{"id":187918,"date":"2019-11-06T06:30:28","date_gmt":"2019-11-05T22:30:28","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=187918"},"modified":"2019-11-05T20:07:19","modified_gmt":"2019-11-05T12:07:19","slug":"%e3%80%90%e5%b7%b2%e6%a0%a1%e7%a8%bf%e3%80%91%e5%8c%97%e4%ba%ac%e5%8c%96%e5%b7%a5%e5%a4%a7%e5%ad%a6%e9%bb%84%e4%b8%96%e8%90%8d%e5%9b%a2%e9%98%9facs-catalysis%ef%bc%9a%e5%90%8c%e6%97%b6%e5%ae%9e","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=187918","title":{"rendered":"\u5317\u4eac\u5316\u5de5\u5927\u5b66\u9ec4\u4e16\u840d\u56e2\u961fACS Catalysis\uff1a\u540c\u65f6\u5b9e\u73b0\u5355\u539f\u5b50\u50ac\u5316\u5242\u4e8c\u7535\u5b50O2\u7535\u8fd8\u539f\u7684\u9ad8\u6d3b\u6027\u548c\u9009\u62e9\u6027"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u5229\u7528\u7535\u5316\u5b66\u65b9\u6cd5\u73b0\u573a\u751f\u4ea7\u8fc7\u6c27\u5316\u6c22\uff08H<sub>2<\/sub>O<sub>2<\/sub>\uff09\u53ef\u80fd\u6bd4\u76ee\u524d\u7684\u5de5\u4e1a\u751f\u4ea7\u8fc7\u7a0b\u66f4\u6709\u6548\u3002\u7136\u800c\uff0c\u7531\u4e8e\u5b58\u5728\u5438\u9644\u53cd\u5e94\u4e2d\u95f4\u4f53\u7684\u6bd4\u4f8b\u5173\u7cfb\uff0c\u50ac\u5316\u5242\u7684\u6d3b\u6027\u548c\u9009\u62e9\u6027\u4e4b\u95f4\u5b58\u5728\u7740\u957f\u671f\u7684\u5e73\u8861\uff0c\u56e0\u4e3a\u50ac\u5316\u6d3b\u6027\u7684\u63d0\u9ad8\u901a\u5e38\u662f\u4f34\u968f\u7740\u56db\u7535\u5b50O<sub>2<\/sub>\u8fd8\u539f\u53cd\u5e94\uff08ORR\uff09\uff0c\u5bfc\u81f4\u751f\u4ea7\u8fc7\u6c27\u5316\u6c22\u7684\u9009\u62e9\u6027\u964d\u4f4e\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong><b>\u5317\u4eac\u5316\u5de5\u5927\u5b66\u9ec4\u4e16\u840d\u6559\u6388\u3001\u5357\u4eac\u7406\u5de5\u5927\u5b66\u5f20\u80dc\u5229\u6559\u6388<\/b><\/strong>\u548c<strong><b>\u7f8e\u56fd\u6ce2\u591a\u9ece\u5404\u5927\u5b66\u9648\u4e2d\u65b9\u6559\u6388\u56e2\u961f\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09<\/b><\/strong>\u8fdb\u884c\u5408\u4f5c\uff0c\u901a\u8fc7\u5bc6\u5ea6\u6cdb\u51fd\u7406\u8bba\uff08DFT\uff09\u8ba1\u7b97\uff0c\u62a5\u544a\u4e86\u51e0\u7c7b\u91cd\u8981\u4e14\u6709\u4ee3\u8868\u6027\u7684\u5355\u539f\u5b50\u50ac\u5316\u5242\uff08SACs\uff09\u5e94\u7528\u4e8e\u4e8c\u7535\u5b50ORR\u7684\u53ef\u884c\u6027\uff0c\u5e76\u5173\u6ce8\u4e86\u5b83\u4eec\u5728\u9178\u6027\u4ecb\u8d28\u4e2d\u7684\u7a33\u5b9a\u6027\uff0c\u9009\u62e9\u6027\u548c\u6d3b\u6027\u3002\u4ece210\u4e2a\u4e8c\u7ef4\uff082D\uff09SACs\u5f00\u59cb\uff0c\u8bc1\u660e\u4e86SACs\u5177\u6709\u6253\u7834\u91d1\u5c5e\u7ed3\u57a2\u5173\u7cfb\u7684\u6f5c\u529b\uff0c\u540c\u65f6\u5bf9H<sub>2<\/sub>O<sub>2<\/sub>\u7684\u4ea7\u751f\u5177\u6709\u9ad8\u6d3b\u6027\u548c\u9009\u62e9\u6027\uff0c\u5e76\u5728\u9178\u6027\u4ecb\u8d28\u4e2d\u7b5b\u9009\u51fa\u4e867\u4e2a\u6bd4PtHg<sub>4<\/sub>\u6d3b\u6027\u66f4\u9ad8\u7684SACs\u3002\u5c24\u5176\u662f\u975e\u8d35\u91d1\u5c5e\u7684SAC\uff0c\u5373\u5355Zn\u539f\u5b50\u4e3a\u4e2d\u5fc3\u7684\u915e\u83c1\uff08Zn@Pc-N<sub>4<\/sub>\uff09\uff0c\u5176\u6d3b\u6027\u6539\u5584\u663e\u8457\uff0c\u4e14\u8fc7\u7535\u4f4d\u4ec5\u4e3a0.15V\u3002\u6b64\u5916\uff0c\u4f7f\u7528\u591a\u53d8\u91cf\u5206\u6790\u548c\u673a\u5668\u5b66\u4e60\u6280\u672f\uff0c\u56e2\u961f\u5168\u9762\u4e86\u89e3\u4e86SACs\u9009\u62e9\u6027\u548c\u6d3b\u6027\u7684\u6f5c\u5728\u6765\u6e90\uff0c\u5e76\u63ed\u793a\u4e86\u7ed3\u6784\u4e0e\u50ac\u5316\u6027\u80fd\u4e4b\u95f4\u7684\u5185\u5728\u8054\u7cfb\u3002\u8fd9\u9879\u5de5\u4f5c\u53ef\u80fd\u4e3a\u8bbe\u8ba1\u548c\u53d1\u73b0\u66f4\u6709\u524d\u9014\u7684\u751f\u4ea7H<sub>2<\/sub>O<sub>2<\/sub>\u6750\u6599\u94fa\u5e73\u9053\u8def\u3002\u76f8\u5173\u6210\u679c\u4ee5\u9898\u4e3a<strong><b>\u201cSimultaneously