{"id":179286,"date":"2019-07-15T06:30:55","date_gmt":"2019-07-14T22:30:55","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=179286"},"modified":"2019-07-14T20:37:55","modified_gmt":"2019-07-14T12:37:55","slug":"%e3%80%90ns%e7%b2%be%e8%af%bb%e3%80%91%e6%bf%80%e5%85%89%e7%85%a7%e5%b0%84mote2%ef%bc%9a%e4%b8%80%e6%ad%a5%e5%ae%8c%e6%88%90%e9%9b%86%e6%88%90%e7%94%b5%e8%b7%af%e7%9a%84%e7%a7%81%e4%ba%ba","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=179286","title":{"rendered":"\u6fc0\u5149\u7167\u5c04MoTe2\uff1a\u4e00\u6b65\u5b8c\u6210\u96c6\u6210\u7535\u8def\u7684\u201c\u79c1\u4eba\u5b9a\u5236\u201d"},"content":{"rendered":"<p>\u4e8c\u7ef4\u6750\u6599\u6784\u6210\u7684\u8303\u5fb7\u534e\u5f02\u8d28\u7ed3\u662f\u5f00\u53d1\u4e0b\u4e00\u4ee3\u7535\u5b50\u548c\u5149\u7535\u5b50\u5668\u4ef6\u7684\u7406\u60f3\u6750\u6599\uff0c\u5e76\u4e14\u5c06\u9010\u6e10\u8d70\u5411\u4e8c\u7ef4\u5668\u4ef6\u96c6\u6210\u7535\u8def\u3002\u4f46\u5236\u4f5c\u4e8c\u7ef4\u6750\u6599\u7684\u534a\u5bfc\u4f53\u96c6\u6210\u7535\u8def\u662f\u975e\u5e38\u8270\u8f9b\u7684\u3002\u76ee\u524d\u5e38\u7528\u7684\u5236\u9020\u8303\u5fb7\u534e\u5f02\u8d28\u7ed3\u7684\u65b9\u6cd5\u6709\u4e24\u79cd\uff0c\u4f46\u662f\u90fd\u6709\u5176\u5c40\u9650\u6027\u3002<\/p>\n<p>1.\u7528\u4e24\u79cd\u6750\u6599\u7cbe\u786e\u8f6c\u79fb\u5f62\u6210\u5f02\u8d28\u7ed3\uff1a\u4e0d\u53ef\u6269\u5c55\uff0c\u96be\u7528\u4e8e\u5927\u9762\u79ef\u5236\u9020\uff1b<\/p>\n<p>2.\u84b8\u6c7d\u6216\u6eb6\u89e3\u76f8\u63ba\u6742\u5f62\u6210\u540c\u8d28\u7ed3\uff1a\u901a\u5e38\u662f\u5168\u5c40\u63ba\u6742\uff0c\u63a7\u5236\u6709\u9650\u3002<\/p>\n<p>\u6240\u4ee5\uff0c\u60f3\u8981\u8fbe\u5230\u50cf\u5728CMOS\u52a0\u5de5\u4e2d\u65f6\u7684\u79bb\u5b50\u6ce8\u5165\u4e00\u6837\u7684\u6548\u679c\uff0c\u4e00\u79cd\u7b80\u5355\u3001\u5b9e\u7528\u3001\u53ef\u7cbe\u786e\u63a7\u5236\u7684\u5c40\u90e8\u63ba\u6742\u65b9\u5f0f\u975e\u5e38\u91cd\u8981\u3002<\/p>\n<p>\u97e9\u56fd\u6d66\u9879\u79d1\u6280\u5927\u5b66\u7684Moon-Ho Jo \u8bfe\u9898\u7ec4\u5c55\u793a\u4e86\u4e00\u79cd\u6fc0\u5149\u7167\u5c04\u7684\u65b9\u6cd5\uff0c\u5c06\u53ef\u7f16\u7a0b\u7535\u8def\u5199\u5165\u5230\u4e8c\u7ef4\u534a\u5bfc\u4f53\u53cc\u78b2\u5316\u94bc(2H-MoTe2)\u4e0a<sup>[<\/sup><sup>1]<\/sup>\uff0c\u5b8c\u6210\u4e9a\u5fae\u7c73\u5c3a\u5ea6\u4e0a\u63a7\u5236\u63ba\u6742\u3002\u4e0b\u9762\u662f\u6765\u81eaMoon-Ho Jo \u6559\u6388\u8bfe\u9898\u7ec4\u5b98\u7f51\u7684\u7167\u7247\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-179288 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724712.png\" alt=\"\" width=\"650\" height=\"241\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724712.