{"id":192198,"date":"2020-01-21T06:09:47","date_gmt":"2020-01-20T22:09:47","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=192198"},"modified":"2020-01-20T22:10:13","modified_gmt":"2020-01-20T14:10:13","slug":"tial%e5%90%88%e9%87%91%e7%9a%84%e5%8f%91%e5%b1%95%e5%8e%86%e7%a8%8b%e5%8f%8a%e5%ba%94%e7%94%a8%e5%89%8d%e6%99%af","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=192198","title":{"rendered":"TiAl\u5408\u91d1\u7684\u53d1\u5c55\u5386\u7a0b\u53ca\u5e94\u7528\u524d\u666f"},"content":{"rendered":"<p>\u968f\u7740\u822a\u7a7a\u5de5\u4e1a\u7684\u5feb\u901f\u53d1\u5c55\uff0c\u5bf9\u6750\u6599\u7684\u8981\u6c42\u4e5f\u8d8a\u6765\u8d8a\u9ad8\uff0c\u76ee\u524d\uff0c\u5176\u7ed3\u6784\u6750\u6599\u6b63\u5728\u671d\u7740\u201c\u66f4\u5f3a\u66f4\u8f7b\u201d\u7684\u65b9\u5411\u53d1\u5c55\uff0c\u66f4\u8f7b\u7684\u6750\u6599\u610f\u5473\u7740\u98de\u673a\u80fd\u591f\u975e\u5f97\u66f4\u9ad8\u4e14\u53ef\u4ee5\u6709\u6548\u51cf\u5c11CO<sub>2<\/sub>\u7684\u6392\u653e\u3002\u91d1\u5c5e\u95f4\u5316\u5408\u7269\u03b3-TiAl\u5408\u91d1\u5177\u6709\u8bb8\u591a\u4f18\u5f02\u7684\u6027\u80fd\uff0c\u5982\u6bd4\u5f3a\u5ea6\u9ad8\uff0c\u8d28\u91cf\u8f7b\uff0c\u8010\u9ad8\u6e29\u4ee5\u53ca\u826f\u597d\u7684\u9ad8\u6e29\u6297\u8815\u53d8\u6027\u80fd\u7b49\u3002\u53ef\u4ee5\u5f88\u597d\u5730\u6ee1\u8db3\u822a\u7a7a\u4ee5\u53ca\u81ea\u52a8\u5316\u5de5\u4e1a\u7684\u9700\u6c42\uff0c\u662f\u8fd1\u51e0\u5e74\u6765\u7684\u70ed\u70b9\u91d1\u5c5e\u6750\u6599\u4e4b\u4e00\uff0c\u53d7\u5230\u4e86\u822a\u7a7a\u5de5\u4e1a\u7684\u9752\u7750\u3002\u867d\u7136TiAl\u57fa\u5408\u91d1\u6709\u8bb8\u591a\u4f18\u70b9\uff0c\u5e76\u5728\u6280\u672f\u4e0a\u53d6\u5f97\u4e86\u8bb8\u591a\u91cd\u8981\u7a81\u7834\uff0c\u4f46\u4ecd\u6709\u8bb8\u591a\u6027\u80fd\u65b9\u9762\u7684\u95ee\u9898\u9700\u8981\u89e3\u51b3\uff0c\u6bd4\u5982TiAl\u5408\u91d1\u4f4e\u7684\u5ba4\u6e29\u5851\u6027\u53ca\u4f34\u968f\u800c\u6765\u7684\u6210\u5f62\u6027\u5dee\uff0c\u5bf9\u4e8e1000\u2103\u4ee5\u4e0a\u4f7f\u7528\u7684\u9ad8\u6e29\u90e8\u4ef6\u5177\u6709\u76f8\u5bf9\u8f83\u4f4e\u7684\u9ad8\u6e29\u5f3a\u5ea6\uff0c800\u2103\u4ee5\u4e0a\u7684\u6297\u6c27\u5316\u6027\u80fd\u4e0d\u8db3\uff0c\u62c9\u4f38\u5f3a\u5ea6\u3001\u5851\u6027\u4e0e\u65ad\u88c2\/\u8815\u53d8\u6297\u529b\u5177\u6709\u76f8\u53cd\u5173\u7cfb\u7b49\uff0c\u6240\u4ee5\u5176\u5e94\u7528\u53d7\u5230\u4e00\u5b9a\u9650\u5236\uff0c\u4e0b\u9762\u6211\u4eec\u770b\u770b\u8fd9\u79cd\u6750\u6599\u7684\u53d1\u5c55\u5386\u7a0b\u548c\u5e94\u7528\u524d\u666f\u3002<\/p>\n<h3>1.