Achieving High Activity and Selectivity towards Two-Electron O<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u00a0Electroreduction: the Power of Single-Atom Catalysts\u201d<\/b><\/strong>\u53d1\u8868\u5728\u4e86<strong><b>ACS Catalysis<\/b><\/strong>\u4e0a\u3002\u8bba\u6587\u7684\u7b2c\u4e00\u4f5c\u8005\u4e3a\u5317\u4eac\u5316\u5de5\u5927\u5b66\u535a\u58eb\u751f<strong><b>\u90ed\u7fd4\u5b87<\/b><\/strong>\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u53cd\u5e94\u9014\u5f84\u4ee5\u53caO<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u7684\u7535\u8fd8\u539f<\/b><\/strong><b><\/b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187919\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/1-27.jpg\" alt=\"\" width=\"600\" height=\"305\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/1-27.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/1-27-300x153.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe2<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u7535\u5316\u5b66\u5408\u6210H<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>O<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u7684SACs\u7684\u53d1\u73b0\u548c\u8bbe\u8ba1\u793a\u610f\u56fe<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187920\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/2-23.jpg\" alt=\"\" width=\"600\" height=\"445\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/2-23.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/2-23-300x223.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe3<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u4e00\u7cfb\u5217\u5355\u91d1\u5c5e\u539f\u5b50<\/b><\/strong><strong><b>\u6a21\u578b<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187921\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/3-24.jpg\" alt=\"\" width=\"600\" height=\"433\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/3-24.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/3-24-300x217.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u8003\u8651\u7684\u91d1\u5c5e\u539f\u5b50\u7c7b\u578b\u53ca\u5176\u6700\u7a33\u5b9a\u4f53\u76f8\u7ed3\u6784\u3002<\/p>\n<p>\uff08b\uff09SACs\u6a21\u578b\u793a\u610f\u56fe\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4 <\/b><\/strong><strong><b>210\u4e2aSAC<\/b><\/strong><strong><b>s<\/b><\/strong><strong><b>\u7684\u91d1\u5c5e\u539f\u5b50\u7684\u6eb6\u89e3\u52bf\uff08<\/b><\/strong><strong><em><b><i>U<\/i><\/b><\/em><\/strong><strong><em><sub><b><i>diss<\/i><\/b><\/sub><\/em><\/strong><strong><b>\uff09\u4e0e\u5f62\u6210\u80fd\uff08<\/b><\/strong><strong><em><b><i>E<\/i><\/b><\/em><\/strong><strong><em><sub><b><i>f<\/i><\/b><\/sub><\/em><\/strong><strong><b>\uff09\u7684\u5173\u7cfb<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187922\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/4-23.jpg\" alt=\"\" width=\"600\" height=\"844\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/4-23.