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724712-300x111.png 300w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/> \u00a0\u00a0\u00a0\u00a0<\/p>\n<p>\u5982\u6b64\u795e\u5947\u7684\u65b9\u6cd5\u662f\u5982\u4f55\u5b9e\u73b0\uff0c\u53c8\u662f\u5982\u4f55\u4f5c\u7528\u548c\u5e94\u7528\u5462\uff1f<\/p>\n<p><strong>1\u3001\u6211\u662f\u5668\u4ef6\u6784\u7b51\u5206\u754c\u7ebf<\/strong><\/p>\n<p>\u9996\u5148\uff0cN\u578b\u76842H-MoTe2\u901a\u9053\u88ab\u8bbe\u8ba1\u6210\u5404\u79cd\u5f62\u72b6\uff0c\u5e76\u901a\u8fc7\u4f7f\u7528\u5149\u523b\u80f6\u63a9\u6a21\u548cCF<sub>4<\/sub>\u7b49\u79bb\u5b50\u4f53\u523b\u8680\u3002\u7136\u540e\u8fdb\u884c\u7535\u6781\u9635\u5217\u6c89\u79ef(Cr 1 nm\/Au 20 nm)\uff0c\u4ece\u800c\u5728\u573a\u6548\u5e94\u6676\u4f53\u7ba1(FET)\u51e0\u4f55\u7ed3\u6784\u4e2d\u4ea7\u751f\u591a\u4e2a\u901a\u9053\u3002\u6700\u540e\uff0c\u752820mW\u7684532\u6fc0\u5149\u675f\u7167\u5c04\u57282H-MoTe<sub>2<\/sub>\u4e0a\u7684\u91d1\u7535\u6781\uff0c\u5c31\u5b8c\u6210\u4e86\u5668\u4ef6\u5c40\u90e8p\u63ba\u548cp-n\u7ed3\u7684\u6784\u7b51\uff0c\u5982\u56fe1a\u3002<\/p>\n<p><strong>\u56fe1<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-179289 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724713.png\" alt=\"\" width=\"620\" height=\"437\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724713.png 620w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724713-300x211.png 300w\" sizes=\"(max-width: 620px) 100vw, 620px\" \/><\/p>\n<p>\u56fe1b\u4e2d\u7684\u5668\u4ef6\u5728\u5927\u6c14\u6761\u4ef6\u4e0b\uff0c\u6cbf\u63a5\u89e6\u7535\u67811\u548c2\u4e0a\u7684\u7eff\u8272\u865a\u7ebf\u9009\u62e9\u6027\u6fc0\u5149\u626b\u63cf30\u79d2\u3002<\/p>\n<p>\u56fe1-b\u4e2d\u4e0d\u540c\u7535\u6781\u4e4b\u95f4\u6240\u6d4b\u5f97\u7684\u8f93\u51fa\u66f2\u7ebfc\u548c\u8f6c\u79fb\u66f2\u7ebfd\u53ef\u4ee5\u9a8c\u8bc1\u5bf9MoTe2\u6750\u6599p\u63ba\u7684\u6548\u679c\u30023 \u2013 4\uff08\u9ed1\u8272\u66f2\u7ebf\uff09\u63a5\u89e6\u7684\u901a\u9053\u662f\u539f\u59cb2H-MoTe2\uff0c\u663e\u793an\u578b\u7279\u5f81\uff1b1-2\uff08\u84dd\u8272\u66f2\u7ebf\uff09\u63a5\u89e6\u7684\u901a\u9053\u662fp\u63ba\u6742\u5904\u7406\u4f4d\u7f6e\uff0c\u663e\u793a\u51fa\u7535\u5b66\u6027\u80fd\u7684\u964d\u4f4e\u548c\u660e\u663ep-\u578b\u7279\u5f81\uff1b2-3\uff08\u7ea2\u7ebf\uff09\u5728\u8f93\u51fa\u66f2\u7ebf\u4e2d\u663e\u793a\u5f3a\u6574\u6d41\u6027\uff0c\u8868\u660e\u5176\u4e2d\u5f62\u6210\u4e86p-n\u7ed3\u3002\u5229\u7528\u4e8c\u6781\u7ba1\u62df\u5408\u548c\u626b\u63cf\u5149\u7535\u6d41\u6210\u50cf\u6280\u672f\u5206\u6790\u4e86p-n\u7ed3\u7684\u5b58\u5728\u6027\u5e76\u83b7\u5f971.0 eV\u7684Eg\u503c(\u8865\u5145\u56fe1)\u3002\u56fe1 