\u7b2c\u4e00\u4ee3TiAl\u5408\u91d1<\/h3>\n<p>\u7b2c\u4e00\u4ee3TiAl\u5408\u91d1\u4e3b\u8981\u4e3a\u03b3-TiAl\u5408\u91d1\uff0c\u987e\u540d\u601d\u4e49\uff0c\u8fd9\u7c7b\u5408\u91d1\u4e3b\u8981\u7684\u76f8\u6210\u5206\u4e3a\u03b3\u76f8\uff0c\u5916\u52a0\u5c11\u91cf\u03b1<sub>2<\/sub>\u76f8\uff0c\u6240\u4ee5\u8fd9\u7c7b\u5408\u91d1\u4e00\u822cAl\u5143\u7d20\u7684\u542b\u91cf\u8f83\u9ad8\uff08\u767e\u5206\u542b\u91cf\u572846~48%\u4e4b\u95f4\uff09\uff0c\u5916\u52a0\u5c11\u91cf\u03b2\u7a33\u5b9a\u5143\u7d20\uff0c\u5982Cr\u3001Mn\u3001V\u7b49\u3002\u7ecf\u5178\u7684\u5408\u91d1\u4e3a\u7f8e\u56fd\u751f\u4ea7\u7684Ti-48Al-1V-0.5C\u5408\u91d1\uff08\u901a\u5e38\u8ba4\u4e3a\u8fd9\u662f\u7b2c\u4e00\u4ee3TiAl \u5408\u91d1\u7684\u4ee3\u8868\uff09\uff0cTi-46.5Al-4(Cr\u3001Mn\u3001Ta)\u7b49\u5408\u91d1\u3002\u4e4b\u540e\u5f00\u5c55\u4e86\u4e00\u7cfb\u5217\u529b\u5b66\u6027\u80fd\u3001\u6210\u5f62\u5de5\u827a\u548c\u5178\u578b\u8bd5\u9a8c\u4ef6\u7814\u7a76\u3002\u00a0\u8be5\u5408\u91d1\u65ad\u88c2\u97e7\u6027\u8f83\u597d\uff0c\u53ef\u673a\u68b0\u52a0\u5de5\uff0c\u53ef\u94f8\u9020\uff0c\u4f46\u5ba4\u6e29\u5851\u6027\u548c\u51b2\u51fb\u6027\u80fd\u8f83\u4f4e\uff0c\u94f8\u4ef6\u6613\u4ea7\u751f\u8868\u9762\u758f\u677e\u3002\u91c7\u7528\u8be5\u5408\u91d1\u94f8\u9020\u7684\u5178\u578b\u7ed3\u6784\u4ef6\u5305\u62ecF100\u53d1\u52a8\u673a\u538b\u6c14\u673a\u53f6\u7247\u6bdb\u576f\u548cJT9D\u53d1\u52a8\u673a\u4f4e\u538b\u6da1\u8f6e\u53f6\u7247\u3002\u7b2c\u4e00\u4ee3TiAl\u5408\u91d1\u53c8\u79f0\u8fd1\u03b3-TiAl\u5408\u91d1\uff0c\u5176\u53d8\u5f62\u673a\u7406\u4e3a1\/2&lt;110}{111}\u666e\u901a\u4f4d\u9519\u5916\u52a01\/2&lt;11-2}{111}\u5b6a\u6676\u53d8\u5f62\u3002\u5982figure 1\u6240\u793a\u4e3aTi-46.5Al-4(Cr\u3001Mn\u3001Ta)\u6837\u54c1\u5728\u538b\u7f29\u53d8\u5f62\u65f6\u7684\u53d8\u5f62\u673a\u7406\u3002<\/p>\n<p><strong>Figure 1 <\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-192199 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/12\/\u56fe\u72471-21.png\" alt=\"\" width=\"487\" height=\"352\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/12\/\u56fe\u72471-21.png 487w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/12\/\u56fe\u72471-21-300x217.png 300w\" sizes=\"(max-width: 487px) 100vw, 487px\" \/><\/p>\n<p>Ti-46.5Al-4(Cr\u3001Mn\u3001Ta)\u6837\u54c1\u5728\u538b\u7f295%\u65f6\u7684TEM\u7167\u7247\uff0cD\u4ee3\u8868\u4f4d\u9519\u6ed1\u79fb\uff0cT\u4ee3\u8868\u53d8\u5f62\u5b6a\u6676\uff0c\u53ef\u4ee5\u770b\u51fa\u8be5\u7c7b\u5408\u91d1\u7684\u53d8\u5f62\u673a\u7406\u4e3a\u4f4d\u9519\u52a0\u5b6a\u6676\u7684\u8fd0\u52a8\u3002<\/p>\n<h3>2.\u7b2c\u4e8c\u4ee3TiAl\u5408\u91d1<\/h3>\n<p>\u7b2c\u4e8c\u4ee3TiAl\u5408\u91d1\u4e5f\u4e3a\u03b3-TiAl\u5408\u91d1\uff0c\u4e0d\u540c\u4e4b\u5904\u5728\u4e8e\u5176\u5185\u90e8\u52a0\u5165\u4e86\u5c11\u91cf\u7684Si, B, C\u7b49\u975e\u91d1\u5c5e\u5143\u7d20\u3002 \u5176\u6210\u5206\u53ef\u4ee5\u6982\u62ec\u5982\u4e0b\uff1a<\/p>\n<p>Ti-\uff0845-48\uff09Al-\uff081-3\uff09X-\uff082-5\uff09 Y-\uff08 &lt; 1\uff09Z\uff0c<\/p>\n<p>\u5176\u4e2dX=Cr, Mn, V\uff1b Y=Nb, Ta, W, Mo\uff1b