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/4-23-213x300.jpg 213w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>5<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>O<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u7535\u8fd8\u539f\u53cd\u5e94\u548c\u5e73\u8861\u7535\u4f4d\u7684\u793a\u610f\u56fe<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187923\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/5-17.jpg\" alt=\"\" width=\"600\" height=\"766\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/5-17.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/5-17-235x300.jpg 235w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09O<sub>2<\/sub>\u7535\u8fd8\u539f\u53cd\u5e94\u548c\u5e73\u8861\u7535\u4f4d\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p>\uff08b-h\uff09149\u4e2a\u7a33\u5b9aSACs\u7684\u6c27\u539f\u5b50\u5438\u9644\u81ea\u7531\u80fd\uff08\u0394G(O*)\uff09\u3002\u6c34\u5e73\u865a\u7ebf\u8868\u793a\u4e3a\u0394G(O*)=\u0394G(H<sub>2<\/sub>O<sub>2<\/sub>)-\u0394G(H<sub>2<\/sub>O)=3.52 eV\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>6<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u5bf9\u6bd4\u4e0d\u540c\u4ea7H<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>O<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u7684SAC<\/b><\/strong><strong><b>s<\/b><\/strong><strong><b>\u6d3b\u6027<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187926\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/6-11.jpg\" alt=\"\" width=\"600\" height=\"382\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/6-11.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/6-11-300x191.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u4e0ePtHg<sub>4<\/sub>\u57fa\u51c6\uff08U<sub>L<\/sub>=0.46 V\uff09\u76f8\u6bd4\uff0c\u8ba1\u7b97\u51fa31\u4e2aSACs\u7684U<sub>L<\/sub>\u503c\u3002<\/p>\n<p>\uff08b\uff09SACs\u7684U<sub>L<\/sub>\u548c\u0394G(OOH*)\u4e4b\u95f4\u7684\u706b\u5c71\u56fe\u5173\u7cfb\u3002<\/p>\n<p>\uff08c\uff09SACs\u7684\u6d3b\u6027\u4e0e\u9009\u62e9\u6027\u7684\u53d8\u5316\u5173\u7cfb\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>7<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>H<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>O<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>\u4ea7\u751f\u7684\u6d3b\u6027\u548c\u9009\u62e9\u6027\u7684\u8d77\u6e90<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187927\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/7-5.jpg\" alt=\"\" width=\"600\" height=\"449\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/7-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/7-5-300x225.