{"id":180973,"date":"2019-07-21T06:39:55","date_gmt":"2019-07-20T22:39:55","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=180973"},"modified":"2019-07-20T21:40:12","modified_gmt":"2019-07-20T13:40:12","slug":"%e7%b2%be%e5%93%81%e5%b9%b2%e8%b4%a7%ef%bc%9a%e6%99%b6%e4%bd%93%e5%ad%a6%e5%8f%96%e5%90%91%e7%9a%84%e5%88%86%e6%9e%90%e6%96%b9%e6%b3%95","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=180973","title":{"rendered":"\u7cbe\u54c1\u5e72\u8d27\uff1a\u6676\u4f53\u5b66\u53d6\u5411\u7684\u5206\u6790\u65b9\u6cd5"},"content":{"rendered":"<p>\u6676\u4f53\u5b66\u53d6\u5411\u662f\u6750\u6599\u5b66\u79d1\u4e2d\u7684\u91cd\u8981\u5206\u652f\uff0c\u5f53\u6676\u7c92\u53d1\u751f\u62e9\u4f18\u53d6\u5411\u65f6\uff0c\u5219\u5bfc\u81f4\u6750\u6599\u6027\u80fd\uff08\u529b\u5b66\uff0c\u7269\u7406\u548c\u5316\u5b66\u6027\u80fd\uff09\u7684\u5404\u5411\u5f02\u6027\u3002\u5404\u5411\u5f02\u6027\u4f1a\u9020\u6210\u6750\u6599\u5b9e\u9645\u5e94\u7528\u4e2d\u7684\u5404\u79cd\u95ee\u9898\uff0c\u5982\u94dd\u5408\u91d1\u5178\u578b\u7684\u5236\u8033\u73b0\u8c61\uff0c\u518d\u5982\u53d6\u5411\u7845\u94a2\u4e2d\u5b58\u5728Goss\u7ec7\u6784\u65f6\uff0c\u6709\u5229\u4e8e\u5176\u78c1\u5b66\u6027\u80fd\u3002\u5728\u57fa\u7840\u7814\u7a76\u9886\u57df\uff0c\u7ec7\u6784\u7684\u5f62\u6210\u4e0e\u6f14\u53d8\u662f\u57fa\u672c\u7684\u79d1\u5b66\u95ee\u9898\u3002\u5728\u5de5\u4e1a\u5e94\u7528\u9886\u57df\uff0c\u901a\u8fc7\u7ec7\u6784\u7684\u8bbe\u8ba1\u548c\u63a7\u5236\u53ef\u4ee5\u63d0\u9ad8\u6750\u6599\u7684\u6027\u80fd\u3002\u968f\u7740\u8fd1\u5e74\u6765EBSD\u548cXRD\u7b49\u8868\u5f81\u6280\u672f\u7684\u53d1\u5c55\uff0c\u5404\u79cdSCI\u671f\u520a\u7684\u53d1\u6587\u90fd\u5df2\u79bb\u4e0d\u5f00\u5bf9\u6750\u6599\u6676\u4f53\u5b66\u53d6\u5411\u7684\u5206\u6790\u3002\u7136\u800c\u5173\u4e8e\u6676\u4f53\u5b66\u53d6\u5411\u7684\u5206\u6790\u4e00\u76f4\u662f\u96be\u70b9\uff0c\u6709\u4e9b\u7814\u7a76\u751f\u751a\u81f3\u5927\u5b66\u8001\u5e08\u5728\u9762\u5bf9\u6781\u56fe\u3001\u53cd\u6781\u56fe\u548cODF\u56fe\u65f6\u4e00\u8138\u832b\u7136\u3002\u7b14\u8005\u5f53\u5e74\u4e5f\u5bf9\u6676\u4f53\u5b66\u53d6\u5411\u7684\u5206\u6790\u611f\u89c9\u751a\u4e3a\u68d8\u624b\uff0c\u7ecf\u8fc7\u4e0a\u767e\u7bc7\u6587\u732e\u548c\u4e66\u7c4d\u7684\u9605\u8bfb\uff0c\u540c\u65f6\u8f97\u8f6c\u591a\u6b21\u5411\u591a\u4f4d\u56fd\u5185\u5927\u725b\u8001\u5e08\u8bf7\u6559\u624d\u5f97\u4ee5\u5165\u95e8\u3002\u6709\u611f\u4e8e\u6676\u4f53\u5b66\u53d6\u5411\u5206\u6790\u7684\u96be\u5ea6\uff0c\u7b14\u8005\u4eca\u5929\u4fbf\u5c06\u6240\u5b66\u5fc3\u5f97\u6089\u6570\u5206\u4eab\u7ed9\u5927\u5bb6\uff0c\u5e0c\u671b\u80fd\u4fc3\u8fdb\u5b66\u672f\u7684\u4ea4\u6d41\uff0c\u5171\u540c\u53d6\u5f97\u8fdb\u6b65\u3002<\/p>\n<p><strong>1. \u6676\u5e26\u5b9a\u5f8b<\/strong><\/p>\n<p>\u6676\u5e26\u5b9a\u5f8b\u662f\u6676\u4f53\u5b66\u4e2d\u7684\u91cd\u8981\u5b9a\u5f8b\uff0c\u5355\u6676\u6781\u5c04\u8d64\u9762\u6295\u5f71\u7684\u6b63\u786e\u7406\u89e3\u548c\u6781\u56fe\u3001\u53cd\u6781\u56fe\u7684\u5206\u6790\u90fd\u5fc5\u987b\u8981\u6b63\u786e\u638c\u63e1\u6676\u5e26\u5b9a\u5f8b\u3002\u5728\u7a7a\u95f4\u70b9\u9635\u4e2d\uff0c\u6240\u6709\u5e73\u884c\u4e8e\u67d0\u4e00\u76f4\u7ebf\u7684\u4e00\u7ec4\u6676\u9762\u7684\u7ec4\u5408\u79f0\u4e3a\u4e00\u4e2a\u6676\u5e26\u3002\u6216\u8005\u8bf4\u4ea4\u7ebf\u76f8\u4e92\u5e73\u884c\u7684\u4e00\u7ec4\u6676\u9762\u7684\u7ec4\u5408\u79f0\u4e3a\u4e00\u4e2a\u6676\u5e26\u3002\u8fd9\u4e00\u76f4\u7ebf\u5c31\u79f0\u4e3a\u6676\u5e26\u8f74\uff0c\u5b83\u7528\u6676\u5411\u6307\u6570\u6765\u8868\u793a\u3002<\/p>\n<p>1\uff09\u6676\u5e26\u5b9a\u5f8b\u7684\u542b\u4e49\uff1a<\/p>\n<p>\u5df2\u77e5\u4e00\u4e2a\u6676\u9762\u00a0(hkl) \u548c\u5b83\u6240\u5c5e\u7684\u6676\u5e26[uvw]\uff0c\u5c31\u5f88\u5bb9\u6613\u5f97\u5230\u4e8c\u8005\u4e4b\u95f4\u7684\u5173\u7cfb\uff1ahu+kv+lw=0\uff0c\u901a\u5e38\u628a\u8fd9\u4e2a\u5173\u7cfb\u5f0f\