Z=Si, B, C\u3002<\/p>\n<p>\u975e\u91d1\u5c5e\u5143\u7d20\u7684\u52a0\u5165\u6709\u52a9\u4e8e\u5408\u91d1\u7ec6\u5316\u6676\u7c92\uff0c\u5c24\u5176\u662f\u5143\u7d20B\uff0c\u53ef\u4ee5\u663e\u8457\u7684\u7ec6\u5316TiAl\u5408\u91d1\u94f8\u9020\u8fc7\u7a0b\u7684\u5185\u90e8\u7ec4\u7ec7\uff0c\u4ece\u800c\u8fbe\u5230\u589e\u5f3a\u589e\u97e7\u7684\u76ee\u7684\u3002Si\u5143\u7d20\u7684\u52a0\u5165\u53ef\u4ee5\u63d0\u5347\u5408\u91d1\u7684\u8815\u53d8\u6027\u80fd\u3002C\u5143\u7d20\u7684\u6dfb\u52a0\u53ef\u4ee5\u53ef\u4ee5\u62d3\u5bbd\u03b1\u76f8\u533a\uff0c\u540c\u65f6\u51cf\u5c0f\u03b1\/\u03b3\u7684\u7247\u5c42\u7a7a\u95f4\uff0c\u5176\u4e3b\u8981\u539f\u56e0\u662fC\u7684\u6dfb\u52a0\u964d\u4f4e\u4e86\u03b3\u76f8\u7684\u5c42\u9519\u80fd\u5e76\u589e\u52a0\u4e86\u5176\u5f62\u6838\u7387\uff0c\u66f4\u5c0f\u7684\u7247\u5c42\u7a7a\u95f4\u5219\u6709\u52a9\u4e8e\u63d0\u9ad8\u5408\u91d1\u7684\u8815\u53d8\u6027\u80fd\uff0c\u5728\u67d0\u4e9b\u65f6\u5019\u8fd8\u53ef\u4ee5\u8d77\u5230\u6790\u51fa\u5f3a\u5316\u7684\u4f5c\u7528\u3002\u5728\u7b2c\u4e8c\u4ee3\u5408\u91d1\u4e2d\u6dfb\u52a0\u03b2\u7a33\u5b9a\u5143\u7d20\uff0c\u5982Nb\uff0cMo\u7b49\u53ef\u4ee5\u5c06\u03b1\u8f6c\u53d8\u7ebf\u5411\u9ad8Al\u65b9\u5411\u63a8\u8fdb\uff0c\u7f29\u5c0f\u4e86\u03b1+\u03b3\u7684\u76f8\u533a\u8303\u56f4\u3002\u901a\u8fc7\u56fa\u6eb6\u5f3a\u5316\uff0c\u8fd9\u4e9b\u5408\u91d1\u5143\u7d20\u7684\u6dfb\u52a0\u53ef\u4ee5\u63d0\u9ad8\u5408\u91d1\u7684\u5f3a\u5ea6\u3002\u57281999\u5e74\u5de6\u53f3,\u51fa\u73b0\u4e86\u5546\u7528\u03b3-TiAl\u5408\u91d1,\u65e5\u672c\u4e09\u83f1\u516c\u53f8\u9996\u6b21\u5728\u8d5b\u8f66\u7684\u6da1\u8f6e\u589e\u538b\u5668\u4e0a\u4f7f\u7528\u4e86TiAl\u5408\u91d1\uff0c2002\u5e74\u5de6\u53f3,\u4e00\u7cfb\u5217\u953b\u9020\u5904\u7406\u7684\u03b3-TiAl\u5408\u91d1\u9600\u95e8\u5e94\u8fd0\u800c\u751f\u3002\u51e0\u5e74\u540e,\u7f8e\u56fd\u822a\u7a7a\u516c\u53f8\u5ba3\u5e03\uff0c\u5176\u5236\u9020\u7684Ti-48Al-2Nb-2Cr\u5408\u91d1\u6210\u529f\u5b89\u88c5\u5728\u6ce2\u97f3784\u98de\u673a\u7684\u4f4e\u538b\u6da1\u8f6e\u53f6\u7247\u4e0a\u3002<\/p>\n<p>\u7b2c\u4e8c\u4ee3TiAl\u5408\u91d1\u81f3\u5c11\u6709\u4e00\u4e2aX\u5143\u7d20\u548c\u4e00\u4e2aY\u5143\u7d20\uff0c\u8fd9\u6837\u6dfb\u52a0\u7684\u76ee\u7684\u662f\u8003\u8651\u5230\u5ba4\u6e29\u5851\u6027\u4ee5\u53ca\u9ad8\u6e29\u8815\u53d8\u548c\u6297\u6c27\u5316\u6027\u80fd\u7684\u5e73\u8861\u3002\u603b\u4f53\u6765\u8bf4\uff0c\u7b2c\u4e8c\u4ee3TiAl\u5408\u91d1\u6709\u826f\u597d\u7684\u52a0\u5de5\u6027\u80fd\uff0c\u4e2d\u5ea6\u7684\u62c9\u4f38\u6027\u80fd\uff0c\u5176\u5ba4\u6e29\u5851\u6027\u5927\u7ea6\u57281-3%\u5de6\u53f3\uff0c\u65ad\u88c2\u97e7\u6027\u4ecb\u4e8e10-25MPa\uff0c\u5f53\u7136\u8fd9\u4e3b\u8981\u53d6\u51b3\u4e8e\u5176\u7ec4\u7ec7\u4e0e\u5316\u5b66\u5143\u7d20\u6210\u5206\u3002\u5178\u578b\u7684\u7b2c\u4e8c\u4ee3\u949b\u94dd\u5408\u91d1\u6709\u4e09\u79cd\uff0c\u5176\u4e2d4822 \u5ba4\u6e29\u5851\u6027\u6700\u9ad8\uff1b45XD\u53ef\u94f8\u6027\u597d, \u94f8\u6001\u7ec4\u7ec7\u6700\u4f73, \u9ad8\u6e29\u5f3a\u5ea6\u548c\u75b2\u52b3\u6027\u80fd\u597d\uff1b47WSi\u5408\u91d1\u7684\u9ad8\u6e29(760 \u2103)\u8815\u53d8\u6027\u80fd\u4f18\u5f02\u3002<\/p>\n<h3>3.