{"id":190040,"date":"2019-11-23T06:30:44","date_gmt":"2019-11-22T22:30:44","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=190040"},"modified":"2019-11-22T21:21:17","modified_gmt":"2019-11-22T13:21:17","slug":"%e5%b7%b2%e6%a0%a1%e7%a8%bf%e4%bb%b6-%e5%8c%97%e8%88%aa%e5%88%98%e6%ac%a2%e5%9b%a2%e9%98%9f%e5%92%8c%e6%b2%b3%e5%8d%97%e5%a4%a7%e5%ad%a6%e6%9d%9c%e7%a5%96%e4%ba%ae%e5%9b%a2%e9%98%9f%e8%81%94%e5%90%88a","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=190040","title":{"rendered":"\u5317\u822a\u5218\u6b22\u56e2\u961f\u548c\u6cb3\u5357\u5927\u5b66\u675c\u7956\u4eae\u56e2\u961f\u8054\u5408Adv. Mater.\u62a5\u9053:  \u7ea4\u7ef4\u6db2\u6865\u5f15\u5bfc\u7684\u6db2\u4f53\u8fde\u7eed\u53ef\u63a7\u8f93\u8fd0\uff1a\u9762\u5411\u9ad8\u6027\u80fdQLEDs"},"content":{"rendered":"<p><strong>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011<\/strong><\/p>\n<p>\u00a0 \u00a0 \u00a0 \u00a0 \u80f6\u4f53\u7684\u91cf\u5b50\u70b9\uff08QDs\uff09\u662f\u5177\u6709\u7a84\u5149\u8c31\u53d1\u5c04\u5e26\u5bbd\u3001\u5bbd\u5438\u6536\u7387\u3001\u9ad8\u5149\u81f4\u53d1\u5149\u91cf\u5b50\u6548\u7387\u548c\u53ef\u63a7\u5236\u5e26\u9699\u7b49\u4f18\u5f02 \u6027\u80fd\u7684\u7eb3\u7c73\u6676\u4f53\uff0c\u88ab\u5e7f\u6cdb\u7528\u4f5c\u4e0b\u4e00\u4ee3\u7167\u660e\u548c\u663e\u793a\u8bbe\u5907\u4e2d\uff0c\u6bd4\u5982\u57fa\u4e8eQDs\u7684\u53d1\u5149\u4e8c\u6781\u7ba1\u663e\u793a\u5668\uff08QLED\uff09\u3002\u5176\u4e2d\uff0cQD\u8584\u819c\u7684\u8d28\u91cf\u76f4\u63a5\u5f71\u54cd\u7740\u5668\u4ef6\u7684\u6027\u80fd\u3002QD\u8584\u819c\u7684\u539a\u5ea6\u548c\u5747\u5300\u6027\u4e0d\u4ec5\u5f71\u54cd\u8584\u819c\u7684\u7535\u8377\u8f6c\u79fb\uff0c\u800c\u4e14\u5f71\u54cd\u4e0e\u76f8\u90bb\u5c42\u7684\u7535\u8377\u5e73\u8861\uff0c\u4ece\u800c\u76f4\u63a5\u5f71\u54cd\u91cf\u5b50\u6548\u7387\u3002\u56e0\u6b64\uff0c\u9700\u8981\u5f00\u53d1\u4e00\u79cd\u7b80\u4fbf\u4e14\u4f4e\u6210\u672c\u7684\u65b9\u6cd5\u6765\u5236\u5907\u9ad8\u8d28\u91cf\u7684QD\u8584\u819c\u3002<\/p>\n<p>\u00a0 \u00a0 \u00a0 \u00a0\u76ee\u524d\uff0c\u6eb6\u6db2\u5de5\u827a\u5df2\u88ab\u5e7f\u6cdb\u7528\u4e8e\u5236\u9020QD\u8584\u819c\uff0c\u73b0\u6709\u7684\u65b9\u6cd5\u901a\u5e38\u5b58\u5728\u6216\u8005\u9ad8\u6210\u672c\u3001\u6216\u8005\u8584\u819c\u8d28\u91cf\u4f4e\u7684\u5c40\u9650\u6027\u3002\u56e0\u6b64\uff0c\u53d1\u5c55\u4e00\u79cd\u7b80\u4fbf\u7684\u65b9\u6cd5\u6765\u5236\u5907\u9ad8\u8d28\u91cf\u7684QD\u8584\u819c\uff0c\u5c24\u5176\u662f\u53ef\u4ee5\u540c\u65f6\u5b9e\u73b0\u6db2\u4f53\u53ef\u63a7\u8