u79f0\u4e3a\u6676\u5e26\u5b9a\u5f8b\u3002\u6676\u5e26\u5b9a\u5f8b\u5b9e\u9645\u4e0a\u7ed9\u51fa\u4e86\u6676\u9762\u4e0e\u6676\u5411\u4e4b\u95f4\u7684\u5173\u7cfb\uff0c\u5982\u679c\u6676\u5411[uvw]\u5305\u62ec\u5728\u6676\u9762(hkl)\u4e2d\uff0c\u4e8c\u8005\u5c31\u6ee1\u8db3\u8fd9\u4e2a\u5173\u7cfb\u5f0f\u3002\u6709\u4e86\u8fd9\u4e2a\u5173\u7cfb\uff0c\u6211\u4eec\u5c31\u53ef\u4ee5\u6839\u636e\u5df2\u77e5\u7684\u6676\u9762\u6216\u6676\u5e26\u6765\u6c42\u5f97\u53e6\u5916\u4e00\u4e9b\u6676\u9762\u6216\u6676\u5e26\u3002<\/p>\n<p>2\uff09\u6676\u5e26\u5b9a\u5f8b\u7684\u4e24\u4e2a\u91cd\u8981\u5e94\u7528<\/p>\n<p>\u5df2\u77e5\u4e24\u6676\u9762(h<sub>1<\/sub>k<sub>1<\/sub>l<sub>1<\/sub>)\u548c(h<sub>2<\/sub>k<sub>2<\/sub>l<sub>2<\/sub>)\uff0c\u6c42\u4ea4\u7ebf[uvw]\u3002<br \/>\n \u89e3\uff1a\u6839\u636e\u6676\u5e26\u5b9a\u5f8b\uff1a<\/p>\n<p>h<sub>1<\/sub>u+k<sub>1<\/sub>v+l<sub>1<\/sub>w=0<br \/>\n h<sub>2<\/sub>u+k<sub>2<\/sub>v+l<sub>2<\/sub>w=0<br \/>\n u\uff1av\uff1aw=(k<sub>1<\/sub>l<sub>2<\/sub>-k<sub>2<\/sub>l<sub>1<\/sub>):(l<sub>1<\/sub>h<sub>2<\/sub>-l<sub>2<\/sub>h<sub>1<\/sub>):(h<sub>1<\/sub>k<sub>2<\/sub>-h<sub>2<\/sub>k<sub>1<\/sub>)<\/p>\n<p>\u5df2\u77e5\u4e24\u6676\u5e26[u<sub>1<\/sub>v<sub>1<\/sub>w<sub>1<\/sub>]\u548c[u<sub>2<\/sub>v<sub>2<\/sub>w<sub>2<\/sub>]\uff0c\u6c42\u6676\u9762\u6307\u6570(hkl)\u3002<br \/>\n \u89e3\uff1a\u6839\u636e\u6676\u5e26\u5b9a\u5f8b\uff1a<\/p>\n<p>hu<sub>1<\/sub>+kv<sub>1<\/sub>+lw<sub>1<\/sub>=0<br \/>\n hu<sub>2<\/sub>+kv<sub>2<\/sub>+lw<sub>2<\/sub>=0<br \/>\n h:k:l=(v<sub>1<\/sub>w<sub>2<\/sub>-v<sub>2<\/sub>w<sub>1<\/sub>):(w<sub>1<\/sub>u<sub>2<\/sub>-w<sub>2<\/sub>u<sub>1<\/sub>):(u<sub>1<\/sub>v<sub>2<\/sub>-u<sub>2<\/sub>v<sub>1<\/sub>)<\/p>\n<p><strong>2. \u5355\u6676\u6781\u5c04\u8d64\u9762\u6295\u5f71<\/strong><\/p>\n<p>\u6676\u4f53\u5185\u90e8\u5404\u6676\u9762\u548c\u6676\u5411\u4e4b\u95f4\u7684\u53d6\u5411\u5173\u7cfb\u672c\u8d28\u4e0a\u4e3a\u4e09\u7ef4\u7a7a\u95f4\u7684\u76f8\u5bf9\u5173\u7cfb\uff0c\u8868\u793a\u8d77\u6765\u901a\u5e38\u5f88\u4e0d\u65b9\u4fbf\u3002\u6240\u4ee5\u4eba\u4eec\u603b\u662f\u5e0c\u671b\u8fd9\u79cd\u4e09\u7ef4\u5173\u7cfb\u8f6c\u5316\u4e3a\u4e00\u79cd\u5e73\u9762\u5173\u7cfb\u3002\u76ee\u524d\u6700\u5e38\u7528\u7684\u4fbf\u662f\u6781\u5c04\u8d64\u9762\u6295\u5f71\u3002\u5355\u6676\u6781\u5c04\u8d64\u9762\u6295\u5f71\u7684\u6b63\u786e\u7406\u89e3\u9700\u8981\u6b63\u786e\u638c\u63e1\u6676\u5e26\u5b9a\u5f8b\u548c\u6676\u9762\u5939\u89d2\u7684\u8ba1\u7b97\u3002\u5173\u4e8e\u6676\u9762\u5939\u89d2\u7684\u8ba1\u7b97\u516c\u5f0f\u6bd4\u8f83\u7b80\u5355\uff0c\u5728\u5404\u79cd\u6559\u6750\u4e0a\u7686\u5df2\u7ed9\u51fa\uff0c\u7b14\u8005\u8fd9\u91cc\u4e0d\u518d\u5217\u51fa\u3002\u6781\u5c04\u8d64\u9762\u6295\u5f71\u5982\u56fe1\u6240\u793a\uff0c\u5c06\u6676\u80de\u653e\u5728\u7403\u5fc3\uff0c\u7136\u540e\u5f15\u5404\u6676\u9762\u7684\u6cd5\u7ebf\uff08\u56fe\u4e2d\u7eff\u7ebf\u548c\u7ea2\u7ebf\uff09\u65e0\u9650\u5ef6\u4f38\uff0c\u4e0e\u7403\u9762\u76f8\u8f83\u4e8e\u67d0\u70b9\uff08A\u3001B\u4e24\u6781\u70b9\uff09\uff0c\u7136\u540e\u628a\u7403\u9762\u7684\u70b9\u4e0e\u53c2\u8003\u7403\u7684\u5357\u6781\u70b9S\u76f8\u8fde\uff0c\u5219\u5728\u8d64\u9053\u5706\u4e0a\u76f8\u8f83\u4e8eA&#8217;\u548cB&#8217;\u4e24\u70b9\uff0c\u53eb\u505aA\u3001B\u4e24\u6781\u70b9\u7684\u6781\u5c04\u8d64\u9762\u6295\u5f71\u70b9\u3002<\/p>\n<p>\u56fe1\u00a0\u6781\u5c04\u8d64\u9762\u6295\u5f71\u539f\u7406<img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180976 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72471-22.png\" alt=\"\" width=\"680\" height=\"392\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72471-22.png 680w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72471-22-300x173.png 300w\" sizes=\"(max-width: 680px) 100vw, 