6750\u6599\u7684\u5f71\u54cd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177586 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/16.png\" alt=\"\" width=\"700\" height=\"730\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/16.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/16-288x300.png 288w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a-c\uff09Te\u7eb3\u7c73\u7ebf\u7684AFM\u56fe\u50cf\uff0c\u957f\u5ea6\u4e3a284\u00b146\uff0c391\u00b147\uff0c\u5206\u522b\u4e3a867\u00b1101nm\uff1b<\/p>\n<p>d\uff09\u5173\u4e8eTe\u7eb3\u7c73\u7ebf\u957f\u5ea6\u548c\u76f4\u5f84\u7684Te \/ PEDOT\uff1aPSS\u590d\u5408\u6750\u6599\u7684\u7535\u5bfc\u7387\uff08\u03c3\uff09\u548c\u585e\u8d1d\u514b\u7cfb\u6570\uff08S\uff09\uff1b<\/p>\n<p>e-g\uff09PEDOT\uff1aDBSA \/ Cl-Te\u590d\u5408\u6750\u6599\u7684SEM\u56fe\u50cf\u5173\u4e8eTe\u542b\u91cf\uff0c\u5176\u4e2d\u8f83\u5c0f\u7684Te\u70b9\u53ef\u89c1\uff0c\u5177\u6709\u8f83\u4f4e\u7684Te\u542b\u91cf\uff1b<\/p>\n<p>h\uff09PEDOT\u7684\u03c3\u548cS\uff1a\u5173\u4e8eTe\u542b\u91cf\u7684DBSA \/ Cl-Te\u590d\u5408\u7269\u3002<\/p>\n<p><strong>\u56fe17 \u5728\u5bfc\u7535\u805a\u5408\u7269\u590d\u5408\u6750\u6599\u4e2d\u5f62\u6210\u8f7d\u6d41\u5b50\u4f20\u8f93\u96a7\u9053<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177587 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/17.png\" alt=\"\" width=\"700\" height=\"499\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/17.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/17-300x214.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u57fa\u4e8e\u78b3\u7eb3\u7c73\u7ba1\uff08CNT\uff09\/\u805a\u5408\u7269\u590d\u5408\u6750\u6599\u7684\u5178\u578b\u7ed3\u6784\uff0c\u5176\u4e2d\u805a\u5408\u7269\u4e73\u6db2\u7528\u4e8e\u5728\u5e72\u71e5\u540e\u4ea7\u751f\u6392\u9664\u7684\u4f53\u79ef\u5e76\u5c06CNT\u63a8\u5165\u754c\u9762\u7a7a\u95f4\uff0c\u5f62\u6210\u8f7d\u4f53\u4f20\u8f93\u96a7\u9053\uff1b<\/p>\n<p>b\uff09\u5236\u5907\u7684CNT-\u805a\uff08\u4e59\u9178\u4e59\u70ef\u916f\uff09\uff08PVAc\uff09\u590d\u5408\u7269\u7684SEM\u56fe\u50cf\uff0c\u5176\u4e2d\u63ba\u5165\u7684CNT\u5bc6\u96c6\u5730\u5206\u5e03\u5728\u4e73\u6db2\u9897\u7c92\u4e4b\u95f4\u7684\u95f4\u9699\u4e2d\uff0c\u800c\u4e0d\u662f\u968f\u673a\u5206\u5e03\u5728\u7cfb\u7edf\u4e2d\uff1b<\/p>\n<p>c\uff09\u8f7d\u6ce2\u4f20\u8f93\u96a7\u9053\u4e2d\u7535\u8fde\u63a5\u4f46\u70ed\u65ad\u5f00\u7684\u8fde\u63a5\u70b9\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>d\uff09\u5177\u6709\u4e0d\u540cCNT\u548c\u7a33\u5b9a\u5242\u7c7b\u578b\u7684\u590d\u5408\u6750\u6599\u7684\u529f\u7387\u56e0\u6570\uff08S<sup>2<\/sup>\u03c3\uff09\u76f8\u5bf9\u4e8eCNT\u542b\u91cf\u7ed8\u5236\u3002<\/p>\n<p><strong>\u56fe18 \u65e0\u673a\/\u6709\u673a\u8d85\u6676\u683c\u901a\u8fc7\u5c06\u6709\u673a\u5206\u5b50\u5d4c\u5165\u65e0\u673a\u819c\u4e2d<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177558 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/18.png\" alt=\"\" width=\"700\" height=\"680\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/18.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/18-300x291.