f93\u8fd0\u7684\u540c\u65f6\u53ef\u4ee5\u7cbe\u786e\u63a7\u5236\u6db2\u4f53\u6d88\u8017\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u5317\u4eac\u822a\u7a7a\u822a\u5929\u5927\u5b66\u7684\u5218\u6b22\u7814\u7a76\u5458\u548c\u6cb3\u5357\u5927\u5b66\u7684\u675c\u7956\u4eae\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09<\/strong>\u8054\u5408\u62a5\u9053\u4e86\u4e00\u79cd\u7531\u7ea4\u7ef4\u6db2\u6865\u5f15\u5bfc\u7684\u7b80\u4fbf\u65b9\u6cd5\uff0c\u901a\u8fc7\u4f7f\u7528\u62c9\u7d27\u7684\u7ea4\u7ef4\u548c\u6bdb\u7ec6\u7ba1\u7ed3\u5408\u5c06QD\u6eb6\u6db2\u8fde\u7eed\u4e14\u53ef\u63a7\u5236\u7684\u8f6c\u79fb\u5230\u57fa\u5e95\uff0c\u5236\u5907\u5f97\u5230\u8d85\u5149\u6ed1\u7684QD\u8584\u819c\u3002\u7ea4\u7ef4\u7684\u4e24\u7aef\u7f6e\u4e8e\u6bdb\u7ec6\u7ba1\u4e2d\uff0c\u53ef\u4ee5\u5f15\u5bfcQD\u6eb6\u6db2\u6cbf\u7740\u7ea4\u7ef4\u4ece\u6bdb\u7ec6\u7ba1\u4e2d\u6d41\u51fa\uff0c\u6cbf\u7740\u7ea4\u7ef4\u5728\u57fa\u5e95\u94fa\u5c55\uff0c\u4ece\u800c\u5728\u6c34\u5e73\u7ea4\u7ef4\u548c\u57fa\u677f\u4e4b\u95f4\u5f62\u6210\u6db2\u6865\u3002\u540c\u65f6\uff0c\u5782\u76f4\u653e\u7f6e\u7684\u6bdb\u7ec6\u7ba1\u53ef\u4ee5\u7a33\u5b9a\u7684\u5b58\u50a8\u5927\u91cf\u6db2\u4f53\uff0c\u4e14\u80fd\u6301\u7eed\u4f9b\u6db2\u4fdd\u6301\u7a33\u5b9a\u7684\u6db2\u6865\u3002\u5b9a\u5411\u79fb\u52a8\u6db2\u6865\u53ef\u5728\u57fa\u677f\u76f4\u63a5\u5236\u5907\u5927\u9762\u79ef\u9ad8\u8d28\u91cf\u7684\u8d85\u5e73\u6ed1QD\u8584\u819c\u3002\u503c\u5f97\u4e00\u63d0\u7684\u662f\uff0c\u6db2\u4f53\u6d88\u8017\u662f\u5b9a\u91cf\u7684\uff0c\u5373\u4e0e\u6240\u5236\u5907\u7684\u8584\u819c\u7684\u9762\u79ef\u6210\u6bd4\u4f8b\u3002\u6b64\u5916\uff0c\u901a\u8fc7\u5c06\u6eb6\u6db2\u4f9d\u6b21\u8f6c\u79fb\u5230\u76f8\u540c\u7684\u76ee\u6807\u533a\u57df\u4e0a\uff0c\u53ef\u4ee5\u5236\u5907\u591a\u5c42\u8d85\u5149\u6ed1\u7684\u7ea2\u8272\/\u7eff\u8272\/\u84dd\u8272QD\u8584\u819c\u3002\u6240\u5236\u5907\u7684\u767d\u8272QLEDs\u5177\u6709\u76f8\u5f53\u9ad8\u7684\u6027\u80fd\uff0c\u5176\u4e2d\u6700\u5927\u4eae\u5ea6\u4e3a57190 cd m<sup>-2<\/sup>\uff0c\u6700\u5927\u7535\u6d41\u6548\u7387\u4e3a15.868 cd A<sup>-1<\/sup>\u3002\u8be5\u7b56\u7565\u4e3a\u4f4e\u6210\u672c\u5236\u5907\u9ad8\u6027\u80fdQLEDs\u63d0\u4f9b\u4e86\u65b0\u601d\u8def\u3002\u7814\u7a76\u6210\u679c\u4ee5\u9898\u4e3a<strong>\u201cContinuous and Controllable Liquid Transfer Guided by a Fibrous Liquid Bridge: Toward High-Performance QLEDs\u201d<\/strong>\u53d1\u5e03\u5728\u56fd\u9645\u8457\u540d\u671f\u520a<strong>Adv. Mater.