680px\" \/><\/p>\n<p>\u56fe2\u4e3a\u7acb\u65b9\u6676\u80de\uff08001\uff09\u3001\uff08100\uff09\u548c\uff08010\uff09\u9762\u7684\u6781\u5c04\u6295\u5f71\uff0c\u5927\u5bb6\u53ef\u4ee5\u53c2\u8003\u56fe1\u6240\u7ed9\u51fa\u7684\u539f\u7406\u8fdb\u884c\u7406\u89e3\u3002\u53ef\u4ee5\u770b\u51fa\uff0c\u6b64\u6676\u80de\u5728\u53c2\u8003\u7403\u4e2d\u653e\u7f6e\u659c\u4e86\uff0c\u5047\u8bbe\u5982\u679c\uff08001\uff09\u9762\u5782\u76f4\u4e8eND\u8f74\uff0c\u5219\u6295\u5f71\u7684\u7ed3\u679c\u4e3a\uff08001\uff09\u4f4d\u4e8e\u57fa\u5706\u5706\u5fc3\uff0c\uff08100\uff09\u4f4d\u4e8eTD\u76f4\u7ebf\u4e0e\u57fa\u5706\u7684\u5de6\u4ea4\u70b9\uff0c\uff08010\uff09\u70b9\u4f4d\u4e8eTD\u76f4\u7ebf\u4e0e\u57fa\u5706\u7684\u4e0b\u4ea4\u70b9\uff08\u89c1\u56fe2\u4e2d\u7684\u4e09\u4e2a\u7ea2\u70b9\u6240\u793a\uff09\u3002\uff08001\uff09\u3001\uff08100\uff09\u548c\uff08010\uff09\u4e09\u4e2a\u9762\u662f\u4e24\u4e24\u5782\u76f4\u7684\u5173\u7cfb\uff0c\u4ed6\u4eec\u4e4b\u95f4\u7684\u5939\u89d2\u662f90\u00b0\u3002\u4ece\u56fe\u4e2d\u4e0d\u96be\u8054\u60f3\u5230\u57fa\u5706\u7684\u534a\u5f84\u957f\u4e3a90\u00b0\uff0c1\/4\u5706\u5f27\u4e5f\u4e3a90\u00b0\u3002<\/p>\n<p>\u56fe2\u00a0\u7acb\u65b9\u6676\u80de\uff08001\uff09\u3001\uff08100\uff09\u548c\uff08010\uff09\u9762\u7684\u6781\u5c04\u6295\u5f71<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180978 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72472-21.png\" alt=\"\" width=\"680\" height=\"258\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72472-21.png 680w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72472-21-300x114.png 300w\" sizes=\"(max-width: 680px) 100vw, 680px\" \/><\/p>\n<p>\u6781\u5c04\u6295\u5f71\u7684\u89c4\u5f8b\u662f\uff1a\u4e0e\u8d64\u9053\u9762\u5e73\u884c\u7684\u6676\u9762\uff0c\u5b83\u7684\u6781\u5c04\u6295\u5f71\u5fc5\u5728\u6781\u5706\u4e2d\u5fc3\uff1b\u5782\u76f4\u4e8e\u8d64\u9053\u9762\u7684\u6676\u9762\uff0c\u5b83\u4eec\u7684\u6781\u70b9\u7684\u6295\u5f71\u5fc5\u5728\u6781\u5706\u7684\u5706\u5468\u4e0a\uff1b\u503e\u659c\u6676\u9762\u6781\u70b9\u7684\u6295\u5f71\u5fc5\u5728\u6781\u5706\u5185\uff0c\u6676\u9762\u6cd5\u7ebf\u4e0e\u6295\u5f71\u7684\u5939\u89d2\u8d8a\u5c0f\uff0c\u5219\u6295\u5f71\u70b9\u8ddd\u6781\u5706\u4e2d\u5fc3\u8d8a\u8fd1\u3002\u6295\u5f71\u56fe\u4e0a\u7684\u76f4\u7ebf\u548c\u5706\u5f27\u4e0a\u6240\u6709\u7684\u70b9\u5c5e\u4e8e\u6676\u540c\u4e00\u5e26\u3002\u6bcf\u4e00\u70b9\u7684\u4f4d\u7f6e\u53ef\u4ee5\u6839\u636e\u4ed6\u6240\u5c5e\u6676\u5e26\u4ee5\u53ca\u4e0e\u5706\u5fc3\u548c\u4e0a\u4e0b\u6781\u70b9\u7684\u6240\u5448\u89d2\u5ea6\u6c42\u51fa\u3002\u6295\u5f71\u7403\u9762\u4e0a\u4efb\u610f\u4e24\u70b9P<sub>1<\/sub>\u548cP<sub>2<\/sub>\u4e4b\u95f4\u7684\u5927\u5706\u5f27\u6bb5\u7684\u5f27\u5ea6(P<sub>1 <\/sub>P<sub>2<\/sub>)\uff0c\u65e2\u662fP<sub>1<\/sub>\u3001P<sub>2<\/sub>\u4e24\u70b9\u6240\u4ee3\u8868\u7684\u4e24\u6761\u76f4\u7ebf\u95f4\u7684\u4ea4\u89d2\uff0c\u4e5f\u662f\u5b83\u4eec\u6240\u4ee3\u8868\u7684\u4e24\u4e2a\u5e73\u9762\u95f4\u7684\u4ea4\u89d2\u6216\u8865\u89d2\u3002\u4e00\u3001\u4e09\u8c61\u9650\u548c\u4e8c\u3001\u56db\u8c61\u9650\u5bf9\u79f0\u70b9\u4e92\u4e3a\u76f8\u53cd\u6570\u3002<\/p>\n<p>\u4e0b\u9762\u7b14\u8005\u5e26\u9886\u5927\u5bb6\u753b\u51fa\u7acb\u65b9\u6676\u80de\uff08001\uff09\u7684\u6781\u5c04\u6295\u5f71\u3002\u9996\u5148\u53ef\u4ee5\u786e\u5b9a\uff08001\uff09\u6781\u70b9\u5728\u6295\u5f71\u56fe\u57fa\u5706\u4e2d\u5fc3\uff0c\u5176\u5bf9\u5e94\u7684\u5927\u5706\u662f\u57fa\u5706\u5706\u5468\uff0c\u56e0\u6b64[001]\u4e3a\u6676\u5e26\u8f74\u7684\u6240\u6709\u6781\u70b9\u90fd\u5728\u57fa\u5706\u5706\u5468\u4e0a\uff0c\u56e0\u4e3a\u9996\u5148\u6839\u636e\u5750\u6807\u7cfb\uff0c\u786e\u5b9a\uff08100\uff09\u6781\u70b9\uff0c\u7531\u4e8e\uff08010\uff09 \u22a5\u00a0\uff08100\uff09\uff0c\u9006\u8f6c90\u00b0\u4fbf\u5f97\uff08010\uff09\u3002\uff08110\uff09\u548c\uff08-110\uff09\u4e5f\u5c5e\u4e8e[001]\u6676\u5e26\uff0c\u7531\u4e8e\uff08110\uff09\u4e0e\uff08100\uff09\u548c\uff08010\uff09\u6781\u70b9\u5939\u89d2\u5206\u522b\u4e3a135\u00b0\u548c45\u00b0\uff0c\u5728\u5706\u5468\u4e0a\u65cb\u8f6c\u76f8\u5e94\u89d2\u5ea6\u4fbf\u5f97\u4e24\u4e2a\u6781\u70b9\u4f4d\u7f6e\u3002\u6839\u636e\u8c61\u9650\u89c4\u5f8b\u53ef\u5f97\uff080-11\uff09\u548c\uff08011\uff09\u6781\u70b9\u3002\u4ee5[010]\u4e3a\u6676\u5e26\u8f74\u7684\u6676\u5e26\u4f4d\u4e8e\u8fc7\uff08100\uff09\u6781\u70b9\u548c\u5706\u5fc3\u7684\u76f4\u5f84\u4e0a\uff0c\uff08101\uff09\uff08-101\uff09\u5c5e\u4e8e\u6b64\u6676\u5e26\uff0c\u540c\u6837\uff0c\u8ba1\u7b97\u4ed6\u4eec\u4e0e\uff08010\uff09\u548c\uff08001\uff09\u7684\u5939\u89d2\u5c31\u53ef\u4ee5\u5b9a\u51fa\u4ed6\u4eec\u7684\u6781\u70b9\u4f4d\u7f6e\u3002[-101]\u8fc7 (010)\u548c\uff08101\uff09\u7684\u5927\u5706\u5f27\uff0c[0-11]\u6676\u5e26\u8fc7\uff08100\uff09\u548c\uff08011\uff09\u6781\u70b9\u7684\u5927\u5706\u5f27\uff0c\uff08111\uff09\u540c\u5c5e\uff08-101\uff09\u548c\uff080-11\uff09\u6676\u5e26\uff0c\u6240\u4ee5\u4ea4\u70b9\u5c31\u5c5e\u4e8e\uff08111\uff09\u6781\u70b9\u3002\u5176\u4ed6\u7684\u70b9\u90fd\u53ef\u4ee5\u6839\u636e\u540c\u6837\u7684\u539f\u7406\u753b\u51fa<sup>[<\/sup><sup>1]<\/sup>\u3002<\/p>\n<p>\u56fe 3 \u7acb\u65b9\u6676\u80de\uff08001\uff09\u9762\u7684\u91cd\u8981\u70b9\u7684\u6781\u5c04\u6295\u5f71<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180995 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72473-22.png\" alt=\"\" width=\"450\" height=\"449\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72473-22.png 450w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72473-22-150x150.png 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72473-22-300x300.png 300w\" sizes=\"(max-width: 450px) 100vw, 450px\" \/><\/p>\n<p>\u7531\u6b64\u53ef\u89c1\uff1a\u786e\u5b9a\u4efb\u4e00\u6781\u70b9\u4f4d\u7f6e\u7684\u8981\u7d20\u4e3b\u8981\u6709\u4e24\u4e2a\uff1a1.\u786e\u5b9a\u6240\u5c5e\u6676\u5e26\u8f74\uff1b2.\u786e\u5b9a\u6b64\u70b9\u4e0e\u539f\u70b9\u548c\u4e24\u6781\u70b9\u7684\u5939\u89d2\u3002\u5355\u6676\u6781\u5c04\u8d64\u9762\u6295\u5f71\u662f\u5206\u6790\u6781\u56fe\u7684\u57fa\u7840\uff0c\u5927\u5bb6\u5e73\u65f6\u80fd\u591f\u6b63\u786e\u7406\u89e3\u6b64\u56fe\u7684\u539f\u7406\u4e0e\u7279\u70b9\u5c31\u884c\uff0c\u6ca1\u6709\u5fc5\u8981\u4eb2\u624b\u7ed8\u5236\u3002\u4e8b\u5b9e\u4e0a\uff0c\u73b0\u5728\u5f88\u591a\u8f6f\u4ef6\u90fd\u53ef\u4ee5\u753b\u51fa\u4efb\u4e00\u6676\u7cfb\u4efb\u4e00\u6676\u9762\u7684\u6781\u5c04\u6295\u5f71\uff0c\u7b14\u8005\u5728\u8fd9\u91cc\u7ed9\u5927\u5bb6\u63a8\u8350\u7684\u662fPTC lab\u8f6f\u4ef6\u3002\u8fd9\u6b3e\u8f6f\u4ef6\u5728\u5c0f\u6728\u866b\u4e0a\u5c31\u53ef\u4ee5\u4e0b\u8f7d\uff0c<\/p>\n<p>1\uff09\u6807\u51c6\u6781\u56fe\u7684\u753b\u6cd5<\/p>\n<p>\u9996\u5148\uff0c\u6211\u4eec\u5e94\u8be5\u4e86\u89e3\u6781\u56fe\u7684\u5b9a\u4e49\uff0c\u6781\u56fe\u662f\u6676\u4f53\u7684\u67d0\u4e00\u6676\u9762\u76f8\u5bf9\u4e8e\u6750\u6599\u5b8f\u89c2\u5750\u6807\u7cfb\u7684\u6295\u5f71\u3002\u8fd9\u4e00\u6676\u9762\u4e00\u822c\u9009\u62e9\u6676\u80de\u7684\u4f4e\u6307\u6570\u9762\uff0c\u5728\u7acb\u65b9\u6676\u7cfb\u4e2d\u4e00\u822c\u7528\uff08100\uff09\u3001\uff08110\uff09\u3001\uff08111\uff09\u9762\uff0c\u800c\u5728\u516d\u65b9\u6676\u7cfb\u4e2d\u7528\uff080001\uff09\u3001\uff0810-10\uff09\u3001\uff0811-20\uff09\u9762\u3002\u5728\u8868\u5f81\u6750\u6599\u7684\u7ec7\u6784\u65f6\uff0c\u4e00\u822c\u4e00\u4e2a\u9762\u7684\u6781\u56fe\u65e2\u53ef\u4ee5\u8868\u793a\u51fa\u5168\u90e8\u7684\u7ec7\u6784\uff0c\u5176\u4ed6\u6676\u9762\u7684\u6781\u56fe\u53ef\u4ee5\u7528\u4e8e\u76f8\u4e92\u9a8c\u8bc1\u3002\u6781\u56fe\u4e3b\u8981\u7528\u6765\u63cf\u8ff0\u677f\u7ec7\u6784{hkl}&lt;uvw&gt;\u3002\u6839\u636e\u6781\u56fe\u7684\u5b9a\u4e49\uff0c\u5f88\u5bb9\u6613\u7684\u770b\u51fa\uff0c\u5b83\u8868\u793a\u7684\u662f\u6676\u4f53\u5750\u6807\u7cfb\u4e0e\u6837\u54c1\u5750\u6807\u7