\u7b2c\u4e09\u4ee3TiAl\u5408\u91d1\uff08\u8bbe\u8ba1\u8981\u6c42\uff0c\u6210\u5206\uff0c\u6027\u80fd\uff09<\/h3>\n<p>\u7b2c\u4e09\u4ee3TiAl\u5408\u91d1\u4e3b\u8981\u8003\u8651\u9ad8\u6e29\u70ed\u52a0\u5de5\u6027\u80fd\uff0c\u4ee5\u964d\u4f4e\u5176\u5e94\u7528\u6210\u672c\u53ca\u6790\u51fa\u5f3a\u5316\uff0c\u5176\u6210\u5206\u53ef\u4ee5\u603b\u7ed3\u5982\u4e0b\uff1a<\/p>\n<p>Ti-\uff0842-48\uff09Al-\uff080-10\uff09X-\uff080-3\uff09 Y-\uff08 0-1\uff09Z-\uff080-0.5RE\uff09\uff0c<\/p>\n<p>\u5176\u4e2dX=Cr, Mn\uff0cNb, Ta\uff1bY=Mo, W, Hf, Zr\uff1bZ=C,B,Si\uff1bRE\u4ee3\u8868\u7a00\u571f\u5143\u7d20\u3002<\/p>\n<p>\u4e0e\u7b2c\u4e8c\u4ee3\u5408\u91d1\u4e0d\u540c\u7684\u662f\uff0c\u7b2c\u4e09\u4ee3\u5408\u91d1\u7279\u522b\u6ce8\u91cd\u4e8e\u6dfb\u52a0\u8f83\u9ad8\u7684Nb\u4ee5\u53caMo\u5143\u7d20\uff0c\u5178\u578b\u7684\u4ee3\u8868\u4e3aTNM\u5408\u91d1\u3002\u5728\u9ad8\u6e29\u4e0b\uff08\u901a\u5e38\u5728\u03b1+\u03b3\u76f8\u533a\uff09\u4e0b\uff0c\u8be5\u7c7b\u5408\u91d1\u5177\u6709\u5f88\u597d\u7684\u52a0\u5de5\u6027\u80fd\uff0c\u53ef\u4ee5\u4f7f\u7528\u4f20\u7edf\u5de5\u827a\u8fdb\u884c\u953b\u9020\u3002\u953b\u9020\u540e\u901a\u8fc7\u70ed\u5904\u7406\u53ef\u4ee5\u8c03\u63a7\u6709\u5e8f\u03b2\u76f8\u7684\u542b\u91cf\uff0c\u4ece\u800c\u8c03\u6574\u5176\u529b\u5b66\u6027\u80fd\u3002\u4e0e\u7b2c\u4e8c\u4ee3\u5408\u91d1\u76f8\u6bd4\uff0c\u7b2c\u4e09\u4ee3\u5408\u91d1\u7684\u5f3a\u5ea6\u660e\u663e\u63d0\u9ad8\uff0c\u9ad8\u6e29\u6297\u6c27\u5316\u6027\u80fd\u9010\u6e10\u63d0\u9ad8\uff0c\u5176\u5ba4\u6e29\u6027\u80fd\u53ef\u4ee5\u8fbe\u5230800~1100\u00a0Mpa\uff0c\u800c\u62c9\u4f38\u5851\u6027\u5219\u5927\u4e8e2%\u3002\u5176\u4e3b\u8981\u539f\u56e0\u662f\u9ad8Nb\u4ee5\u53caMo\u5143\u7d20\u6291\u5236\u4e86\u6269\u6563\u8fc7\u7a0b\uff0c\u4ece\u800c\u964d\u4f4e\u4e86\u4f4d\u9519\u7684\u6500\u79fb\u3002\u4e0b\u9762\u4ee5TNM\u5408\u91d1\u7684\u8bbe\u8ba1\u7406\u5ff5\u4e3a\u4f8b\uff0c\u5177\u4f53\u8bf4\u660e\u7b2c\u4e09\u4ee3TiAl\u5408\u91d1\u7684\u4f18\u8d8a\u6027\u3002<\/p>\n<p>\u7b2c\u4e00\u4ee3\u548c\u7b2c\u4e8c\u4ee3\u949b\u94dd\u5408\u91d1\u7684\u953b\u9020\u65b9\u5f0f\u4e3b\u8981\u662f\u7b49\u6e29\u953b\u9020\uff0c\u7b49\u6e29\u953b\u9020\u7684\u6210\u672c\u9ad8\u6602\uff0c\u4e25\u91cd\u9650\u5236\u7684TiAl\u5408\u91d1\u7684\u5927\u89c4\u6a21\u5e94\u7528\u3002\u5728TiAl\u5408\u91d1\u4e2d\u52a0\u5165\u5927\u91cf\u7684\u03b2\u7a33\u5b9a\u5143\u7d20\uff0c\u53ef\u4ee5\u5728\u5408\u91d1\u5185\u90e8\u5f15\u5165\u5927\u91cf\u7684\u03b2\u76f8\uff0c\u03b2\u76f8\u5177\u6709\u7acb\u65b9\u7ed3\u6784\uff0c\u6ed1\u79fb\u7cfb\u8f83\u591a\uff0c\u5177\u6709\u826f\u597d\u7684\u5851\u6027\u53d8\u5f62\u80fd\u529b\uff0c\u4ece\u800c\u53ef\u4ee5\u5b9e\u73b0\u949b\u94dd\u5408\u91d1\u7684\u81ea\u7531\u953b\uff0c\u6240\u4ee5TNM\u5408\u91d1\u4e2d\u5177\u6709\u8f83\u9ad8\u7684Nb\u548cMo\u5143\u7d20\u3002\u8003\u8651\u5230\u8981\u5b9e\u73b0\u4f20\u7edf\u81ea\u7531\u953b\u9020\