e\u662f\u9759\u6001\u7167\u5c04MoTe<sub>2<\/sub>\u901a\u9053\u8bf1\u5bfc\u63ba\u6742\u7684\u7ed3\u679c\uff0c\u4ea7\u751f\u540c\u6837\u7c7b\u4f3c\u5730\u63ba\u6742\u5f71\u54cd\u3002<strong><b>\u6240\u4ee5\uff0c\u65e0\u8bba\u662f\u76f4\u63a5\u7167\u5c04\uff0c\u8fd8\u662f\u7167\u5c04\u5728\u7535\u6781\u4e0a\uff0c\u90fd\u80fd\u591f\u4ea7\u751fp\u63ba\u7684\u6548\u679c\u3002<\/b><\/strong><\/p>\n<p><strong><b>\u90a3\u4e482<\/b><\/strong><strong><b>H<\/b><\/strong><strong><b>&#8211;<\/b><\/strong><strong><b>M<\/b><\/strong><strong><b>o<\/b><\/strong><strong><b>T<\/b><\/strong><strong><b>e2\u901a\u9053\u4e2d\u91d1\u7535\u6781\u5728\u5149\u7167\u4e0b\u7684\u4f5c\u7528\u662f\u4ec0\u4e48\u5462\uff1f<\/b><\/strong>\u91d1\u5177\u6709\u66f4\u9ad8\u7684\u70ed\u5bfc\u7387\uff08\u6bd4MoTe<sub>2<\/sub>\u9ad8100\u500d\u5de6\u53f3\uff09\uff0c\u56e0\u6b64\u5728\u8fd9\u91cc\u662f\u4f5c\u4e3a\u539f\u4f4d\u5149\u7167\u4ea7\u751f\u70ed\u91cf\u7684\u51e0\u4f55\u5bfc\u5411\uff08geometrical guide\uff09\u3002\u90a3\u53c8\u662f\u4e3a\u4ec0\u4e48532\u6fc0\u5149\u675f\u80fd\u591f\u8d77\u5230\u8fd9\u6837\u7684\u63ba\u6742\u4f5c\u7528\u5462\uff1f<\/p>\n<p><strong>2\u3001\u6211\u662f\u673a\u7406\u89e3\u91ca\u5206\u754c\u7ebf<\/strong><\/p>\n<p>\u4f5c\u8005\u901a\u8fc7\u626b\u63cf\u96a7\u9053\u663e\u5fae\u955c\u548c\u5149\u8c31\u5b66(STM\/STS)\u89c2\u5bdf\u5fae\u533a\u7f3a\u9677\u548c\u5c40\u90e8\u5fae\u5206\u7535\u5bfc\uff0c\u8bf4\u660e\u548c\u9a8c\u8bc1p\u578b\u63ba\u6742\u7684\u673a\u7406\u3002<\/p>\n<p><strong>\u56fe2<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-179290 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724714.png\" alt=\"\" width=\"555\" height=\"483\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724714.png 555w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724714-300x261.png 300w\" sizes=\"(max-width: 555px) 100vw, 555px\" \/><\/p>\n<p>\u56fe2b\u662f\u539f\u59cb\u7684STM\u56fe\uff08\u4e0e\u7167\u5c04\u533a\u57df\u7684\u4f4d\u7f6e\u8ddd\u79bb\u5927\u4e8e300\u03bcm),\u53d1\u73b0\u4e86\u539f\u5b50\u5438\u9644\uff08adatom\uff09\u7f3a\u9677\u548cTe\u7a7a\u4f4d\u7f3a\u9677\u70b9\u3002\u6307\u5b9a\u539f\u5b50\u5438\u9644\u4e3aA\u578b\u7f3a\u9677\uff0c\u5982\u56fe2c\uff0c\u8fd9\u79cd\u5438\u9644\u7684\u539f\u5b50\u5728\u4e3b\u6676\u683c\u7684Te\u4f4d\u70b9\u5468\u56f4\u5448\u73b0\u4e09\u89d2\u5f62\u7a81\u51fa\u7269\u5f62\uff0c\u9ad8\u5ea6\u7ea62a (\u8865\u5145\u56fe8)\u3002A\u578b\u7f3a\u9677\u662f\u9488\u5c16\u626b\u63cf\u671f\u95f4\u4ea7\u751f\u7684\u539f\u5b50\u8fc1\u79fb\u548c\u5438\u9644\uff0c\u6240\u4ee5\u63a8\u6d4b\u662f\u8d85\u9ad8\u771f\u7a7a\u4e0b\u7ecf\u5e38\u51fa\u73b0\u7684H\u539f\u5b50\u3002\u8fd9\u4e24\u79cd\u7f3a\u9677\u90fd\u662f\u56fa\u6709\u7f3a\u9677\uff0c\u5c31\u662f\u65e0\u5149\u7167\u5c31\u5e26\u6709\u7684\u3002\u5c40\u90e8\u5fae\u5206\u7535\u5bfc(dI \/ dV)\u4ee3\u8868\u7740\u6001\u5bc6\u5ea6(LDOS)\u3002A\u578b\u7f3a\u9677\u7684\u5c40\u90e8\u5fae\u5206\u7535\u5bfc\uff0c\u5982\u56fe2d\u4e2d\u7ea2\u7ebf\uff0c\u663e\u793a\u4e86V = &#8211; 0.6 V\u5904\u7684\u4e2d\u95f4\u9699\u72b6\u6001\uff0c\u5e76\u5e26\u6709\u4e00\u4e2a\u4e0b\u79fb\u7684\u4ef7\u5e26\u6700\u5927\u503c(VBM)\u3002\u6362\u53e5\u8bdd\u8bf4\uff0cA\u578b\u7f3a\u9677\u5728\u5bbf\u4e3b\u6676\u683c\u4e2d\u5145\u5f53\u7535\u5b50\u4f9b\u4f53\u3002<\/p>\n<p>\u56fe2e\u4e3a\u7167\u5c04\u70b9\u9644\u8fd1\u7684STM\u56fe\u3002\u7ea2\u8272\u3001\u7eff\u8272\u548c\u84dd\u8272\u65b9\u5757\u5206\u522b\u8868\u793a\u5438\u9644\u539f\u5b50\u7f3a\u9677\u3001\u94bc\u7a7a\u4f4d\u548c\u56e2\u7c07\u7f3a\u9677\u3002Mo\u7a7a\u4f4d\u7684\u539f\u5b50\u5206\u8fa8\u5f62\u8c8c\u662f\u5728Mo\u4f4d\u70b9\u9644\u8fd1\u6709\u4e00\u4e2a\u660e\u663e\u7684\u5751\uff0c\u6307\u5b9a\u4e3a<strong><b>B\u578b\u7f3a\u9677<\/b><\/strong>\uff08\u56fe2f\uff09\u3002B\u578b\u7f3a\u9677\u662f\u5149\u8bf1\u5bfc\u7684\u52a0\u70ed\u4ea7\u751f\u7684\u8fc7\u6e21\u91d1\u5c5e\u70b9\u7a7a\u4f4d\u3002dI\/dV\u5728B\u578b\u7f3a\u9677\u4f4d\u70b9\u7684\u503c\u4e0e\u539f\u59cb\u76842H-MoTe2\u76f8\u4f3c(\u56fe2g)\uff0c\u8fd9\u8868\u660eB\u578b\u7f3a\u9677\u4e0d\u662f\u4e00\u4e2a\u6d3b\u6027\u63ba\u6742\u7269\u3002\u56e2\u7c07\u7f3a\u9677\u5728STM\u56fe\u4e2d\u89c2\u5bdf\u5230\u5468\u56f4\u6709\u8f83\u5927\u7684\u6ce2\u7eb9(\u9ad8\u5ea6~5 &#8211; 7a\uff0c\u534a\u5f84~2 nm)\uff0c\u65e0\u7279\u6b8a\u7684\u539f\u5b50\u7279\u5f81(\u56fe2h)\uff0c\u6307\u5b9a\u4e3a<strong><b>C\u578b\u7f3a\u9677<\/b><\/strong>\u3002C\u578b\u7f3a\u9677\u4f4d\u7f6e\u7684LDOS\u5411\u672a\u5360\u636e\u72b6\u6001\u663e\u793a\u4e86\u7ea60.5 eV\u7684\u5b9e\u8d28\u6027\u6f5c\u5728\u504f\u79fb(\u56fe2i)\u3002\u6cbfH\u4e2d\u7684\u865a\u7ebf\u7bad\u5934\u7ed8\u5236\u6240\u6709dI\/dV\u66f2\u7ebf\u5728\u539f\u5b50\u5c3a\u5ea6\u4e0a\u6355\u83b7\u4e86CBM\u548cVBM\u4f4d\u7f6e\u7684\u5c40\u90e8\u53d8\u5316\u4ee5\u53ca\u5e26\u8fb9\u5c3e\u8ff9\u3002\u53ef\u4ee5\u8bf4\uff0cC\u578b\u7f3a\u9677\u662f\u5bbf\u4e3bMoTe2\u6676\u683c\u4e2d\u7684\u7535\u5b50\u53d7\u4f53\uff0c\u662f\u5e26\u7535\u8377\u7684\u5438\u9644\u6c27\u539f\u5b50\u56e2\u7c07\u3002<\/p>\n<p><strong><b>\u6572\u9ed1\u677f\uff0c\u5212\u91cd\u70b9\u4e86\uff01\uff01\uff01 <\/b><\/strong><\/p>\n<p>\u6240\u4ee5\uff0c\u6c9f\u9053\u5728\u5149\u7167\u540e\u7684p\u578b\u63ba\u6742\u5927\u90e8\u5206\u662f\u56e0\u4e3a\u6c27\u539f\u5b50\u5728\u5149\u7167\u8fc7\u7a0b\u4e2d\u6269\u6563\u5230\u8303\u5fb7\u534e\u5c42\u95f4\u95f4\u9699\u4e2d\u5e76\u5f62\u6210\u4e86\u6c27\u539f\u5b50\u56e2\u7c07\u3002\u6700\u8fd1\u5bc6\u5ea6\u51fd\u7406\u8bba\u8ba1\u7b97\u548c\u5b9e\u9a8c\u89c2\u5bdf\u7684\u5de5\u4f5c\u4e5f\u662f\u8ba4\u4e3a\u6c27\u5bf9TMDCs\u6765\u8bf4\u4e3ap\u578b\u63ba\u6742\u5242\uff01<\/p>\n<p><strong>3\u3001\u5feb\u901f\u53ef\u7f16\u