cfb\u7684\u5173\u7cfb\u3002\u4e0b\u9762\u6211\u4eec\u91cd\u70b9\u4ecb\u7ecd\u4efb\u4e00\u7ec7\u6784{hkl}&lt;uvw&gt;\u5bf9\u5e94\u7684\u67d0\u4e00\u6676\u9762(HKL)\u7684\u6781\u56fe\u753b\u6cd5\u3002<\/p>\n<p><strong><b>\u6b65\u9aa4\uff1a<\/b><\/strong><\/p>\n<p>1. \u6839\u636e\u6676\u9762\u4e4b\u95f4\u5939\u89d2\u7684\u8ba1\u7b97\u516c\u5f0f\u53ef\u4ee5\u7b97\u51fa{hkl}\u4e0e(HKL)\u4e4b\u95f4\u7684\u5939\u89d2\u03b8\u3001{uvw}\u4e0e(HKL)\u4e4b\u95f4\u7684\u5939\u89d2\u03c6\u3002<\/p>\n<p>2. \u5728\u4e4c\u6c0f\u7f51\u4e0a\u4ee5\u5706\u5fc3\u4e3a\u4e2d\u5fc3\uff0c\u5206\u522b\u4ee5\u03b8\u4e3a\u534a\u5f84\u5212\u5706\uff0c\u518d\u4ee5\u4e0a\u4e0b\u6781\u70b9\u4e3a\u4e2d\u5fc3\uff0c\u5728\u4e4c\u6c0f\u7f51(Wulff\u2019net)\u4e0a\u627e\u5230\u4e0e\u03c6\u5bf9\u5e94\u7684\u4e24\u6761\u7b49\u66f2\u7ebf\uff0c\u4e0e\u524d\u9762\u7684\u5706\u5171\u6709\u82e5\u5e72\u4e2a\u4ea4\u70b9\u3002\u8fd9\u4e9b\u70b9\u5c31\u4ee3\u8868\u4e86\u5728(HKL)\u6781\u56fe\u7684{hkl}&lt;uvw&gt;\u7ec7\u6784\u3002<\/p>\n<p>\u4f8b1\uff1a{001}&lt;100&gt;\u7acb\u65b9\u7ec7\u6784\u7684(111)\u3001(200)\u3001(220)\u6807\u51c6\u6781\u56fe\u7684\u7ed8\u5236\u65b9\u6cd5<sup>[<\/sup><sup>2]<\/sup>\u3002<\/p>\n<p>a. {100}\u4e0e(111)\u6676\u9762\u7684\u5939\u89d2\u662f7\u00b0\uff0c\u5728\u5434\u6c0f\u7f51(Wulff\u2019net)\u4e0a\u4ee5\u5706\u5fc3\u4e3a\u4e2d\u5fc3\uff08\u96f6\u5ea6\uff09\uff0c\u5728\u6c34\u5e73\u7ebf\u6216\u5782\u76f4\u7ebf\u4e0a\u627e\u523054.7\u00b0\u70b9\u4e3a\u534a\u5f84\u5212\u5706\uff1b\u8be5\u5706\u4e0e\u4ee5\u4e0a\u4e0b\u6781\u70b9\u4e3a\u4e2d\u5fc3\u8ddd\u79bb\u4e3a54.7\u00b0\u7684\u4e24\u6761\u5f27\u7ebf\u76f8\u4ea4\u4e8e4\u4e2a\u70b9\uff0c\u8fd9\u5c31\u7ed8\u6210\u4e86\u7acb\u65b9\u7ec7\u6784\u7684(111)\u6781\u56fe\u3002<\/p>\n<p>\u56fe4\u00a0{001}&lt;100&gt;\u7acb\u65b9\u7ec7\u6784\u7684(111)\u6781\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180980 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72474-18.png\" alt=\"\" width=\"473\" height=\"189\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72474-18.png 473w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72474-18-300x120.png 300w\" sizes=\"(max-width: 473px) 100vw, 473px\" \/>b. {100}\u4e0e(200)\u6676\u9762\u7684\u5939\u89d2\u662f0\u00b0\u548c90\u00b0\uff0c\u5728\u5434\u6c0f\u7f51(Wulff\u2019net)\u4e0a\u7684\u5706\u5fc3\u548c\u5706\u5468\u6ee1\u8db3(100)\/\/ND\u7684\u6761\u4ef6\uff0c\u4e0a\u4e0b\u6781\u70b9\u548c\u6c34\u5e73\u7ebf\u6ee1\u8db3&lt;100&gt;\/\/RD\u7684\u6761\u4ef6\uff0c\u56e0\u6b64\uff0c\u4e0a\u4e0b\u6781\u70b9\u3001\u5de6\u53f3\u6781\u70b9\u548c\u4e2d\u5fc3\u5706\u70b9\u51715\u4e2a\u70b9\u5c31\u6784\u6210\u4e86\u7acb\u65b9\u7ec7\u6784\u7684(200)\u5168\u6781\u56fe\u3002<\/p>\n<p>\u56fe5\u00a0\u56fe4\u00a0{001}&lt;100&gt;\u7acb\u65b9\u7ec7\u6784\u7684(200)\u6781\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180981 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72475-16.png\" alt=\"\" width=\"525\" height=\"221\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72475-16.png 525w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72475-16-300x126.png 300w\" sizes=\"(max-width: 525px) 100vw, 525px\" \/>c. {100}\u4e0e(220)\u6676\u9762\u7684\u5939\u89d2\u662f45\u00b0\u548c90\u00b0\uff0c\u5728\u5434\u6c0f\u7f51(Wulff\u2019net)\u4e0a\u4ee5\u5706\u5fc3\u4e3a\u4e2d\u5fc3\uff0c\u8ddd\u79bb\u5706\u5fc3\u4e3a45\u00b0\u548c90\u00b0\u7684\u5706\u5c31\u4ee3\u8868\u4e86(100)\/\/ND,\u4ee5\u4e0a\u4e0b\u6781\u70b9\u4e3a\u4e2d\u5fc3\uff0c\u8ddd\u79bb\u6781\u70b9\u4e3a45\u00b0\u7684\u5f27\u7ebf\u548c\u901a\u8fc7\u5706\u5fc3\u7684\u6c34\u5e73\u7ebf\u8868\u793a&lt;100&gt;\/\/RD,\u4e0a\u8ff0\u5706\u548c\u5f27\u7ebf\u3001\u6c34\u5e73\u7ebf\u7684\u6240\u670910\u4e2a\u4ea4\u70b9\u6784\u6210\u7acb\u65b9\u7ec7\u6784\u7684(220)\u5168\u6781\u56fe\u3002<\/p>\n<p>\u56fe6 \u56fe4\u00a0{001}&lt;100&gt;\u7acb\u65b9\u7ec7\u6784\u7684(220)\u6781\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180982 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72476-14.png\" alt=\"\" width=\"520\" height=\"213\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72476-14.png 520w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72476-14-300x123.png 300w\" sizes=\"(max-width: 520px) 100vw, 520px\" \/><\/p>\n<p>\u6709\u4e86\u6807\u51c6\u6781\u56fe\uff0c\u6211\u4eec\u5c31\u53ef\u4ee5\u62ff\u6240\u6d4b\u7684\u6781\u56fe\u505a\u6bd4\u8f83\uff0c\u5f88\u5bb9\u6613\u770b\u51fa\u7ec7\u6784\u6210\u5206\uff0c\u7b80\u5355\u6613\u884c\u3002\u5927\u5bb6\u53ef\u4ee5\u770b\u51fa\uff0c\u753b\u6807\u51c6\u6781\u56fe\u6700\u4e3b\u8981\u7684\u662f\u6b63\u786e\u7684\u8ba1\u7b97\u6676\u9762\u65cf\u4e4b\u95f4\u7684\u5939\u89d2\u3002<\/p>\n<p>2\uff09\u6781\u56fe\u3001\u53cd\u6781\u56fe\u7684\u5206\u6790\u65b9\u6cd5<\/p>\n<p>A. \u5f88\u591a\u540c\u5b66\u6216\u8005\u8001\u5e08\u5728\u9762\u5bf9\u6781\u56fe\u548c\u53cd\u6781\u56fe\u65f6\u5f80\u5f80\u4e00\u8138\u8ff7\u832b\u3002\u6781\u56fe\u7684\u5206\u6790\u5bf9\u4e8e\u521d\u5b66\u8005\u786e\u5b9e\u6bd4\u8f83\u96be\uff0c\u4e00\u822c\u7684\u5206\u6790\u65b9\u6cd5\u662f\u5c06\u6240\u5f97\u6781\u56fe\u4e0e\u5355\u6676\u6781\u5c04\u8d64\u9762\u6295\u5f71\u5bf9\u6bd4\uff0c\u4e00\u65e6\u5bf9\u4e0a\uff0c\u5219\u5355\u6676\u6295\u5f71\u56fe\u7684\u5706\u5fc3\u7ed9\u51fa\u6676\u9762\u6307\u6570\uff08HKL\uff09\uff0c\u8f67\u5411\u6240\u6307\u7684\u6676\u9762\u7ed9\u51fa\u6676\u5411\u6307\u6570&lt;uvw&gt;. \u4f46\u5b9e\u9645\u6240\u6d4b\u7684\u7ec7\u6784\u6210\u5206\u5f80\u5f80\u6709\u5f88\u591a\u79cd\uff0c\u8fd9\u79cd\u5bf9\u6bd4\u7684\u65b9\u6cd5\u5de5\u4f5c\u91cf\u975e\u5e38\u4e4b\u5927\u3002\u7b14\u8005\u5efa\u8bae\u6781\u56fe\u5206\u6790\u7528\u89e3\u6790\u6cd5\u3002\u5176\u4e00\u822c\u6b65\u9aa4\u5982\u4e0b\uff1a<\/p>\n<p>a.\u5148\u770b\u5bf9\u79f0\u6027\uff08\u7ec7\u6784\u7684\u6210\u5206\u4e00\u822c\u5177\u6709\u5bf9\u79f0\u6027\u7684\uff0c\u7acb\u65b9\u7ec7\u6784\uff09\uff1b<\/p>\n<p>b.\u518d\u6839\u636e\u770b\u4e0e\u6295\u5f71\u4e2d\u5fc3\u548c\u4e0a\u4e0b\u4e24\u6781\u70b9\u7684\u5939\u89d2\uff1b<\/p>\n<p>c.\u4e0e\u4e2d\u5fc3\u8ba1\u7b97\u7684\u5939\u89d2\u6c42\u5f97\u6676\u9762\u6307\u6570\uff0c\u4e0e\u4e0a\u4e0b\u6781\u70b9\u7684\u5939\u89d2\u8bfb\u4e66\u6c42\u5f97\u6676\u5411\u6307\u6570\u3002<\/p>\n<p>\u56fe7\u00a0\u7acb\u65b9\u7ed3\u6784\uff08111\uff09\u6781\u56fe\u5206\u6790\u56fe\u89e3<\/p>\n<p>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-181044 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe7-4.jpg\" alt=\"\" width=\"380\" height=\"400\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe7-4.jpg 380w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe7-4-285x300.jpg 285w\" sizes=\"(max-width: 380px) 100vw, 380px\" \/><\/p>\n<p>\u4e3e\u4f8b1\uff1a\u5982\u56fe7\u6240\u793a\u4e3a\uff08111\uff09\u6781\u56fe\uff0c\u8fd9\u610f\u5473\u7740\u7ec7\u6784\u5bc6\u5ea6\u6700\u5927\u7684\u56db\u4e2a\u70b9\uff08\u56fe\u4e2d\u4e3a\u7ea2\u70b9\uff09\u90fd\u4e3a{111}\u6676\u9762\u65cf\u7684\u5b50\u9762\u3002\u9996\u5148\u8ba1\u7b97\u51fa\u4e0e\uff08111\uff09\u6676\u9762\u5448\u03b1\u89d2\u5ea6\u7684\u6676{hkl}\u2014\u6676\u9762\u6307\u6570\uff0c\u518d\u5229\u7528\u03b2\u89d2\u5ea6\u6c42\u51fa\u6676\u5411\u6307\u6570&lt;uvw&gt;.