uff0c\u5408\u91d1\u7684\u94f8\u6001\u7ec4\u7ec7\u5c3d\u91cf\u7ec6\u5c0f\u4e14\u5747\u5300\u3002\u6709\u9274\u4e8e\u6b64\uff0cTNM\u5408\u91d1\u5728\u8bbe\u8ba1\u65f6\u5e94\u8be5\u6ee1\u8db3\u4ee5\u4e0b\u7684\u6761\u4ef6\uff1a<\/p>\n<p>1\uff09\u5728\u5408\u91d1\u94f8\u9020\u51dd\u56fa\u4e4b\u540e\u5177\u6709\u7ec6\u5c0f\u7684\u7b49\u8f74\u7ec4\u7ec7\u4e14\u65e0\u660e\u663e\u7684\u7ec7\u6784\u51fa\u73b0\uff1b<\/p>\n<p>2\uff09\u5c3d\u91cf\u4fdd\u8bc1\u5408\u91d1\u5728\u51dd\u56fa\u8fc7\u7a0b\u4e2d\u6309\u7167L\u2192L+\u03b2\u2192\u03b2\u2026\u800c\u975e\u5305\u6676\u53cd\u5e94L\u2192L+\u03b2\u2192\u03b1\u2192\u2026\uff0c\u539f\u56e0\u662f\u5305\u6676\u53cd\u5e94\u4f1a\u5bfc\u81f4\u5143\u7d20\u7684\u504f\u6790\u3002\u03b2\u2192\u03b1\u8f6c\u53d8\u4f1a\u5f62\u621012\u79cd\u53d8\u4f53\uff0c\u53ef\u4ee5\u5f88\u597d\u5730\u7ec6\u5316\u6676\u7c92\uff1b<\/p>\n<p>3\uff09\u540e\u7eed\u953b\u9020\u65f6\uff0c\u7531\u4e8e\u5408\u91d1\u542b\u6709\u5927\u91cf\u7684\u03b2\u76f8\uff0c\u4e3a\u5851\u6027\u53d8\u5f62\u63d0\u4f9b\u4e86\u6ed1\u79fb\u7cfb\uff0c\u56e0\u6b64\u63d0\u9ad8\u4e86\u5408\u91d1\u9ad8\u6e29\u53d8\u6027\u80fd\u529b\uff0c\u4ece\u800c\u53ef\u4ee5\u5b9e\u73b0\u6324\u538b\u3001\u953b\u9020\u4ee5\u53ca\u8f67\u5236\u3002\u53e6\u5916\u5927\u91cf\u03b2\u76f8\u7684\u5b58\u5728\u53ef\u4ee5\u6709\u6548\u6291\u5236\u5408\u91d1\u5728\u591a\u6b65\u6210\u5f62\u548c\u70ed\u5904\u7406\u8fc7\u7a0b\u4e2d\u6676\u7c92\u7684\u8fc7\u5ea6\u751f\u957f\u3002\u4f46\u662f\u03b2\u76f8\u51b7\u5374\u8fc7\u7a0b\u4e2d\u8f6c\u53d8\u5f97\u5230\u7684\u6709\u5e8f\u03b2<sub>0<\/sub>\u76f8\u5e94\u8be5\u5c3d\u91cf\u6d88\u9664\uff0c\u56e0\u4e3a\u4ed6\u4eec\u4f1a\u5bfc\u81f4\u6750\u6599\u7684\u8106\u6027\u65ad\u88c2\uff1b<\/p>\n<p>4\uff09\u4e3a\u4e86\u907f\u514d\u901a\u8fc7\u70ed\u5904\u7406\u8c03\u63a7\u953b\u4ef6\u548c\u94f8\u4ef6\u5185\u90e8\u6676\u7c92\u7684\u8fc7\u5ea6\u751f\u957f\uff0c\u5e94\u8be5\u5c3d\u529b\u907f\u514d\u9ad8\u6e29\u4e0b\u5355\u76f8\u03b1\u533a\u7684\u5b58\u5728\uff0c\u6216\u8005\u4fdd\u6301\u03b1\u5355\u76f8\u533a\u5c3d\u91cf\u72ed\u5c0f\u3002\u6240\u4ee5\u5408\u91d1\u4e2d\u52a0\u5165\u6269\u6563\u80fd\u529b\u5c0f\u7684Nb\u548cMo\u7b49\u5143\u7d20\uff0c\u4fbf\u53ef\u4ee5\u6709\u6548\u6291\u5236\u5355\u76f8\u03b1\u7684\u8fc7\u5ea6\u751f\u957f\uff1b<\/p>\n<p>5\uff09\u5408\u91d1\u4e2d\u5e94\u8be5\u5b58\u5728\u5339\u914d\u5f88\u597d\u7684\u03b3\u548c\u03b1<sub>2<\/sub>\u76f8\uff0c\u76f8\u542b\u91cf\u53ef\u4ee5\u901a\u8fc7\u540e\u5904\u7406\u6765\u8fdb\u884c\u8c03\u63a7\uff1b<\/p>\n<p>6\uff09\u5728\u4e2d\u6e29\u4fdd\u6e29\u65f6\uff0c\u901a\u8fc7\u03b2\u76f8\u6790\u51fa\u7684\u03c9\u76f8\u5e94\u8be5\u88ab\u6291\u5236\uff0c\u7531\u4e8e\u5176\u53ef\u4ee5\u5bfc\u81f4\u6750\u6599\u8106\u6027\u65ad\u88c2\uff1b<\/p>\n<p>\u57fa\u4e8e\u4ee5\u4e0a\u7684\u8bbe\u8ba1\u7406\u5ff5\uff0c\u52a0\u4e0a\u7b2c\u4e00\u6027\u539f\u7406\u7684\u8ba1\u7b97\uff0cTNM\u5408\u91d1\u88ab\u6210\u529f