7a0b\u7684\u63ba\u6742<\/strong><\/p>\n<p>\u5c40\u90e8p\u578b\u63ba\u6742\u662f\u7531\u4e8e\u5149\u8bf1\u5bfc\u7684n\u578b\u4e3b\u6676\u683c\u5185\u5206\u5b50-\u7a7a\u4f4d\u56e2\u7c07\u7684\u4ea7\u751f\uff0c\u6240\u4ee5\u5728\u7535\u8def\u5236\u4f5c\u8fc7\u7a0b\u4e2d\u53ef\u4ee5\u5c06\u5149\u7167\u65f6\u95f4\u4f5c\u4e3a\u4e00\u4e2a\u7b80\u5355\u7684\u5de5\u827a\u53c2\u6570\u6765\u63a7\u5236\u63ba\u6742\u7a0b\u5ea6\u3002<\/p>\n<p>\u4f5c\u8005\u9996\u5148\u5bf9\u901a\u9053\u957f\u5ea6\u548c\u539a\u5ea6\u7684\u5f71\u54cd\u8fdb\u884c\u4e86\u63a2\u7d22\u3002\u4fdd\u6301\u5149\u7167\u65f6\u95f4\u4e3a60s\uff0c\u6539\u53d8\u6c9f\u9053\u539a\u5ea6\u4e3a12.7\u30017.6\u30016.2\u548c3.2 nm\uff0c\u53ef\u4ee5\u53d1\u73b0\u5728\u8f83\u8584\u7684\u6c9f\u9053\u4e0a\uff0cp\u578b\u7279\u5f81\u9010\u6e10\u589e\u5f3a\uff0c\u5f00\/\u5173\u6bd4\u589e\u5927\u3002\uff08\u8865\u5145\u56fe12\u548c\u56fe13\uff09\u3002<\/p>\n<p>\u540c\u65f6\u4f5c\u8005\u7814\u7a76\u4e86\u4e0d\u540c\u901a\u9053\u957f\u5ea6\u7684\u5149\u7167-\u65f6\u95f4\u4f9d\u8d56\u6027\u63ba\u6742(\u56fe3a)\u548c\u970d\u5c14\u6d4b\u91cf(\u56fe3b)\u3002\u56fe3c\u4e2d,\u57281.0\u03bcm\u957f\u7684\u6c9f\u9053\u4e2d,\u7535\u963b\uff08Rsheet\uff09\u5148\u572820s\u7684\u7167\u5c04\u540e\u589e\u52a0\u00a0(\u5de6\u8fb9),\u7136\u540e\u572820-90s\u7167\u5c04\u540e\u964d\u4f4e(\u53f3\u8fb9)\u3002\u56fe3d\u7684\u8f6c\u79fb\u66f2\u7ebf\u4e5f\u663e\u793a\u51fa\u6c9f\u9053\u7684\u9010\u6e10p\u63ba\u6742\u5316\u3002\u4ece\u56fe3e\u4e2d\uff0c\u53ef\u4ee5\u770b\u51fa\u4ece0\u523090\u79d2\uff0c\u901a\u9053\u7535\u963b\u548c\u8f7d\u6d41\u5b50\u6d53\u5ea6\u968f\u5149\u7167\u65f6\u95f4\u7684\u53d8\u5316\uff0c\u540c\u65f6\u663e\u793a\u970d\u5c14\u6d4b\u91cf\u4e2d\u8f7d\u6d41\u5b50\u6d53\u5ea6\u7684\u8bef\u5dee\u8303\u56f4\u3002\u4e24\u79cd\u6d4b\u8bd5\u5171\u540c\u8bc1\u5b9e\u4e86\u5149\u7167\u524d\uff0c\u6c9f\u9053\u4e2d\u521d\u59cb\u8f7d\u6d41\u5b50\uff08\u7535\u5b50\uff09\u6d53\u5ea6\u5728\u4e3a2.5\u2009\u00d7\u200910<sup>11<\/sup>\u2009cm<sup>-2<\/sup>\uff1b\u5149\u7167\u540e\uff0c\u6c9f\u9053\u4e2d\u6700\u9ad8\u7a7a\u7a74\u6d53\u5ea6\u53ef\u4ee5\u8fbe\u52303.0\u2009\u00d7\u200910<sup>13<\/sup>\u2009cm<sup>-2<\/sup>\u3002<\/p>\n<p><strong>\u56fe3<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-179291 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724715.png\" alt=\"\" width=\"650\" height=\"201\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724715.