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u7535\u5316\u5b66\u7684\u793a\u610f\u56fe\uff0c\u5c42\u6cd5\u5236\u5907TiS2 [\uff08HA\uff09x\uff08H2O\uff09y\uff08DMSO\uff09z]\u8d85\u6676\u683c\uff1b<\/p>\n<p>b\uff09TiS<sub>2<\/sub> [\uff08HA\uff09<sub>x<\/sub>\uff08H <sub>2<\/sub> O\uff09<sub>y<\/sub>\uff08DMSO\uff09<sub>z<\/sub>]\u8d85\u6676\u683c\u7684\u653e\u5927\u7684HAADF-STEM\u56fe\u50cf\uff0c\u5176\u4e2dHA\u5206\u5b50\u5d4c\u5165TiS<sub>2<\/sub>\u5355\u6676\u4e2d\uff1b<\/p>\n<p>c\uff09HA\u5206\u5b50\u53bb\u5d4c\u5165\u540e\u8f7d\u6d41\u5b50\u6d53\u5ea6\uff08n\uff09\u7684\u964d\u4f4e\uff0c\u5176\u4e2dn\u88ab\u7ea2\u8272\u865a\u7ebf\u7a81\u51fa\u663e\u793a\uff1b<\/p>\n<p>d\uff09\u4e0d\u540c\u8d85\u6676\u683c\u7684\u9762\u5185zT\u76f8\u5bf9\u4e8e\u6e29\u5ea6\uff0c\u5176\u4e2d\u5728413K\u4e0b\u4eceTiS2\uff08TBA\uff09<sub>0.025<\/sub>\uff08HA\uff09<sub>0.012<\/sub>\u83b7\u5f970.33\u7684\u8bb0\u5f55zT\u3002<\/p>\n<p><strong>\u56fe19 \u901a\u8fc7\u7269\u7406\u6c14\u76f8\u6c89\u79ef\u548c\u5316\u5b66\u6d74\u6c89\u79ef\u5728\u67d4\u6027\u57fa\u5e95\u4e0a\u5236\u5907\u8fde\u7eed\u65e0\u673a\u819c<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177559 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/19.png\" alt=\"\" width=\"700\" height=\"566\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/19.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/19-300x243.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u901a\u8fc7\u53cd\u5e94\u6e85\u5c04\u6cd5\u6c89\u79ef\u5728PET\u57fa\u677f\u4e0a\u7684CuI\u8584\u819c\u7684\u7167\u7247\uff1b<\/p>\n<p>b\uff09CuI\u8584\u819c\u7684zT\u4f5c\u4e3a300K\u4e0b\u7a7a\u7a74\u6d53\u5ea6p\u7684\u51fd\u6570\uff1b<\/p>\n<p>c\uff09\u6cbf\u7740[001]\u65b9\u5411\u7684\u03b1-Ag<sub>2<\/sub>S\u7684\u6676\u4f53\u7ed3\u6784\uff1b<\/p>\n<p>d\uff09\u5b9e\u9a8c\u6b8b\u7559\u7535\u5b50\u5bc6\u5ea6\u7684\u7b49\u503c\u9762\u663e\u793a\u6676\u4f53\u7ed3\u6784\u4e2dAg\u79bb\u5b50\u7684\u65e0\u5e8f\uff1b<\/p>\n<p>e\uff09\u5728\u8367\u5149\u5e95\u7269\u4e0a\u6c89\u79ef\u7684\u67d4\u8f6f\u03b1-Ag<sub>2<\/sub>S\u8584\u819c\u7684\u7167\u7247\u3002<\/p>\n<p><strong>\u56fe20 \u8fc7\u7eb3\u7c73\u7ed3\u6784\u5b9a\u5236\u5236\u5907\u72ec\u7acb\u7684Ca<sub>3<\/sub>Co<sub>4<\/sub>O<sub>9<\/sub>\u8584\u819c<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177560 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/20.png\" alt=\"\" width=\"700\" height=\"780\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/20.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/20-269x300.png 269w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09Ca<sub>3<\/sub>Co<sub>4<\/sub>O<sub>9<\/sub>\u8584\u819c\u7684\u6a2a\u622a\u9762SEM\u56fe\u50cf\uff1b<\/p>\n<p>b\uff09\u4ece\u9876\u89c6\u56fe\u770b\u7684Ca<sub>3<\/sub>Co<sub>4<\/sub>O<sub>9<\/sub>\u8584\u819c\u7684TEM\u56fe\u50cf\uff1b<\/p>\n<p>c\uff09\u72ec\u7acb\u7684\u67d4\u8f6fCa<sub>3<\/sub>Co<sub>4<\/sub>O<sub>9<\/sub>\u8584\u7247\u7684\u7167\u7247\uff1b<\/p>\n<p>\u4ece\u4e91\u6bcd\u57fa\u5e95\u4e2d\u5206\u79bbCa<sub>3<\/sub>Co<sub>4<\/sub>O<sub>9<\/sub>\u8584\u819c\u7684\u65b9\u6cd5\u3002<\/p>\n<p><strong>\u56fe21 \u901a\u8fc7\u5e94\u7528CNT\u652f\u67b6\u5236\u9020\u72ec\u7acb\u7684FTE\u8584\u819c<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177561 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/21.png\" alt=\"\" width=\"700\" height=\"710\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/21.