\u8bbe\u8ba1\u51fa\uff0c\u5176\u82b1\u6751\u6210\u5206\u4e3aTi-43Al-4Nb-1Mo\u3002\u540e\u6765\u5728\u8be5\u5408\u91d1\u7684\u57fa\u7840\u4e0a\u52a0\u4e860.1B\u5143\u7d20\uff0c\u4ece\u800c\u5f62\u6210\u65b0\u4e00\u4ee3TNM<sup>+<\/sup>\u5408\u91d1\u3002\u4e3b\u8981\u8003\u8651\u7684\u662fB\u5143\u7d20\u5177\u6709\u826f\u597d\u7684\u7ec6\u5316\u6676\u7c92\u7684\u4f5c\u7528\u3002\u7b2c\u4e09\u4ee3\u5408\u91d1\u7684AL\u5143\u7d20\u542b\u91cf\u7565\u5fae\u51cf\u5c0f\uff08\u4f46\u5bf9\u76f8\u53d8\u5f71\u54cd\u5f88\u5927\uff09\uff0c\u03b2\u6e29\u5ea6\u5143\u7d20\u6781\u5927\u63d0\u9ad8\u3002\u76f8\u8f83\u7b2c\u4e8c\u4ee3\u5408\u91d1\uff0c\u5f3a\u5ea6\u6781\u5927\u63d0\u9ad8\uff0c\u4f46\u5851\u6027\u7565\u6709\u964d\u4f4e\u3002<\/p>\n<h3>4.\u03b2\u2014TiAl\u5408\u91d1\uff08\u8bbe\u8ba1\u8981\u6c42\uff0c\u6210\u5206\uff0c\u6027\u80fd\uff09<\/h3>\n<p>\u03b2\u2014TiAl\u5408\u91d1\u4e25\u683c\u610f\u4e49\u6765\u8bf4\u4f9d\u7136\u5c5e\u4e8e\u7b2c\u4e09\u4ee3\u5408\u91d1\uff0c\u5176\u5960\u57fa\u6027\u7684\u57fa\u7840\u5de5\u4f5c\u5219\u7531\u6211\u56fd\u5317\u4eac\u79d1\u6280\u5927\u5b66\u9648\u56fd\u826f\u9662\u58eb\u6240\u505a\u3002\u4ed6\u4eec\u7ec4\u6210\u529f\u5f00\u53d1\u51fa\u4e86\u9ad8Nb\u949b\u94dd\u5408\u91d1\u3002\u5728\u7b2c\u4e00\u5c4a\u56fd\u9645TiAl\u5408\u91d1\u5927\u4f1a\u4e0a\uff0cTiAl\u5408\u91d1\u9886\u57df\u7684\u4e16\u754c\u6743\u5a01Y.W. Kim\u535a\u58eb\u6307\u51fa\uff0c\u7531\u5317\u4eac\u79d1\u6280\u5927\u5b66\u5e75\u53d1\u7684\u9ad8Nb\u2014TiAl\u5408\u91d1\u662f\u9ad8\u6e29\u9ad8\u6027\u80fd\u5408\u91d1\u7684\u201c\u9996\u521b\u201d\u3002\u9ad8Nb\u2014TiA\u5408\u91d1\u5df2\u7ecf\u6210\u4e3a\u65b0\u4e00\u4ee3\u9ad8\u6e29\u5408\u91d1\u7684\u53d1\u5c55\u65b9\u5411\u3002\u9ad8Nb\u5408\u91d1\u4e0e\u666e\u901a\u5408\u91d1\u76f8\u6bd4\uff0c\u5176\u4f7f\u7528\u6e29\u5ea6\u63d0\u9ad860-100\u2103\uff0c\u5ba4\u6e29\u5f3a\u5ea6\u63d0\u9ad8\u7ea6300-500MPa\u3002\u5176\u5f3a\u5ea6\u6027\u80fd\u4e0e\u6da1\u8f6e\u76d8\u7528\u666e\u901a\u53d8\u5f62\u954d\u57fa\u9ad8\u6e29\u5408\u91d1\u76f8\u8fd1\uff0c\u800c\u6bd4\u91cd\u7ea6\u4e3a\u5176\u4e00\u534a\u3002\u5176\u6297\u6c27\u5316\u6027\u80fd\u8fdc\u4f18\u4e8e\u666e\u901aTiAl\u5408\u91d1\uff0c\u800c\u6297\u6c27\u5316\u6027\u4e0e\u954d\u57fa\u9ad8\u6e29\u5408\u91d1\u76f8\u8fd1\u3002\u56fd\u9645\u4e0a\u76ee\u524d\u53d1\u5c55\u7684\u591a\u79cd\u5408\u91d1\u4e2d\uff0c\u90fd\u662f\u4ee5\u9ad8\u7684\u6dfb\u52a0\u4f5c\u4e3a\u5408\u91d1\u5316\u57fa\u7840\u7684\uff0c\u4f8b\u5982TNB\u5408\u91d1\uff08Ti-45Al-8Nb-0.2C\uff09\u3001TNM\u5408\u91d1\u4ee5\u53caY.W. Kim\u535a\u58eb\u6700\u8fd1\u5021\u5bfc\u7814\u53d1\u7684\u03b2\u2014TiAl\u5408\u91d1\u7b49\u3002\u6211\u56fd\u53d1\u5c55\u7684\u9ad8Nb\u2014TiAl\u5408\u91d1\u7684\u6210\u5206\u4ee5Ti-45Al-8.5Nb\u4e3a\u57fa\u7840\u3002\u8fd9\u4e9b\u5408\u91d1\u7684\u7279\u5f81\u5747\u4ee5\u9ad8\uff2eb\u4f4e\uff21l\u4e3a\u4e3b\uff0c\u7136\u540e\u518d\u5728\u9ad8\uff2e\uff42\u5