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724715-300x93.png 300w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/p>\n<p>\u6574\u4f53\u89c2\u6d4b\u7ed3\u679c\u8868\u660e\uff0c\u5728\u4e9a\u5fae\u7c73\u5c3a\u5ea6\u4e0b\uff0c\u5c40\u90e8\u63ba\u6742\u53ef\u4ee5\u901a\u8fc7\u4e00\u5206\u949f\u5185\u7684\u5149\u7167\u65f6\u95f4\u7cbe\u786e\u7f16\u7a0b\u3002\u5728\u8865\u5145\u6587\u732e\u56fe14\u4e2d\uff0c\u4f5c\u8005\u752840\u4e2a\u5668\u4ef6\u505a\u4e86\u91cd\u590d\u6027\u5b9e\u9a8c\uff0c\u9a8c\u8bc1\u5668\u4ef6\u6027\u80fd\u53ef\u9760\u4e0e\u7a33\u5b9a\u6027\u3002<\/p>\n<p><strong>4\u3001\u5171\u9762BJTs\u548c\u5149\u4f0f\u7535\u6c60\u7684\u53ef\u7f16\u7a0b\u5236\u4f5c<\/strong><\/p>\n<p>\u7814\u7a76\u4e86\u673a\u7406\u548c\u5f71\u54cd\u56e0\u7d20\uff0c\u6700\u540e\u5c31\u8981\u6765\u5e94\u7528\u8fd9\u4e2a\u7f3a\u9677\u8bf1\u5bfcp\u63ba\u6742\u5566\u3002<\/p>\n<p><strong>\u5e94\u7528\u4e00\uff1an-p-n\u53cc\u6781\u7ed3\u6676\u4f53\u7ba1(BJTs)\u7684\u9635\u5217\uff08\u5982\u56fe4a\u548c4b\uff09\u3002<\/strong><\/p>\n<p>\u56fe4c\u663e\u793a\u4e86\u4e00\u4e2an-p-n BJT\uff0c\u914d\u7f6e\u4e3a\u4e00\u4e2a\u5171\u53d1\u5c04\u6781\u51e0\u4f55\u5f62\u72b6\u7684\u7535\u6d41\u653e\u5927\u5668\u30024-\u03bcm-long\u901a\u9053\u9009\u62e9\u6027\u7167\u5c04\u7535\u678130s\u5f62\u6210p\u578b\u57fa\u6781(B)\uff0c\u800c\u5de6\u548c\u53f3\u7535\u6781\u4e3an\u578b\uff0c\u5206\u522b\u4e3a\u96c6\u7535\u6781(C)\u548c\u53d1\u5c04\u6781(E)\u3002<\/p>\n<p>\u626b\u63cf\u5149\u7535\u6d41\u6210\u50cf\u9a8c\u8bc1\u4e86\u4e24\u4e2aP-N\u4e8c\u6781\u7ba1\u8fde\u63a5\u5f62\u6210\u4e00\u4e2aN-P-N BJT\uff08\u56fe4d\u7684\u63d2\u56fe\uff09\u3002\u56fe4d\u4e2d\u7684\u4e8c\u6781\u7ba1I\u2013V\u7279\u6027\u9a8c\u8bc1\u4e86\u57fa\u6781-\u96c6\u7535\u6781\u7ed3\u4e3aP\u2013N\uff08\u7ea2\u8272\uff09\uff0c\u53d1\u5c04\u6781-\u57fa\u6781\u7ed3\u4e3aN\u2013P\uff08\u84dd\u8272\uff09\u3002\u5728\u56fe4e\u7684\u51fa\u7279\u6027\u4e2d\uff0c\u8f93\u5165\u7535\u6d41I<sub>b<\/sub>\u4e3a0.5 na\uff0c\u5728\u96c6\u7535\u6781\u7535\u6d41Ic\u653e\u5927\u52303\u20139 na\uff0c\u5176\u4e2d\u03b2\u6d4b\u91cf\u503c\u76f8\u5bf9\u8f83\u5c0f\uff0c\u5927\u7ea610\u201320\uff08\u56fe4e\uff0c\u84dd\u8272\u4e0b\uff09\u3002\u7531\u4e8en\u2013p\u2013n BJT\u88ab\u653e\u7f6e\u5728SiO2\/p+-Si\u57fa\u677f\u4e0a\uff0c\u56e0\u6b64\u53ef\u4ee5\u901a\u8fc7\u65bd\u52a0\u4e00\u4e2a\u6b63\u80cc\u6805\u7535\u538bV<sub>g<\/sub>\u8c03\u6574BJT\u5185\u7684\u80fd\u91cf\u504f\u79fb\uff08\u4ece\u800c\u53ef\u4ee5\u8c03\u6574\u53d1\u5c04\u6781\u3001\u57fa\u6781\u548c\u96c6\u7535\u6781\u533a\u57df\u7684\u63ba\u6742\u5206\u5e03\u4ee5\u53ca\u53d1\u5c04\u6781-\u57fa\u6781\u548c\u57fa\u6781-\u96c6\u7535\u6781\u8fde\u63a5\u5904\u7684\u8017\u5c3d\u5bbd\u5ea6\uff09\uff0c\u4ece\u800c\u4f7f\u8be5\u5668\u4ef6\u53d8\u4e3a\u8f6c\u6362\u5668\u4ef6\u3002\u65bd\u52a040 