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/21-296x300.png 296w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5236\u5907\u72ec\u7acb\u7684\u9ad8\u5ea6\u6709\u5e8f\u7684Bi<sub>2<\/sub>Te<sub>3<\/sub>-SWCNT FTE\u8584\u819c\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>b\uff09Bi<sub>2<\/sub>Te<sub>3<\/sub>\u7eb3\u7c73\u6676\u4f53\u4e0eSWCNT\u675f\u4e4b\u95f4\u7684\u754c\u9762\u7684\u660e\u4eae\u7684TEM\u56fe\u50cf\u3002\u63d2\u56fe\uff1aBi<sub>2<\/sub>Te<sub>3<\/sub>\u7684\u76f8\u5e94\u5feb\u901f\u5085\u91cc\u53f6\u53d8\u6362\uff08FFT\uff09\u56fe\u6848\uff1b<\/p>\n<p>c\uff09Bi<sub>2<\/sub>Te<sub>3<\/sub>\u7eb3\u7c73\u6676\u4f53\u751f\u957f\u671f\u95f4\u7eb3\u7c73\u5b54\u751f\u6210\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>d\uff09\u81ea\u652f\u6491Bi<sub>2<\/sub>Te<sub>3<\/sub>-SWCNT FTE\u8584\u819c\u7684\u6a2a\u622a\u9762SEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe22 \u5177\u6709\u03c0\u578b\u7ed3\u6784\u7684\u6709\u673a\u548c\u65e0\u673a\u67d4\u6027\u70ed\u7535\uff08FTE\uff09\u5668\u4ef6<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177562 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/22.png\" alt=\"\" width=\"700\" height=\"639\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/22.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/22-300x274.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5377\u5bf9\u5377\u5370\u5237\u6709\u673aFTE\u88c5\u7f6e\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>b\uff09\u5236\u9020\u7684FTE\u88c5\u7f6e\u7684\u5149\u5b66\u56fe\u50cf\uff1b<\/p>\n<p>c\uff09\u5236\u9020\u7684FTE\u8bbe\u5907\u7684\u8f93\u51fa\u529f\u7387\u5bc6\u5ea6\uff0c\u5176\u4e2d\u63d2\u56fe\u663e\u793aFTE\u8bbe\u5907\u662f\u7075\u6d3b\u7684\uff1b<\/p>\n<p>d\uff09\u7c7b\u4f3c\u624b\u956f\u7684\u65e0\u673a\u57faFTE\u88c5\u7f6e\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>e\uff09\u5236\u9020\u7684\u5668\u4ef6\u7684\u8f93\u51fa\u529f\u7387\u548c\u7535\u538b\uff0c\u5c3a\u5bf8\u4e3a156 mm\u00d716 mm\u3002<\/p>\n<p><strong>\u56fe23 \u03c0\u578b\u67d4\u6027\u70ed\u7535\uff08FTE\uff09\u88c5\u7f6e\uff0c\u5177\u6709\u81ea\u6211\u4fee\u590d\u7684\u6db2-\u91d1\u4e92\u8fde<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177563 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/23.png\" alt=\"\" width=\"700\" height=\"724\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/23.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/23-290x300.png 290w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5177\u6709\u81ea\u4fee\u590d\u6db2\u6001\u91d1\u5c5e\u4e92\u8fde\u7684\u03c0\u578b\u7ed3\u6784\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>b-d\uff09\u5236\u9020\u7684\u88c5\u7f6e\u7684\u6a2a\u622a\u9762\u56fe\u50cf\uff0c\u5176\u663e\u793a\u51fa\u5408\u7406\u7684\u7075\u6d3b\u6027\uff0c\u5176\u4e2d\u6db2\u6001\u91d1\u5c5e\u4e92\u8fde\u5668\u7531\u7ea2\u8272\u865a\u7ebf\u5f3a\u8c03\uff1b<\/p>\n<p>e\uff09\u591a\u6b21\u5f2f\u66f2\u5faa\u73af\u540e\u7684\u975e\u7b80\u5e76\u7535\u963b\u7387\uff08\u03a9\uff09\uff0c\u8bf4\u660e\u6db2\u6001\u91d1\u5c5e\u4e92\u8fde\u5668\u7684\u81ea\u6108\u5408\u529f\u80fd\uff1b<\/p>\n<p>f\uff09\u76f8\u5bf9\u4e8e\u5ba4\u6e29\u4e0b\u7684\u7a7a\u6c14\u901f\u5ea6\u6d4b\u91cf\u7684\u8f93\u51fa\u7535\u538b\u548c\u529f\u7387\u3002 \u63d2\u56fe\u663e\u793a\u4e86\u8bbe\u5907\u5982\u4f55\u8fde\u63a5\u5230\u4eba\u7684\u624b\u8155\u3002<\/p>\n<p><strong>\u56fe24\u00a0 Y\u578b\u67d4\u6027\u70ed\u7535\uff08FTE\uff09\u88c5\u7f6e\uff0c\u5177\u6709\u6a2a\u5411\u5355\u5143\u548c\u5782\u76f4\u70ed\u6d41<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177564 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/24.png\" alt=\"\" width=\"700\" height=\"677\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/24.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/24-300x290.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09Y\u578b\u7ed3\u6784\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>b\uff09\u5f53\u5468\u56f4\u73af\u5883\u6e29\u5ea6\u4e3a288K\u65f6\uff0c\u5177\u6709\u4e0d\u540c\u65bd\u52a0\u6e29\u5ea6\u7684\u5f00\u8def\u7535\u538b\u548c\u8f93\u51fa\u529f\u7387\u5bc6\u5ea6\uff1b<\/p>\n<p>c\uff09Y\u578bFTE\u88c5\u7f6e\u7684\u5236\u9020\u8fc7\u7a0b\uff1b<\/p>\n<p>d\uff0ce\uff09\u5177\u6709\u5408\u7406\u67d4\u97e7\u6027\u7684\u6240\u5236\u5907\u7684Y\u578b\u88c5\u7f6e\u7684\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe25 \u5377\u8d77\u7684\u67d4\u6027\u70ed\u7535\uff08FTE\uff09\u88c5\u7f6e\uff0c\u5e26\u6709\u677f\u576fTE\u817f\u548c\u7ba1\u72b6TE\u817f<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177565 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/25.png\" alt=\"\" width=\"700\" height=\"698\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/25.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/25-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/25-300x300.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5177\u6709Bi2Te3-\u73af\u6c27\u6811\u8102\u7684\u793a\u610f\u6027\u5377\u8d77\u7ed3\u6784\uff08n\u578b\uff09\u548cSb2Te3-\u73af\u6c27\uff08p\u578b\uff09TE\u817f\u5728\u67d4\u8f6f\u7684\u805a\u9170\u4e9a\u80fa\u57fa\u5e95\u4e0a\uff1b<\/p>\n<p>b\uff09\u6d4b\u91cf\u7684\u7535\u538b\u548c\u529f\u7387\u76f8\u5bf9\u4e8e1 cm<sup>2<\/sup>\u5377\u8d77\u7684FTE\u8bbe\u5907\u7684\u7535\u6d41\u3002\u63d2\u56fe\u4e2d\u793a\u51fa\u4e86\u5236\u9020\u7684\u88c5\u7f6e\u7684\u7167\u7247\uff1b<\/p>\n<p>c\uff09\u5177\u6709\u7ba1\u72b6TE\u817f\u7684\u793a\u610f\u6027\u5377\u8d77\u7ed3\u6784\uff1b<\/p>\n<p>d\uff0ce\uff09\u6240\u5236\u5907\u7684\u5355\u4e2a\u81ea\u52a8\u6eda\u52a8TE\u817f\u548c\u76f8\u5e94\u7684FTE\u88c5\u7f6e\u7684\u5149\u5b66\u7167\u7247\uff1b<\/p>\n<p>f\uff09\u5728\u4e0d\u540c\u6e29\u5ea6\u4e0b\u5177\u6709\u5404\u79cdTE\u5355\u5143\u7684\u8bbe\u5907\u8f93\u51fa\u529f\u7387\u3002<\/p>\n<p><strong>\u56fe26 \u91c7\u7528\u73bb\u7483\u7ea4\u7ef4\u7684\u67d4\u6027\u70ed\u7535\uff08FTE\uff09\u88c5\u7f6e<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177566 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/26.png\" alt=\"\" width=\"700\" height=\"753\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/26.