408\u91d1\u5316\u7684\u57fa\u7840\u4e0a\uff0c\u901a\u8fc7\u5176\u5b83\u95f4\u9699\u5143\u7d20\u3001\u8fc7\u6e21\u5143\u7d20\u548c\u7a00\u571f\u5143\u7d20\u8fdb\u884c\u5fae\u5408\u91d1\u5316\uff0c\u4ece\u800c\u5b9e\u73b0\u7efc\u5408\u6027\u80fd\u7684\u63d0\u9ad8\u3002\u5982\uff37\u3001\uff2do\u3001\uff34a\u7b49\u8fc7\u6e21\u5143\u7d20\u53ef\u901a\u8fc7\u56fa\u6eb6\u5f3a\u5316\u6765\u63d0\u9ad8\uff34i\uff21l\u5408\u91d1\u7684\u9ad8\u6e29\u5f3a\u5ea6\uff1b\u800c\uff23\u3001\uff33i\u3001\uff2e\u7b49\u53ef\u4ea7\u751f\u6c89\u6dc0\u6790\u51fa\uff0c\u963b\u788d\u4f4d\u9519\u8fd0\u52a8\u548c\u6676\u754c\u8fc1\u79fb\uff0c\u5f62\u6210\u7b2c\u4e8c\u76f8\u5f3a\u5316\uff0c\u6709\u5229\u4e8e\u8815\u53d8\u6027\u80fd\u7684\u63d0\u9ad8\uff1b\uff22\u5219\u53ef\u4ee5\u7ec6\u5316\u6676\u7c92\u3001\u51cf\u5c11\u51dd\u56fa\u504f\u6790\uff0c\u63d0\u9ad8\u5f3a\u5ea6\u53ca\u70ed\u52a0\u5de5\u6027\uff1b\u800c\uff39\u7684\u6dfb\u52a0\u5219\u53ef\u4ee5\u5f62\u6210\u7a33\u5b9a\u7684\u6c27\u5316\u5c42\u3002\u9ad8\u94cc\u5408\u91d1\u7684\u7279\u70b9\u662f\u9ad8\u6e29\u8815\u53d8\u548c\u6297\u6c27\u5316\u6027\u80fd\u597d\uff0c\u7f3a\u70b9\u662f\u5ba4\u6e29\u5851\u6027\u4f4e, \u96be\u4ee5\u94f8\u9020\u3002\u91c7\u7528\u53d8\u5f62\u5de5\u827a\u53ef\u5728\u4e00\u5b9a\u7a0b\u5ea6\u4e0a\u63d0\u9ad8\u5ba4\u6e29\u5851\u6027\uff0c\u4f46Al \u504f\u6790\u95ee\u9898\u4ecd\u6709\u5f85\u89e3\u51b3\u3002<\/p>\n<p>\u9ad8\uff2eb\u5408\u91d1\u5316\u5bf9TiAl\u5408\u91d1\u76f8\u56fe\u7684\u4e3b\u8981\u5f71\u54cd\u5982\u4e0b(\u89c1figure 2)\uff1a<\/p>\n<p>\uff08\uff11\uff09\u7194\u70b9\u63d0\u9ad8\u4e86\u7ea61000\u2103\uff1b<\/p>\n<p>\uff08\uff12\uff09\u03b2\/\u03b2<sub>0<\/sub>\u76f8\u533a\u5411\u9ad8\uff21\uff11\u65b9\u5411\u6269\u5927\uff0c\u03b2\/\u03b2<sub>0<\/sub>\u8f6c\u53d8\u6e29\u5ea6\u964d\u4f4e\u4e8650-80\u2103\uff1b<\/p>\n<p>\uff08\uff13\uff09\u03b1\u76f8\u754c\u7ebf\u964d\u4f4e\u7ea630\u2103\uff23\uff0c\u03b1\/\u03b1+\u03b2\u76f8\u754c\u7ebf\u964d\u4f4e\u7ea650-100\u2103\u3002\u03b1\u76f8\u533a\u53d8\u7a84\uff0c\u6574\u4f53\u5411\u9ad8\uff21l\u533a\u79fb\u52a8\uff1b<\/p>\n<p>\uff08\uff14\uff09\u03b3\u76f8\u533a\u5411\u4f4e\uff21l\u533a\u79fb\u52a8\uff0c\u6709\u5229\u4e8e\u5ba4\u6e29\u5851\u6027\u7684\u6539\u5584\uff1b<\/p>\n<p>\uff08\uff15\uff09\u03b1\/\u03b1<sub>2<\/sub>+\u03b3\u5171\u6790\u6e29\u5ea6\u751f\u9ad9\uff1b<\/p>\n<p>\uff08\uff16\uff09\u5f53\uff2eb\u542b\u91cf\u8d85\u8fc79.5\uff05\u65f6\uff0c\u4f4e\u6e29\u03b1<sub>2<\/sub>\uff0b\u03b3\u4e24\u76f8\u533a\u53d8\u6210\u03b1<sub>2<\/sub>\uff0b\u03b3\uff0b\u03b2<sub>0<\/sub>\u4e09\u76f8\u533a\uff0c\u03b2<sub>0<\/sub>\u76f8\u4e0d\u5229\u4e8e\u5ba4\u6e29\u5851\u6027\uff0c\u6545\u800c\u9650\u5236\u4e86Nb\u542b\u91cf\u5408\u91d1\u5316\u7684\u4e0a\u9650\u3002<\/p>\n<p><strong>Figure 2 \u9ad8Nb\u542b\u91cf\u5bf9\u76f8\u56fe\u7684\u5f71\u54cd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-192200 