\u6240\u5f97\u5230\u7684\uff08hkl\uff09&lt;uvw&gt;\u4fbf\u662f\u8be5\u6781\u56fe\u53cd\u5e94\u7684\u7ec7\u6784\u3002\u8fd9\u4ec5\u4e3a\u7406\u8bba\u4e0a\u6781\u56fe\u7684\u5206\u6790\uff0c\u5b9e\u9645\u6d4b\u5f97\u7684\u6781\u56fe\u8fdc\u4e3a\u590d\u6742\uff0c\u5206\u6790\u65f6\u9700\u8981\u5927\u5bb6\u7efc\u5408\u5206\u6790\u3002\u4e0b\u9762\u7b14\u8005\u5e26\u5927\u5bb6\u5206\u6790\u4e2a\u5b9e\u6d4b\u7684\u6781\u56fe\u3002<\/p>\n<p>\u4e3e\u4f8b2\uff1a\u5982\u56fe8\u6240\u793a\uff0c\u9996\u5148\u6211\u4eec\u627e\u4e09\u4e2a\u6781\u56fe\u7684\u5bf9\u79f0\u6027\uff08\u4e0d\u540c\u989c\u8272\u7684\u5c0f\u4e09\u89d2\u5f62\u8868\u793a\uff09\uff0c\u53ef\u4ee5\u770b\u51fa\uff0c\u8be5\u6750\u6599\u4e3b\u8981\u5b58\u5728\u4e09\u79cd\u677f\u7ec7\u6784\uff0c\u5206\u6790\u65b9\u6cd5\u5982\u4e0a\u3002\u5b9e\u9645\u4e2d\u7531\u4e8e\u5404\u79cd\u590d\u6742\u7684\u56e0\u7d20\uff0c\u6781\u56fe\u7684\u5bf9\u79f0\u6027\u4e0d\u662f\u7279\u522b\u7406\u60f3\uff0c\u6211\u4eec\u5728\u5206\u6790\u7ec7\u6784\u65f6\u4e5f\u4e0d\u5fc5\u8981\u523b\u610f\u6c42\u5bf9\u79f0\u6027\uff0c\u53ef\u4ee5\u5047\u60f3\u67d0\u51e0\u4e2a\u70b9\u65cb\u8f6c\u67d0\u4e00\u89d2\u5ea6\u5bf9\u79f0\u5373\u53ef\u3002<\/p>\n<p>\u56fe8\u00a0\u7acb\u65b9\u7ed3\u6784\u6781\u56fe\u7684\u5206\u6790<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180984 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72478-13.png\" alt=\"\" width=\"680\" height=\"269\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72478-13.png 680w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72478-13-300x119.png 300w\" sizes=\"(max-width: 680px) 100vw, 680px\" \/><\/p>\n<p>\u4e3e\u4f8b3\uff1a\u5982\u56fe9\u6240\u793a\uff0c\u7ea2\u8272\u7684\u4e24\u90e8\u5206\u660e\u663e\u5bf9\u79f0\uff0c\u800c\u9ec4\u8272\u7684\u5e76\u4e0d\u5bf9\u79f0\uff0c\u4f46\u662f\u516d\u65b9\u6676\u7cfb\u7684\u7ec7\u6784\u4e00\u822c\u662f\u5bf9\u79f0\u7684\uff0c\u6240\u4ee5\u6211\u4eec\u53ef\u4ee5\u6839\u636e\u6781\u56fe\u7684\u60c5\u51b5\u5047\u8bbe\u56db\u70b9\u5bf9\u79f0\uff0c\u4ece\u800c\u6c42\u51fa\u6676\u5411\u6307\u6570\u4e0e\u6676\u9762\u6307\u6570\u3002\u56fe\u4e2d\u7ea2\u8272\u90e8\u5206\u7ec7\u6784\u4e3a\uff1a\uff0811-20\uff09[1-100]\u3002\u84dd\u8272\u90e8\u5206\u7ec7\u6784\u4e3a\uff1a(11-20) [3-302].<\/p>\n<p>\u56fe9\u00a0\u949b\u5408\u91d1\uff080001\uff09\u548c\uff0810-10\uff09\u6781\u56fe\u5206\u6790<sup>[3]<\/sup><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180985 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u72479-11.png\" alt=\"\" width=\"259\" height=\"202\" \/>B. \u53cd\u6781\u56fe\u7684\u5206\u6790\u65b9\u6cd5<\/p>\n<p>\u53cd\u6781\u56fe\u4e0e\u6781\u56fe\u6b63\u597d\u76f8\u53cd\uff0c\u5b83\u8868\u793a\u5404\u6676\u7c92\u5bf9\u5e94\u7684\u5916\u89c2\u65b9\u5411\uff08\u5982\u8f67\u9762\u7684\u6a2a\u5411\u3001\u8f67\u5411\u548c\u6cd5\u5411\uff09\u5728\u6676\u4f53\u5b66\u53d6\u5411\u5750\u6807\u7cfb\u4e2d\u6240\u505a\u7684\u6295\u5f71\u3002\u53cd\u6781\u56fe\u7279\u522b\u9002\u5408\u5206\u6790\u4e1d\u7ec7\u6784\u3002\u4f8b\u5982\u56fe10\u6240\u793a\u4e3a\u7acb\u65b9\u6750\u6599\u5728XO\u3001YO\u3001ZO\u4e09\u4e2a\u65b9\u5411\u6240\u5f97\u53cd\u6781\u56fe\u3002\u53ef\u4ee5\u770b\u51fa\uff0c\u53cd\u6781\u56fe\u4e2dXO\u548cZO\u65b9\u5411\u7684&lt;101&gt;\u548c&lt;111&gt;\u65b9\u5411\u7ec7\u6784\u5bc6\u5ea6\u6700\u5927.\u6240\u4ee5\u6750\u6599\u4e2d\u5b58\u5728&lt;101&gt;\/\/XO\u4e0e&lt;111&gt;\/\/ZO\u4e24\u79cd\u4e1d\u7ec7\u6784\u3002\u53cd\u6781\u56fe\u7684\u5206\u6790\u65b9\u6cd5\u6bd4\u8f83\u7b80\u5355\uff0c\u7279\u522b\u9700\u8981\u6ce8\u610f\u7684\u662f\u5982\u679c\u8981\u5206\u6790\u677f\u7ec7\u6784\uff0c\u5219\u9700\u8981\u4e09\u4e2a\u65b9\u5411\u7684\u53cd\u6781\u56fe\u3002\u5b9e\u9645\u4e2d\u5982\u679c\u6750\u6599\u4e2d\u5b58\u5728\u53cd\u6781\u56fe\uff0c\u7b14\u8005\u5efa\u8bae\u8fd8\u662f\u5229\u7528\u6781\u56fe\u8fdb\u884c\u5206\u6790\u3002<\/p>\n<p>\u56fe10 \u53cd\u6781\u56fe\u7684\u5206\u6790<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180986 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724710-11.png\" alt=\"\" width=\"680\" height=\"235\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724710-11.png 680w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u56fe\u724710-11-300x104.png 300w\" sizes=\"(max-width: 680px) 100vw, 