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/26-279x300.png 279w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u4e0e\u751f\u4ea7\u73bb\u7483\u7ea4\u7ef4FTE\u88c5\u7f6e\u76f8\u5173\u7684\u5236\u9020\u5de5\u827a\uff1b<\/p>\n<p>b\uff09\u57fa\u4e8e\u73bb\u7483\u7ea4\u7ef4\u7684FTE\u8bbe\u5907\u7684\u56fe\u50cf\uff1b<\/p>\n<p>c\uff09\u8fde\u63a5\u5230\u4eba\u624b\u8155\u7684FTE\u88c5\u7f6e\uff0c\u5df2\u663e\u793a\u5728288K\u5468\u56f4\u73af\u5883\u4e0b\u4ea7\u751f2.9mV\u7684\u5f00\u8def\u8f93\u51fa\u7535\u538b\uff1b<\/p>\n<p>d\uff09\u5404\u79cd\u6e29\u5dee\u7684\u5668\u4ef6\u8f93\u51fa\u7535\u538b\u548c\u529f\u7387\u5bc6\u5ea6\u3002<\/p>\n<p><strong>\u56fe27 \u7ed3\u5408\u7eba\u7ec7\u7ea4\u7ef4\u7684\u67d4\u6027\u70ed\u7535\uff08FTE\uff09\u88c5\u7f6e<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177567 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/27.png\" alt=\"\" width=\"700\" height=\"580\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/27.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/27-300x249.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u57fa\u4e8e\u7eba\u7ec7\u54c1\u7684FTE\u88c5\u7f6e\u7684\u793a\u610f\u56fe\uff0c\u5176\u4e2dTE\u5355\u5143\u88ab\u5206\u914d\u5230\u7ec7\u7269\u7684\u95f4\u9699\u4e2d\uff1b<\/p>\n<p>b\uff09FTE\u8bbe\u5907\u7684\u56fe\u50cf\uff0c\u5176\u4e2dTE\u5355\u5143\u548c\u5bfc\u7535\u7ebf\u88ab\u7a81\u51fa\u663e\u793a\uff1b<\/p>\n<p>c\uff09\u9488\u5bf9\u4e0d\u540c\u6e29\u5ea6\u5dee\u83b7\u5f97\u7684\u8f93\u51fa\u7535\u538b\u548c\u529f\u7387\u3002 \u63d2\u56fe\u663e\u793a\u4e86\u6d4b\u91cf\u8bbe\u7f6e\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>d\uff09\u4ece\u4eba\u4f53\u80f8\u90e8\u6536\u96c6\u70ed\u80fd\u7684TE\u670d\u88c5\u7684\u56fe\u793a\u3002<\/p>\n<p><strong>\u56fe28 \u4e00\u79cd\u67d4\u8f6f\u7684\u70ed\u7535\uff08FTE\uff09\u88c5\u7f6e<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177568 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/28.png\" alt=\"\" width=\"700\" height=\"852\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/28.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/28-246x300.png 246w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u57fa\u4e8e\u7eba\u7ec7\u54c1\u7684FTE\u88c5\u7f6e\u7684\u793a\u610f\u56fe\uff0c\u5176\u4e2d\u7eba\u7ec7\u54c1\u7ea4\u7ef4\u5145\u5f53TE\u5355\u5143\u5e76\u4e14\u5b83\u4eec\u88ab\u5145\u5206\u5730\u4f53\u73b0\u5728\u7528\u4f5c\u95f4\u9694\u7269\u7684\u7ec7\u7269\u4e2d\uff1b<\/p>\n<p>b\uff09\u5177\u6709\u5939\u5c42\u7ed3\u6784\u7684FTE\u88c5\u7f6e\u7684\u5236\u9020\u8fc7\u7a0b\u548c\u76f8\u5e94\u7684\u56fe\u50cf\uff1b<\/p>\n<p>c\uff0cd\uff09\u5728\u5404\u79cd\u6e29\u5dee\u4e0b\u5177\u6709\u4e0d\u540c\u6570\u91cfTE\u5355\u5143\u7684\u5236\u9020\u8bbe\u5907\u7684\u8f93\u51fa\u7535\u538b\u548c\u529f\u7387\u3002<\/p>\n<p><strong>\u56fe29 \u4e00\u79cd\u5177\u6709\u5355\u817f\u7ed3\u6784\u7684\u67d4\u6027\u70ed\u7535\uff08FTE\uff09\u88c5\u7f6e<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177569 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/29.png\" alt=\"\" width=\"700\" height=\"770\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/29.