V\u6b63\u6805\u538b\u65f6\uff0c\u5f62\u6210N<sup>+<\/sup>\u2013P\u2013N<sup>+<\/sup>\u578bBJT\uff0c\u03b2\u663e\u8457\u589e\u52a0\u5230150\u4ee5\u4e0a\uff08\u56fe4f\uff0c\u7ea2\u8272\u4e0a\uff09\u3002\u5982\u63d2\u56fe\u6240\u793a\uff0c\u53d1\u5c04\u6781\u548c\u96c6\u7535\u6781\u7684\u91cd\u63ba\u6742\u63d0\u9ad8\u4e86\u6ce8\u5165\u6548\u7387\uff08\u5373\u53d1\u5c04\u6781\u6ce8\u5165\u7684\u8f7d\u6d41\u5b50\u4e0e\u57fa\u6781\u6ce8\u5165\u7684\u8f7d\u6d41\u5b50\u4e4b\u6bd4\uff09\u3002\u53d1\u5c04\u6781\u533a\u57df\u7684\u91cd\u63ba\u6742\u548c\u57fa\u6781\u533a\u57df\u7684\u8f7b\u63ba\u6742\u5bfc\u81f4\u6ce8\u5165\u57fa\u6781\u7684\u7535\u5b50\u6bd4\u4ece\u57fa\u6781\u6ce8\u5165\u53d1\u5c04\u6781\u7684\u7a7a\u7a74\u591a\u5f97\u591a\u3002<\/p>\n<p><strong>\u56fe4<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-179292 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724716.png\" alt=\"\" width=\"657\" height=\"469\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724716.png 657w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724716-300x214.png 300w\" sizes=\"(max-width: 657px) 100vw, 657px\" \/><\/p>\n<p><strong>\u5e94\u7528\u4e8c\uff1a\u5706\u5f62\u5171\u9762p-n\u7ed3\u9635\u5217\u2014\u2014\u5149\u4f0f\u7535\u6c60\uff08\u5982\u56fe5\uff09\u3002<\/strong><\/p>\n<p>\u53ef\u7f16\u5199\u63ba\u6742\u4e5f\u53ef\u7528\u4e8e\u8bbe\u8ba1\u4efb\u610f\u5f62\u72b6\u7684\u5171\u9762\u5668\u4ef6\u7ed3\u6784\u3002\u9996\u5148\u5728\u5927\u9762\u79efMoTe<sub>2<\/sub>\u4e0a\u7ed8\u5236\u5706\u5f62\u9635\u5217\uff0c\u5e76\u901a\u8fc7\u5149\u523b\u5c06\u6bcf\u4e2a\u7535\u6781\u914d\u7f6e\u5728\u5706\u5f62\u7684\u4e2d\u5fc3\u548c\u5916\u56f4\u3002\u7136\u540e\u5bf9\u9635\u5217\u4e2d\u5fc3\u7535\u6781\u4e0a\u5149\u71671 min\u4ea7\u751f\u76d8\u5f62P-N\u4e8c\u6781\u7ba1\uff08\u56fe5a\uff0cb\uff09\u3002\u5149\u7535\u6d41\u6210\u50cf\uff08\u56fe5C\uff09\u8bc1\u5b9e\u5f84\u5411P-N\u7ed3\u3002\u6700\u540e\uff0c\u75281200 nm\u6fc0\u5149\u5668\u6d4b\u91cf\u4e8c\u6781\u7ba1\u7684\u5149\u4f0f\u54cd\u5e94\u3002\u5728\u56fe5d\u4e2d\uff0c\u9ed1\u3001\u7ea2\u3001\u84dd\u3001\u7eff\u7ebf\u5bf9\u5e940\u30010.6\u30012.4\u300113.8 nw\u5149\u529f\u7387\u7684\u5149\u4f0fI-V\u66f2\u7ebf\u3002EQE\u4e3a\u7535\u8377\u8f7d\u6d41\u5b50\u6570\u4e0e\u5149\u5b50\u6570\u4e4b\u6bd4\uff0c\u5373EQE=\uff08I<sub>ph<\/sub>\/e\uff09\/\uff08P<sub>opt<\/sub>\/hv\uff09\uff0c\u5176\u4e2dI<sub>ph<\/sub>\u662fV<sub>b<\/sub>=0\u7684\u5149\u7535\u6d41\uff0ce\u662f\u57fa\u672c\u7535\u8377\uff0cP<sub>opt<\/sub>\u662f\u5149\u529f\u7387\uff0ch\u662f\u666e\u6717\u514b\u5e38\u6570\uff0cv\u662f\u5149\u9891\u7387\u3002\u5f97\u5230EQE\u5206\u522b\u4e3a10%\u300116%\u548c11%\uff0c\u6bd4\u4f7f\u7528MoS<sub>2<\/sub>\u6216WSe<sub>2<\/sub>\u5355\u5c42p-n\u5149\u4f0f\u7535\u6c60\u83b7\u5f97\u7684\u503c\u9ad8\u4e00\u4e2a\u6570\u91cf\u7ea7\uff0c\u53ef\u4e0e\u9ad8\u6027\u80fd2d TMDC\/\u77f3\u58a8\u70ef\u5782\u76f4\u5806\u53e0\u5149\u7535\u6781\u6027\u7535\u6c60\u76f8\u6bd4\u3002<\/p>\n<p><strong><b>\u56fe5<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"wp-image-179293 