<\/strong> \u4e0a\u3002<strong>\u8be5\u5de5\u4f5c\u53d7\u5230\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u7684\u8d44\u52a9<\/strong>\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u89e3\u6790\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00\u3001\u5229\u7528\u7ea4\u7ef4\u6db2\u6865\u65b9\u6cd5\u5236\u5907\u8d85\u5149\u6ed1QD\u8584\u819c<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-190041\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/1-13.jpg\" alt=\"\" width=\"600\" height=\"411\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/1-13.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/1-13-300x206.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u53ef\u63a7\u6eb6\u6db2\u8f6c\u79fb\u8fc7\u7a0b\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u6240\u7528\u5c3c\u9f99\u7ea4\u7ef4\u7684\u626b\u63cf\u7535\u5b50\u663e\u5fae\u955c\u56fe\u50cf\uff1b<\/p>\n<p>\uff08c\uff09\u6db2\u4f53\u8f6c\u79fb\u8fc7\u7a0b\u7684\u5149\u5b66\u7167\u7247\uff1b<\/p>\n<p>\uff08d\uff09\u6240\u51c6\u5907\u7684\u5927\u9762\u79ef\uff0825 cm<sup>2<\/sup>\uff09\u7eff\u8272QD\u8584\u819c\u56fe\u50cf\uff1b<\/p>\n<p>\uff08e-f\uff09\u901a\u8fc7\u673a\u68b0\u8c03\u8282\u5149\u7ea4\u548c\u57fa\u677f\u4e4b\u95f4\u7684\u8ddd\u79bb\u5b9e\u73b0\u7684\u6db2\u6865\u7684\u5f62\u6210\uff08ON\uff09\u548c\u65ad\u5f00\uff08OFF\uff09\uff0c\u4ece\u800c\u8868\u660e\u6db2\u4f53\u8f6c\u79fb\u8fc7\u7a0b\u662f\u53ef\u63a7\u7684\u3002<\/p>\n<p><strong>\u56fe\u4e8c\u3001\u5bf9\u5236\u5907\u597d\u7684QD\u8584\u819c\u7684PL\u548cAFM\u8868\u5f81<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-190042\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/2-12.jpg\" alt=\"\" width=\"600\" height=\"591\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/2-12.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/2-12-300x296.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-c\uff09\u7ea2\u8272\uff08R\uff09\u3001\u7eff\u8272\uff08G\uff09\u548c\u84dd\u8272\uff08B\uff09QD\u8584\u819c\u7684PL\u56fe\u50cf\uff1b<\/p>\n<p>\uff08d-f\uff09\u7531\u4e00\u6b21\u3001\u4e24\u6b21\u548c\u4e09\u6b21\u7684\u6db2\u4f53\u8f6c\u79fb\u6240\u5236\u5907\u7684\u7eff\u8272QD\u8584\u819c\u5728\u57fa\u6750\u7684\u540c\u4e00\u76ee\u6807\u533a\u57df\u4e0a\u7684PL\u56fe\u50cf\uff1b<\/p>\n<p>\uff08g-i\uff09\u6240\u5236\u5907\u7684QD\u8584\u819c\u5177\u6709\u4e0d\u540c\u539a\u5ea6\u548c\u7c97\u7cd9\u5ea6\u7684AFM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u4e09\u3001\u7531\u7ea4\u7ef4\u6db2\u6865\u5f15\u5bfc\u7684\u6db2\u4f53\u5b9a\u91cf\u8f6c\u79fb\u7684\u8868\u5f81<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-190043\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/3-12.jpg\" alt=\"\" width=\"600\" height=\"327\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/3-12.