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/29-273x300.png 273w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>a\uff09\u5177\u6709\u5355\u817f\u7ed3\u6784\u7684\u6ce2\u72b6FTE\u88c5\u7f6e\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>b\uff09\u5177\u6709\u5355\u817f\u7ed3\u6784\u7684\u5377\u8d77\u5f0fFTE\u88c5\u7f6e\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>c\uff09\u5177\u6709\u5355\u817f\u7ed3\u6784\u7684\u5e76\u8054FTE\u88c5\u7f6e\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe30 \u9ad8\u6027\u80fdFTE\u5907\u7528\u6750\u6599\u548c\u8bbe\u5907\u7684\u6218\u7565\u53ca\u524d\u666f<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-177570 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/30.png\" alt=\"\" width=\"700\" height=\"699\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/30.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/30-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/06\/30-300x300.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>&nbsp;<\/p>\n<p><strong>\u3010\u7ed3\u8bba\u548c\u5c55\u671b\u3011<\/strong><\/p>\n<p>\u7814\u7a76\u4eba\u5458\u6307\u51fa\u4e86\u672a\u6765\u7814\u7a76\u5f00\u53d1\u9ad8\u6027\u80fdFTE\u6750\u6599\u548c\u5668\u4ef6\u7684\u51e0\u4e2a\u524d\u666f\uff0c\u5982\u56fe30\u6240\u793a\uff0c\u8fd9\u4e9b\u603b\u7ed3\u5982\u4e0b\uff1a<\/p>\n<ul>\n<li>\u5c06\u5bfc\u7535\u805a\u5408\u7269\u4e2d\u7684\u8f7d\u4f53\u79bb\u5fc3\uff0c\u5e76\u5728\u7406\u8bba\u4e0a\u5efa\u7acb\u89e3\u91ca\u8f7d\u6d41\u5b50\u4f20\u8f93\u6027\u8d28\u7684\u6a21\u578b\u3002\u5bfc\u7535\u805a\u5408\u7269\u4e2d\u7684\u8f7d\u4f53\u5927\u90e8\u5206\u662f\u5c40\u90e8\u7684\uff0c\u5e76\u4e14\u53ea\u6709\u6709\u9650\u7684\u90e8\u5206\u53ef\u4ee5\u901a\u8fc7\u5185\u90e8\u4e2d\u95f4\u5c42\u8f93\u9001\u3002<\/li>\n<li>\u901a\u8fc7\u754c\u9762\u5de5\u7a0b\u7406\u89e3\u548c\u4f18\u5316\u586b\u6599\u7684\u6548\u679c\u3002\u754c\u9762\u5904\u6548\u5e94\u4f1a\u663e\u8457\u5f71\u54cd\u8f7d\u4f53\u7684\u754c\u9762\u4f20\u8f93\uff0c\u5bf9\u5176\u673a\u5236\u7684\u6df1\u5165\u4e86\u89e3\u53ef\u4ee5\u6307\u5bfc\u586b\u6599\u7684\u9009\u62e9\u548c\u5904\u7406\u3002<\/li>\n<li>\u5b9a\u4f4d\u5206\u5e03\u5e76\u52a0\u5f3a\u65e0\u673a\u9897\u7c92\u4e4b\u95f4\u7684\u8fde\u63a5\uff0c\u4ee5\u83b7\u5f97\u9ad8\u5ea6\u7ed3\u6676\u7684\u7ea4\u7ef4\u3002\u9664\u8584\u819c\u8d28\u91cf\u5916\uff0c\u65e0\u673a\u8584\u819c\u4e2d\u7684\u8f7d\u4f53\u4f20\u8f93\u53ef\u80fd\u53d7\u5230\u968f\u673a\u5206\u5e03\u7684\u9897\u7c92\u53ca\u5176\u5f31\u76f8\u90bb\u8fde\u63a5\u7684\u9650\u5236\uff0c\u8fd9\u589e\u5f3a\u4e86\u76f8\u90bb\u9897\u7c92\u4e4b\u95f4\u8f7d\u6d41\u5b50\u4f20\u8f93\u7684\u80fd\u91cf\u969c\u788d\uff0c\u8fdb\u800c\u4f7f\u03c3\u6076\u5316\u3002<\/li>\n<li>\u5339\u914d\u70ed\u6e90\u548cFTE\u8bbe\u5907\u4e4b\u95f4\u7684\u70ed\u963b\uff0c\u4ee5\u53ca\u901a\u8fc7\u5fae\u52a0\u5de5\u514b\u670d\u65e0\u673aTE\u817f\u7684\u673a\u68b0\u7075\u6d3b\u6027\u3002\u4e3a\u4e86\u5339\u914d\u70ed\u6e90\uff0c\u53ef\u4ee5\u901a\u8fc7\u4f18\u5316\u5668\u4ef6\u5c3a\u5bf8\u548c\u51e0\u4f55\u7ed3\u6784\u6765\u8c03\u6574FTE\u5668\u4ef6\u7684\u70ed\u963b\uff0c\u5176\u4e2d\u6709\u9650\u5143\u5206\u6790\u53ef\u4ee5\u6709\u6548\u5730\u9884\u6d4b\u76f8\u5e94\u7684\u70ed\u963b\u3002\u901a\u8fc7\u5c06\u5fae\u578b\u65e0\u673aTE\u817f\u7ed3\u5408\u5230\u67d4\u6027\u57fa\u677f\u4e2d\uff0c\u5fae\u52a0\u5de5\u53ef\u80fd\u662f \u514b\u670d\u65e0\u673aTEs\u673a\u68b0\u6027\u80fd\u7684\u6709\u6548\u65b9\u6cd5\u3002<\/li>\n<\/ul>\n<p>&nbsp;<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/full\/10.1002\/adma.201807916\">Flexible Thermoelectric Materials and Generators: Challenges and Innovations<\/a> (Adv. Mater.\uff0c2019\uff0cDOI: 10.1002\/adma.201807916)<\/p>\n<p>\u9648\u5fd7\u521a\u6559\u6388\u662f\u6fb3\u5927\u5229\u4e9a\u5357\u6606\u58eb\u5170\u5927\u5b66\u529f\u80fd\u6750\u6599\u5b66\u79d1\u5e26\u5934\u4eba\u3002\u957f\u671f\u4ece\u4e8b\u529f\u80fd\u6750\u6599\u5728\u80fd\u91cf\u8f6c\u5316\u7684\u57fa\u7840\u548c\u5e94\u7528\u7814\u7a76\u3002\u4ee5\u91d1\u5c5e\u6c27\u786b\u65cf\u5316\u5408\u7269\u4e3a\u7814\u7a76\u5207\u5165\u70b9\uff0c\u901a\u8fc7\u63a7\u5236\u6750\u6599\u7684\u6676\u4f53\u7ed3\u6784\u3001\u5c3a\u5bf8\u3001\u548c\u63ba\u6742\u6539\u6027\u6765\u8c03\u63a7\u5176\u5149\uff0c\u7535\uff0c\u5316\u5b66\u7279\u6027\u3002\u5f00\u53d1\u4e86\u6027\u80fd\u4f18\u8d8a\u7684\u70ed\u7535\u6750\u6599\uff0c\u5e76\u901a\u8fc7\u80fd\u5e26\u52a0\u5de5\u548c\u5fae\u89c2\u7ed3\u6784\u63a7\u5236\uff0c\u5b9e\u73b0\u4e86\u70ed\u7535\u6027\u80fd\u7684\u63d0\u5347\uff0c\u4e3a\u53d1\u5c55\u65b0\u7684\u5de5\u4e1a\u5e9f\u70ed\u53d1\u7535\u63d0\u4f9b\u65b0\u7684\u5e94\u7528\u5e73\u53f0\uff1b\u901a\u8fc7\u5bf9\u91d1\u5c5e\u6c27\u786b\u65cf\u5316\u5408\u7269\u8868\u9762\u4f20\u8f93\u7279\u6027\u7684\u7406\u89e3\u548c\u7814\u5236\uff0c\u5f00\u53d1\u4e86\u65b0\u4e00\u4ee3\u7684\u72c4\u62c9\u514b\u534a\u91d1\u5c5e\u6750\u6599\uff0c\u4e3a\u5f00\u53d1\u65b0\u4e00\u4ee3\u7535\u5b50\u6750\u6599\u63d0\u4f9b\u65b0\u7684\u7814\u7a76\u5e73\u53f0\u3002\u9648\u5fd7\u521a\u6559\u6388\u5e08\u4ece\u6210\u4f1a\u660e\u9662\u58eb\u548c\u902f\u9ad8\u6e05\u9662\u58eb\u30022008\u5e74\u535a\u58eb\u6bd5\u4e1a\u540e\u5728\u6fb3\u5927\u5229\u4e9a\u6606\u58eb\u5170\u5927\u5b66\u673a\u68b0\u4e0e\u77ff\u4e1a\u5b66\u9662\u5de5\u4f5c\uff0c\u5148\u540e\u62c5\u4efb\u7814\u7a76\u5458\uff0c\u9ad8\u7ea7\u7814\u7a76\u5458\uff0c\u8363\u8a89\u526f\u6559\u6388\uff0c\u540e\u8f6c\u5165\u6fb3\u5927\u5229\u4e9a\u5357\u6606\u58eb\u5170\u5927\u5b66\u62c5\u4efb\u6559\u6388\uff0c\u529f\u80fd\u6750\u6599\u5b66\u79d1\u5e26\u5934\u4eba\uff0c\u5148\u540e\u4e3b\u6301\u5171\u8ba1\u4e03\u767e\u4e07\u6fb3\u5143\u7684\u79d1\u7814\u9879\u76ee\uff0c\u5176\u4e2d\u5305\u62ec6\u9879\u6fb3\u5927\u5229\u4e9a\u7814\u7a76\u59d4\u5458\u4f1a\u30011\u9879\u6fb3\u5927\u5229\u4e9a\u79d1\u5b66\u9662\u30012\u9879\u5dde\u653f\u5e9c\u300110\u9879\u5de5\u4e1a\u9879\u76ee\u548c8\u9879\u6821\u7ea7\u7684\u79d1\u7814\u9879\u76ee\u3002\u5728\u6606\u58eb\u5170\u5927\u5b66\u548c\u5357\u6606\u58eb\u5170\u5927\u5b66\u5de5\u4f5c\u671f\u95f4\uff0c\u5171\u6307\u5bfc17\u540d\u535a\u58eb\u751f\u548c3\u540d\u7855\u58eb\u7814\u7a76\u751f\uff0c\u5176\u4e2d\u5df2\u6bd5\u4e1a\u535a\u58eb\u751f5\u540d\u548c\u7855\u58eb\u751f2\u540d\u3002\u5171\u5728Nat. Nanotech. \uff081\u7bc7\uff09\u3001 