size-full aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724717.png\" alt=\"\" width=\"650\" height=\"189\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724717.png 650w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724717-300x87.png 300w\" sizes=\"(max-width: 650px) 100vw, 650px\" \/><\/p>\n<p><strong>5\u3001\u7ed3\u675f\u7684\u5206\u754c\u7ebf<\/strong><\/p>\n<p>\u6240\u4ee5\uff0c\u7528\u626b\u63cf\u53ef\u89c1\u5149\u63a2\u9488\u5b9e\u73b02H-MoTe<sub>2<\/sub>\u6c9f\u9053\u81ea\u5bf9\u51c6\u63ba\u6742\uff0c\u5feb\u901f\u800c\u7b80\u5355\u5730\u5b8c\u6210\u4e86\u4e8c\u7ef4\u7535\u8def\u7684\u53ef\u7f16\u7a0b\u5199\u5165\uff0c\u5bf9\u5f00\u53d1\u4e8c\u7ef4\u534a\u5bfc\u4f53\u5927\u89c4\u6a21\u7535\u8def\u662f\u975e\u5e38\u6709\u4ef7\u503c\u7684!\u5927\u4f19\u4eec\u4e5f\u53ef\u4ee5\u8003\u8651\u8003\u8651\u5176\u5b83\u4e8c\u7ef4\u6750\u6599\u662f\u5426\u4e5f\u80fd\u5b9e\u73b0\u5982\u6b64\u667a\u80fd\u800c\u7b80\u4fbf\u7684\u96c6\u6210\u5462?<\/p>\n<p><strong><b>\u53c2\u8003\u6587\u732e\uff1a<\/b><\/strong>Seo, S.-Y.; Park, J.; Park, J.; Song, K.; Cha, S.; Sim, S.; Choi, S.-Y.; Yeom, H. W.; Choi, H.; Jo, M.-H., Writing monolithic integrated circuits on a two-dimensional semiconductor with a scanning light probe. Nature Electronics 2018, 1 (9), 512-517.<\/p>\n<p><strong><b>\u6587\u7ae0\u94fe\u63a5\uff1a<\/b><\/strong>https:\/\/www.nature.com\/articles\/s41928-018-0129-6<\/p>\n<p>\u672c\u6587\u7531<strong>linglingbb<\/strong>\u4f9b\u7a3f\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4e8c\u7ef4\u6750\u6599\u6784\u6210\u7684\u8303\u5fb7\u534e\u5f02\u8d28\u7ed3\u662f\u5f00\u53d1\u4e0b\u4e00\u4ee3\u7535\u5b50\u548c\u5149\u7535\u5b50\u5668\u4ef6\u7684\u7406\u60f3\u6750\u6599\uff0c\u5e76\u4e14\u5c06\u9010\u6e10\u8d70\u5411\u4e8c\u7ef4\u5668\u4ef6\u96c6\u6210\u7535\u8def\u3002\u4f46\u5236\u4f5c\u4e8c\u7ef4\u6750\u6599\u7684\u534a\u5bfc\u4f53\u96c6\u6210\u7535\u8def\u662f\u975e\u5e38\u8270\u8f9b\u7684\u3002\u76ee\u524d\u5e38\u7528\u7684\u5236\u9020\u8303\u5fb7&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-179286","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/179286"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=179286"}],"version-history":[{"count":6,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/179286\/revisions"}],"predecessor-version":[{"id":180466,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/179286\/revisions\/180466"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=179286"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=179286"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=179286"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}