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/3-12-300x164.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u5370\u5237\u9762\u79ef\uff08cm2\uff09\u4e0e\u8017\u6db2\u91cf\uff08\u00b5L\uff09\u4e4b\u95f4\u7684\u5173\u7cfb\u56fe\u663e\u793a\u4e3a\u51c6\u7ebf\u6027\u5173\u7cfb\u3002<\/p>\n<p>\uff08b\uff09\u5236\u5907\u9762\u79ef\u4e3a2\u30014\u30016\u30018\u300110\u548c12 cm<sup>2<\/sup>\u7684\u7eff\u8272QD\u8584\u819c\u90fd\u663e\u793a\u51fa\u76f8\u5f53\u5747\u5300\u7684\u8584\u819c\u5206\u5e03\u548c\u6e05\u6670\u7684\u8f6e\u5ed3\uff1b<\/p>\n<p>\uff08c\uff09\u79fb\u52a8\u901f\u5ea6\u548c\u6eb6\u6db2\u6d88\u8017\u4e4b\u95f4\u7684\u7ebf\u6027\u5173\u7cfb\uff1b<\/p>\n<p>\uff08d\uff09\u57281-10 mm s<sup>-1<\/sup>\u7684\u4e0d\u540c\u79fb\u52a8\u901f\u5ea6\u4e0b\uff0c\u5236\u5907\u7684QD\u8584\u819c\u7684AFM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u56db\u3001\u5229\u7528\u7ea4\u7ef4\u6db2\u6865\u8fdb\u884c\u6eb6\u6db2\u8f6c\u79fb\u7684\u673a\u7406\u793a\u610f\u56fe<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-190044\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/4-12.jpg\" alt=\"\" width=\"600\" height=\"496\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/4-12.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/4-12-300x248.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-b\uff09\u88c5\u7f6e\u7684\u5149\u5b66\u56fe\u50cf\u663e\u793a\u4e86\u5782\u76f4\u653e\u7f6e\u7684\u6bdb\u7ec6\u7ba1\u548c\u57fa\u677f\u4e4b\u95f4\u7684\u8ddd\u79bb\u4e3a<em>H<\/em><sub>1<\/sub>\uff1b<\/p>\n<p>\uff08c\uff09\u6db2\u4f53\u6865\u5728\u9ad8\u5ea6<em>H<\/em><sub>2<\/sub>\uff08<em>H<\/em><sub>2<\/sub>&gt;<em>H<\/em><sub>1<\/sub>\uff09\u7a33\u5b9a\u65f6\u7684\u88c5\u7f6e\u52a8\u753b\u548c\u5149\u5b66\u56fe\u50cf\uff1b<\/p>\n<p>\uff08d\uff09\u7ea4\u7ef4\u72b6\u6db2\u4f53\u6865\u7684\u793a\u610f\u56fe\u663e\u793a\u4e86\u8f6c\u79fb\u8fc7\u7a0b\u4e2d\u5411\u524d\u548c\u5411\u540e\u65b9\u5411\u7684\u4e0d\u5bf9\u79f0\u6027\u53ca\u5370\u5237\u51fa\u8d85\u5149\u6ed1\u8584\u819c\u7684\u539f\u7406\u3002<\/p>\n<p><strong>\u56fe\u4e94\u3001\u7eff\u8272\u3001\u7ea2\u8272\u548c\u84dd\u8272QLED\u5668\u4ef6\u7684\u6027\u80fd<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-190045\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/5-8.jpg\" alt=\"\" width=\"600\" height=\"414\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/5-8.