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u572831\u4e2a\u7814\u7a76\u7684SACs\u4e0a\u0394G(O*)\u548c\u0394G(OOH*)\u7684\u53d8\u5316\u3002\u6dfb\u52a0\u4e86-0.02\u548c0.17 eV\u7684\u4fee\u6b63\u503c\uff0c\u5206\u522b\u5c06\u7535\u5b50\u52bf\u8f6c\u6362\u4e3aO*\u548cOOH*\u7684\u5409\u5e03\u65af\u81ea\u7531\u80fd\u3002<\/p>\n<p>\uff08b\uff0cc\uff09O*\uff08b\uff09\u548cOOH*\uff08c\uff09\u5438\u9644\u4e2d\u56db\u4e2a\u53d8\u91cf\u7684\u6743\u91cd\u3002<\/p>\n<p>\uff08d\uff09\u0394G(O*)\u4e0eB<em><sub><i>M-O<\/i><\/sub><\/em>\u7684\u6bd4\u4f8b\u5173\u7cfb\u3002<\/p>\n<p>\uff08e\uff09\u0394G(OOH*)\u4e0eC<em><sub><i>OOH<\/i><\/sub><\/em><em><sub><i>\u2217<\/i><\/sub><\/em>\u4e4b\u95f4\u7684\u6bd4\u4f8b\u5173\u7cfb\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>8<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u5438\u9644\u5728Zn-Pc-N<\/b><\/strong><strong><sub><b>4<\/b><\/sub><\/strong><strong><b>\u548cPtHg<\/b><\/strong><strong><sub><b>4<\/b><\/sub><\/strong><strong><b>\uff08110\uff09\u8868\u9762\u4e0a\u7684O*\/OOH*\u7684COHP\u56fe<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187928\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/8-4.jpg\" alt=\"\" width=\"600\" height=\"538\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/8-4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/8-4-300x269.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u7535\u8377\u5bc6\u5ea6\u5dee\uff0c\uff08b\uff09PDOS\u548c\uff08c\uff09\u5438\u9644\u5728Zn-Pc-N<sub>4<\/sub>\u548cPtHg<sub>4<\/sub>\uff08110\uff09\u8868\u9762\u4e0a\u7684O*\/OOH*\u7684COHP\u56fe<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>9 <\/b><\/strong><strong><b>\u8bc6\u522b\u5185\u5728\u7ed3\u6784-\u9009\u62e9\u6027\u76f8\u5173\u6027<\/b><\/strong><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-187929\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/9-4.jpg\" alt=\"\" width=\"600\" height=\"270\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/9-4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/10\/9-4-300x135.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09DFT\u8ba1\u7b97\u0394G(O*)\u503c\u4e0e\u673a\u5668\u5b66\u4e60\u9884\u6d4b\u503c\u7684\u76f8\u5173\u5ea6\u5206\u6790\uff0c\u5176\u4e2d\u5305\u542b\u8bad\u7ec3\u548c\u6d4b\u8bd5\u6570\u636e\u70b9\u3002<\/p>\n<p>\uff08b\uff09\u672c\u5f81\u7ed3\u6784\u7b26\u5728\u968f\u673a\u68ee\u6797\u6a21\u578b\u9884\u6d4b\u0394G(O*)\u4e2d\u7684\u6743\u91cd\u3002<\/p>\n<p>\u3010<strong><b>\u5c0f\u7ed3<\/b><\/strong>\u3011<\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u56e2\u961f\u901a\u8fc7\u81ea\u65cb\u6781\u5316DFT\u8ba1\u7b97\u548c\u70ed\u529b\u5b66\u5206\u6790\uff0c\u5168\u9762\u4ecb\u7ecd\u4e86\u5b9e\u9a8c\u53ef\u7528\u7684\u5355\u539f\u5b50\u7535\u50ac\u5316\u5242\u5728H<sub>2<\/sub>O<sub>2<\/sub>\u751f\u4ea7\u4e2d\u7684\u5e94\u7528\u3002\u8bc1\u660e\u4e86\u603b\u517131\u79cdSACs\u4e0d\u4ec5\u53ef\u4ee5\u589e\u5f3aOOH*\u5bf9\u91d1\u5c5e\u8868\u9762\u7684\u5438\u9644\uff0c\u800c\u4e14\u53ef\u4ee5\u6291\u5236O*\u5bf9\u91d1\u5c5e\u8868\u9762\u7684\u5438\u9644\uff0c\u4ece\u800c\u4ea7\u751f\u9ad8\u9009\u62e9\u6027\u7684H<sub>2<\/sub>O<sub>2<\/sub>\u3002\u7279\u522b\u7684\uff0c\u4ee5Zn\u539f\u5b50\u4e3a\u4e2d\u5fc3\u7684\u915e\u83c1\uff08Zn@PcN<sub>4<\/sub>\uff09\u5177\u6709\u4f18\u5f02\u7684\u6d3b\u6027\uff0c\u5176\u8d85\u4f4e\u8fc7\u7535\u4f4d\u4e3a0.15 