680px\" \/><\/p>\n<p>3\uff09\u9644\u4ef6\uff0c\u7acb\u65b9\u6676\u7cfb\u548c\u516d\u65b9\u6676\u7cfb\u7684\u6676\u9762\u5939\u89d2<\/p>\n<p>\u6781\u56fe\u7684\u5206\u6790\u4e3b\u8981\u96be\u70b9\u662f\u662f\u6676\u9762\u65cf\u4e4b\u95f4\u5939\u89d2\u7684\u8ba1\u7b97\uff0c\u867d\u7136\u8bfe\u672c\u4e0a\u7ed9\u51fa\u4e86\u516c\u5f0f\uff0c\u4f46\u662f\u5f88\u591a\u540c\u5b66\u4f9d\u7136\u4e0d\u80fd\u591f\u6b63\u786e\u8ba1\u7b97\uff0c\u7b14\u8005\u4eca\u5929\u5c31\u5217\u51fa\u7acb\u65b9\u6676\u80de\u5404\u6676\u9762\u65cf\u4e4b\u95f4\u7684\u5939\u89d2\uff0c\u5728\u5217\u51fa\u516d\u65b9\u6676\u7cfb\u5178\u578b\u6676\u9762\u65cf\u4e4b\u95f4\u7684\u5939\u89d2<sup>[<\/sup><sup>4]<\/sup>\uff0c\u4ee5\u63d0\u4f9b\u7ed9\u5927\u5bb6\u65b9\u4fbf\u3002<\/p>\n<p>\u88681\u00a0\u7acb\u65b9\u7ed3\u6784\u5404\u6676\u9762\u65cf\u4e4b\u95f4\u7684\u5939\u89d2<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180987 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u88681.png\" alt=\"\" width=\"472\" height=\"680\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u88681.png 472w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u88681-208x300.png 208w\" sizes=\"(max-width: 472px) 100vw, 472px\" \/><\/p>\n<p>\u88682\u00a0\u5bc6\u6392\u516d\u65b9\u5178\u578b\u6676\u9762\u65cf\u4e4b\u95f4\u7684\u5939\u89d2<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-180996 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u88682-1.png\" alt=\"\" width=\"550\" height=\"336\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u88682-1.png 550w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/07\/\u88682-1-300x183.png 300w\" sizes=\"(max-width: 550px) 100vw, 550px\" \/><\/p>\n<p><strong><b>\u53c2\u8003\u6587\u732e\uff1a<\/b><\/strong><\/p>\n<p>[1] \u6768\u5e73\uff0c\u7535\u5b50\u80cc\u6563\u5c04\u6280\u672f\u53ca\u5176\u5e94\u7528\uff0c\u51b6\u91d1\u5de5\u4e1a\u51fa\u7248\u793e\uff1b<\/p>\n<p>[2] \u9648\u4eae\u7ef4\uff0c\u53f2\u5e86\u96be\uff0c\u738b\u5251\u534e\u7b49\uff0c\u4e00\u79cd\u6676\u4f53\u7ec7\u6784\u6781\u56fe\u7684\u5206\u6790\u65b9\u6cd5\uff1b<\/p>\n<p>[3]\u00a0Peng Lin, AihanFeng , ShijianYuan et al; Microstructure and texture evolution of a near-a titanium alloy during hot deformation. Materials Science &amp; Engineering A. 563 (2013) 16\u201320<\/p>\n<p>[4] \u9648\u4eae\u7ef4,\u970d\u5e7f\u9e4f\uff0c\u865e\u6f9c\u7b49\uff0c\u91d1\u5c5e\u9506\u7ec7\u6784\u7684\u6807\u51c6\u6781\u56fe\u53ca\u5206\u6790\uff0c\u6606\u660e\u7406\u5de5\u5927\u5b66\u5b66\u62a5\u3002<\/p>\n<p>\u672c\u6587\u7531\u865a\u8c37\u7eb3\u7269\u4f9b\u7a3f\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u6676\u4f53\u5b66\u53d6\u5411\u662f\u6750\u6599\u5b66\u79d1\u4e2d\u7684\u91cd\u8981\u5206\u652f\uff0c\u5f53\u6676\u7c92\u53d1\u751f\u62e9\u4f18\u53d6\u5411\u65f6\uff0c\u5219\u5bfc\u81f4\u6750\u6599\u6027\u80fd\uff08\u529b\u5b66\uff0c\u7269\u7406\u548c\u5316\u5b66\u6027\u80fd\uff09\u7684\u5404\u5411\u5f02\u6027\u3002\u5404\u5411\u5f02\u6027\u4f1a\u9020\u6210\u6750\u6599\u5b9e\u9645\u5e94\u7528\u4e2d\u7684\u5404\u79cd\u95ee\u9898\uff0c\u5982\u94dd\u5408\u91d1\u5178\u578b\u7684&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":180991,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[4],"tags":[],"class_list":["post-180973","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-ganhuo"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/180973"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=180973"}],"version-history":[{"count":7,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/180973\/revisions"}],"predecessor-version":[{"id":181045,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/180973\/revisions\/181045"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/180991"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=180973"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=180973"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=180973"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}