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/5-8-300x207.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-c\uff09\u7ea2\u8272\u3001\u7eff\u8272\u548c\u84dd\u8272QLED\u5668\u4ef6\u7684\u4eae\u5ea6-\u7535\u6d41\u5bc6\u5ea6-\u7535\u538b\uff08L-J-V\uff09\u7279\u6027\uff1b<\/p>\n<p>\uff08d-f\uff09\u5bf9\u4e8e\u6548\u7387\u6700\u9ad8\u7684\u7ea2\u8272\u3001\u7eff\u8272\u548c\u84dd\u8272QLED\u5668\u4ef6\uff0cCE\u548cEQE\u4e0e\u4eae\u5ea6\u7684\u5173\u7cfb\uff1b<\/p>\n<p>\uff08g-i\uff09\u968f\u7740\u9a71\u52a8\u7535\u538b\u7684\u589e\u52a0\uff0c\u4e09\u4e2a\u5f69\u8272QLED\u5668\u4ef6\u7684EL\u5149\u8c31\u6f14\u5316\uff0c\u4ee5\u53ca\u57284 V\u4e0b\u5de5\u4f5c\u5668\u4ef6\u7684\u76f8\u5e94\u7535\u81f4\u53d1\u5149\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u516d\u3001\u767d\u8272QLED\u5668\u4ef6\u7684\u6027\u80fd<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-190046\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/6-3.jpg\" alt=\"\" width=\"600\" height=\"278\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/6-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/11\/6-3-300x139.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u767d\u8272QD\u8584\u819c\u7684PL\u56fe\u50cf\uff1b<\/p>\n<p>\uff08b\uff09\u767d\u8272QD\u8584\u819c\u7684\u5f52\u4e00\u5316EL\u5149\u8c31\uff1b<\/p>\n<p>\uff08c\uff09\u57fa\u4e8e\u591a\u5c42\u7eff\u8272\/\u7ea2\u8272\/\u84dd\u8272QD\u8584\u819c\u7684\u767d\u8272QLED\u5668\u4ef6\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08d\uff09\u5177\u6709\u9ad8\u6027\u80fd\u7684\u767d\u8272QLED\u5668\u4ef6\u7684L-J-V\u7279\u6027\uff1b<\/p>\n<p>\uff08e\uff09\u5bf9\u4e8e\u6548\u7387\u6700\u9ad8\u7684\u767d\u8272QLED\uff0cCE\u548cEQE\u4e0e\u4eae\u5ea6\u7684\u5173\u7cfb\uff1b<\/p>\n<p>\uff08f\uff09\u767d\u8272QLED\u5f52\u4e00\u5316\u7535\u81f4\u53d1\u5149\u5149\u8c31\u4ee5\u53ca\u57284 V\u4e0b\u5de5\u4f5c\u7684\u8bbe\u5907\u7684\u76f8\u5e94\u5149\u5b66\u7535\u81f4\u53d1\u5149\u56fe\u50cf\u3002<\/p>\n<p><strong>\u3010\u603b\u7ed3\u3011<\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u4f5c\u8005\u62a5\u9053\u4e86\u4e00\u79cd\u7cbe\u51c6\u3001\u8fde\u7eed\u4e14\u53ef\u63a7\u7684\u6eb6\u6db2\u8f6c\u79fb\u7b56\u7565\uff0c\u5229\u7528\u7ea4\u7ef4\u6db2\u6865\u5f15\u5bfc\u5b9e\u73b0\u6db2\u4f53\u7684\u53ef\u63a7\u8f6c\u79fb\uff0c\u5236\u5907