V\uff0c\u53ef\u4e0e\u5df2\u62a5\u9053\u7684PtHg<sub>4<\/sub>\u50ac\u5316\u5242\u76f8\u5ab2\u7f8e\u3002\u540c\u65f6\uff0c\u91d1\u5c5e\u539f\u5b50\u7684\u9ad8\u70ed\u529b\u5b66\u548c\u7535\u5316\u5b66\u7a33\u5b9a\u6027\u53ef\u6709\u6548\u907f\u514d\u56e2\u805a\u548c\u6eb6\u89e3\uff0c\u4ece\u800c\u4f7fZn@Pc-N<sub>4<\/sub>\u6210\u4e3a\u51fa\u8272\u7684\u4e24\u7535\u5b50O<sub>2<\/sub>\u8fd8\u539f\u7535\u50ac\u5316\u5242\u3002\u6b64\u5916\uff0c\u901a\u8fc7\u4f7f\u7528\u673a\u5668\u5b66\u4e60\u65b9\u6cd5\u8fdb\u884c\u591a\u53d8\u91cf\u5206\u6790\uff0c\u63ed\u793a\u4e86SACs\u9009\u62e9\u6027\u548c\u6d3b\u6027\u7684\u6f5c\u5728\u8d77\u6e90\uff0c\u5305\u62ec\u91d1\u5c5e\u4e0eO*\u5438\u9644\u7269\u79cd\u7684\u8f68\u9053\u6742\u5316\u4ee5\u53caSACs\u548cOOH*\u4e4b\u95f4\u7684\u7535\u8377\u8f6c\u79fb\uff0c\u5e76\u63d0\u51fa\u4e86\u8bc6\u522bSACs\u4e0eOOH*\u4e2d\u95f4\u4f53\u4e4b\u95f4\u5185\u5728\u76f8\u5173\u6027\u7684\u4e00\u822c\u7b56\u7565\u3002\u56e2\u961f\u76f8\u4fe1\u8fd9\u9879\u5de5\u4f5c\u5c06\u6709\u52a9\u4e8e\u6307\u5bfc\u7a33\u5b9a\u548c\u9ad8\u6548SACs\u7684\u8bbe\u8ba1\u548c\u53d1\u73b0\uff0c\u4ee5\u76f4\u63a5\u751f\u4ea7H<sub>2<\/sub>O<sub>2<\/sub>\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><a href=\"https:\/\/pubs-acs-org.uchile.idm.oclc.org\/doi\/10.1021\/acscatal.9b02778\" target=\"_blank\" rel=\"noopener\"><u>Simultaneously Achieving High Activity and Selectivity towards Two-Electron O<\/u><u><sub>2<\/sub><\/u><u>\u00a0Electroreduction: the Power of Single-Atom Catalyst<\/u><strong><u><b>s<\/b><\/u><\/strong><\/a>\uff08ACS Catalysis\uff0c\u00a02019\uff0c\u00a0DOI:10.1021\/acscatal.9b02778\uff09<\/p>\n<p>\u672c\u6587\u7531<strong><b>\u6728\u6587\u97ec<\/b><\/strong>\u7ffb\u8bd1\uff0c<strong>\u5317\u4eac\u5316\u5de5\u5927\u5b66\u535a\u58eb\u751f<b>\u90ed\u7fd4\u5b87<\/b><\/strong>\u4fee\u6b63\u4f9b\u7a3f<strong><b>\uff0c<\/b><\/strong>\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u5229\u7528\u7535\u5316\u5b66\u65b9\u6cd5\u73b0\u573a\u751f\u4ea7\u8fc7\u6c27\u5316\u6c22\uff08H2O2\uff09\u53ef\u80fd\u6bd4\u76ee\u524d\u7684\u5de5\u4e1a\u751f\u4ea7\u8fc7\u7a0b\u66f4\u6709\u6548\u3002\u7136\u800c\uff0c\u7531\u4e8e\u5b58\u5728\u5438\u9644\u53cd\u5e94\u4e2d\u95f4\u4f53\u7684\u6bd4\u4f8b\u5173\u7cfb\uff0c\u50ac\u5316\u5242\u7684\u6d3b\u6027\u548c\u9009\u62e9\u6027\u4e4b\u95f4\u5b58\u5728\u7740\u957f\u671f\u7684&#8230;<\/p>\n","protected":false},"author":2109,"featured_media":187920,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[3369,2654,116,2923],"class_list":["post-187918","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-keji","tag-dft","tag-orr","tag-catalyst","tag-2923"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/187918"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2109"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=187918"}],"version-history":[{"count":5,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/187918\/revisions"}],"predecessor-version":[{"id":189255,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/187918\/revisions\/189255"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/187920"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=187918"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=187918"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=187918"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}