Nat. Commun. \uff083\u7bc7\uff09\u3001 Prog. Mater. Sci. \uff081\u7bc7\uff09\u3001 Adv. Mater. \uff087\u7bc7\uff09\u3001 J. Am. Chem. Soc. \uff083\u7bc7\uff09\u3001Angew. Chem. Int. Edit.,\uff082\u7bc7\uff09, Nano Lett. \uff083\u7bc7\uff09\u3001Energy Environ. Sci. \uff081\u7bc7\uff09\u3001ACS Nano\uff0813\u7bc7\uff09\u3001Adv. Energy Mater. \uff087\u7bc7\uff09\u3001Adv. Funct. Mater. \uff088\u7bc7\uff09\u3001Nano Energy\uff086\u7bc7\uff09\u548c Energy Storage Mater. \uff081\u7bc7\uff09\u7b49\u56fd\u9645\u5b66\u672f\u671f\u520a\u4e0a\u53d1\u8868200\u4f59\u7bc7\u5b66\u672f\u8bba\u6587\u3002\u8fd9\u4e9b\u8bba\u6587\u5171\u88abScopus\u5f15\u752810600\u4f59\u6b21\uff0cH-index\u8fbe\u523052\u3002<\/p>\n<p>&nbsp;<\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u9ad8\u5206\u5b50\u5b66\u672f\u7ec4\u6c34\u624b\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u7f16\u8f91\u6574\u7406\u3002<\/p>\n<p>\u6750\u6599\u725b\u7f51\u4e13\u6ce8\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u53ca\u884c\u4e1a\u8fdb\u5c55\uff0c\u8fd9\u91cc\u6c47\u96c6\u4e86\u5404\u5927\u9ad8\u6821\u7855\u535a\u751f\u3001\u4e00\u7ebf\u79d1\u7814\u4eba\u5458\u4ee5\u53ca\u884c\u4e1a\u4ece\u4e1a\u8005\uff0c\u5982\u679c\u60a8\u5bf9\u4e8e\u8ddf\u8e2a\u6750\u6599\u9886\u57df\u79d1\u6280\u8fdb\u5c55\uff0c\u89e3\u8bfb\u9ad8\u6c34\u5e73\u6587\u7ae0\u6216\u662f\u8bc4\u8ff0\u884c\u4e1a\u6709\u5174\u8da3\uff0c\u70b9\u6211\u52a0\u5165\u6750\u6599\u4eba\u7f16\u8f91\u90e8\u3002\u53c2\u4e0e\u9ad8\u5206\u5b50\u8bdd\u9898\u8ba8\u8bba\u6216\u4e86\u89e3\u9ad8\u5206\u5b50\u7ec4\u62db\u52df\u8be6\u60c5\uff0c\u8bf7\u52a0\u9ad8\u5206\u5b50\u4ea4\u6d41\u7fa4\uff08298064863\uff09\u3002<\/p>\n<p>\u6750\u6599\u6d4b\u8bd5\u3001\u6570\u636e\u5206\u6790\uff0c\u4e0a\u6d4b\u8bd5\u8c37\uff01<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u5982\u4eca\uff0c\u5c0f\u578b\u5316\u7684\u96c6\u6210\u7535\u5b50\u4ea7\u54c1\u8b6c\u5982\u53ef\u7a7f\u6234\u548c\u533b\u7597\u690d\u5165\u8bbe\u5907\u6b63\u5728\u84ec\u52c3\u53d1\u5c55\u3002\u7531\u4e8e\u67d4\u6027\u70ed\u7535\u6750\u6599\u548c\u88c5\u7f6e\u80fd\u591f\u901a\u8fc7\u5c06\u70ed\u91cf\u4e00\u81f4\u5730\u8fde\u63a5\u5230\u70ed\u6e90\u4e0a\u800c\u5c06\u70ed\u91cf\u76f4\u63a5\u8f6c\u6362\u6210\u7535\u80fd\uff0c\u800c\u53d7\u5230\u8d8a&#8230;<\/p>\n","protected":false},"author":3247,"featured_media":177571,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[533],"tags":[31],"class_list":["post-177544","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zongshu","tag-dianzi"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/177544"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/3247"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=177544"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/177544\/revisions"}],"predecessor-version":[{"id":177901,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/177544\/revisions\/177901"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/177571"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=177544"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=177544"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=177544"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}