\u5f97\u5230\u8d85\u5149\u6ed1QD\u8584\u819c\u3002\u5e76\u4e14\uff0c\u8be5\u8fc7\u7a0b\u53ef\u4ee5\u5b9e\u73b0\u5bf9\u6eb6\u6db2\u7684\u5b9a\u91cf\u63a7\u5236\uff0c\u5373QD\u6eb6\u6db2\u7684\u6d88\u8017\u4e0e\u6240\u5236\u5907\u7684\u8584\u819c\u7684\u9762\u79ef\u6210\u6bd4\u4f8b\u3002\u6b64\u5916\uff0c\u8be5\u6280\u672f\u53ef\u4ee5\u5c06\u591a\u79cd\u6eb6\u6db2\u8f6c\u79fb\u5230\u540c\u4e00\u76ee\u6807\u533a\u57df\uff0c\u4ece\u800c\u53ef\u4ee5\u4f9d\u6b21\u5370\u5237\u8d85\u5149\u6ed1\u7684\u7ea2\u8272\u3001\u7eff\u8272\u548c\u84dd\u8272QD\u8367\u5149\u8584\u819c\u6765\u5236\u5907\u767d\u5149\u8584\u819c\uff0c\u5e76\u4e14\u6240\u5236\u5907\u7684QLED\u5668\u4ef6\u5177\u6709\u76f8\u5f53\u9ad8\u7684\u6027\u80fd\u3002\u8be5\u7b56\u7565\u4e3a\u6eb6\u6db2\u6cd5\u5236\u5907\u9ad8\u6027\u80fdQLED\u5668\u4ef6\u63d0\u4f9b\u4e86\u65b0\u7684\u601d\u8def\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/abs\/10.1002\/adma.201904610\" target=\"_blank\" rel=\"noopener\">Continuous and Controllable Liquid Transfer Guided by a Fibrous Liquid Bridge: Toward High-Performance QLEDs<\/a><\/strong>\uff08<em>Adv. Mater.<\/em>, <strong>2019<\/strong>, DOI: 10.1002\/adma.201904610\uff09<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011 \u00a0 \u00a0 \u00a0 \u00a0 \u80f6\u4f53\u7684\u91cf\u5b50\u70b9\uff08QDs\uff09\u662f\u5177\u6709\u7a84\u5149\u8c31\u53d1\u5c04\u5e26\u5bbd\u3001\u5bbd\u5438\u6536\u7387\u3001\u9ad8\u5149\u81f4\u53d1\u5149\u91cf\u5b50\u6548\u7387\u548c\u53ef\u63a7\u5236\u5e26\u9699\u7b49\u4f18\u5f02 \u6027\u80fd\u7684\u7eb3\u7c73\u6676\u4f53\uff0c\u88ab\u5e7f\u6cdb\u7528\u4f5c\u4e0b\u4e00\u4ee3\u7167\u660e\u548c&#8230;<\/p>\n","protected":false},"author":7770,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215,2],"tags":[4244],"class_list":["post-190040","post","type-post","status-publish","format-standard","hentry","category-jiedu","category-keji","tag-qd"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/190040"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7770"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=190040"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/190040\/revisions"}],"predecessor-version":[{"id":190689,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/190040\/revisions\/190689"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=190040"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=190040"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=190040"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}