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/12\/\u56fe\u72472-19.png\" alt=\"\" width=\"447\" height=\"435\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/12\/\u56fe\u72472-19.png 447w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2019\/12\/\u56fe\u72472-19-300x292.png 300w\" sizes=\"(max-width: 447px) 100vw, 447px\" \/><\/p>\n<h3>5.TiAl\u5408\u91d1\u7684\u6311\u6218\u4e0e\u524d\u666f<\/h3>\n<p>\u57282014 \u5e74\uff0c\u7f8e\u56fd\u53ec\u5f00\u4e86\u77ff\u51b6\u2219\u91d1\u5c5e\u2219\u6750\u6599\u5b66\u4f1a\u7b2c\u4e94\u5c4a\u03b3-TiAl \u56fd\u9645\u4f1a\u8bae\uff0c\u5728\u603b\u7ed3\u8ba8\u8bba\u7684\u65f6\u5019\uff0c\u63d0\u51fa\u4e86\u4ee5\u4e0b\u51e0\u65b9\u9762\u7684\u95ee\u9898\uff1a(1) \u5982\u4f55\u8fdb\u4e00\u6b65\u63d0\u9ad8\u5df2\u83b7\u5e94\u7528\u7684\u94f8\u9020\u5408\u91d1\u548c\u6280\u672f\u7684\u6210\u719f\u5ea6\uff0c\u63d0\u9ad8\u5408\u683c\u7387\uff0c\u964d\u4f4e\u6210\u672c\uff1f\u00a0(2)\u8fc7\u53bb\u51e0\u5341\u5e74\u5bf9\u53d8\u5f62\u5408\u91d1\u7814\u7a76\u5f97\u6700\u4e3a\u5145\u5206, \u4e3a\u4ec0\u4e48\u81f3\u4eca\u672a\u80fd\u83b7\u5f97\u89c4\u6a21\u5e94\u7528? \u80fd\u5426\u901a\u8fc7\u8fdb\u4e00\u6b65\u7814\u7a76\u626b\u9664\u969c\u788d, \u627e\u5230\u51fa\u8def\uff1f(3) \u80fd\u5426\u627e\u5230\u7efc\u5408\u6027\u80fd\u597d\u7684\u7b2c\u4e09\u4ee3\u5408\u91d1\uff1f\u9ad8\u6027\u80fd\u7684\u03b2\u51dd\u56fa\u5408\u91d1\u80fd\u5426\u5b8c\u5168\u5b9e\u73b0\u5e38\u89c4\u5de5\u827a\u953b\u9020, \u80fd\u5426\u5b9e\u73b0\u94f8\u9020\uff1f(4) \u5982\u4f55\u8bc4\u4f30\u5404\u79cd\u65b0\u7684\u5de5\u827a\uff1f\u5982\u4f55\u4fdd\u8bc1\u6210\u5206\u548c\u663e\u5fae\u7ec4\u7ec7\u7684\u5747\u5300\u6027\u548c\u4e00\u81f4\u6027\uff1f\u65b0\u5de5\u827a\u7684\u4f18\u52bf\u548c\u53ef\u5b9e\u73b0\u6027\u5230\u5e95\u5982\u4f55\uff1f(5) \u672a\u6765\u53ef\u4ee5\u62d3\u5c55\u54ea\u4e9b\u65b0\u7684\u5e94\u7528\uff0c\u9700\u8981\u89e3\u51b3\u54ea\u4e9b\u95ee\u9898\uff1f\u8fd9\u4e9b\u95ee\u9898\u5c06\u662f\u672a\u6765\u949b\u94dd\u5408\u91d1\u53d1\u5c55\u9700\u8981\u9762\u5bf9\u7684\u4e3b\u8981\u95ee\u9898\uff0c\u4e5f\u662f\u9700\u8981\u89e3\u51b3\u7684\u6280\u672f\u74f6\u9888\u3002\u5c31\u76ee\u524d\u7684\u60c5\u51b5\u6765\u770b\uff0c\u5728\u949b\u94dd\u5408\u91d1\u7684\u53d1\u5c55\u9053\u8def\u4e0a\uff0c\u4ee5\u4e0b\u95ee\u9898\u5728\u672a\u6765\u9700\u8981\u89e3\u51b3\u3002<\/p>\n<p>1\uff09\u94f8\u9020\u6280\u672f\u7684\u8fdb\u4e00\u6b65\u53d1\u5c55\u4e0e\u5b8c\u5584\uff1b\u7531\u4e8eTiAl\u5408\u91d1\u76f8\u56fe\u7684\u590d\u6742\u6027\uff0c\u51dd\u56fa\u663e\u5fae\u7ec4\u7ec7\u5bf9\u51dd\u56fa\u6761\u4ef6\u548c\u5408\u91d1\u6210\u5206\u975e\u5e38\u654f\u611f\u3002\u5e94\u8be5\u91c7\u7528\u6750\u6599\u57fa\u56e0\u7ec4\u8ba1\u5212\u6240\u5021\u5bfc\u7684\u96c6\u6210\u8ba1\u7b97\u65b9\u6cd5\uff0c\u5c06\u591a\u5c3a\u5ea6\u7684\u8ba1\u7b97\u6a21\u62df\u76f8\u7ed3\u5408\uff0c\u7ed9\u51fa\u6210\u5206-\u76f8-\u663e\u5fae\u7ec4\u7ec7\u5173\u7cfb\u7684\u6846\u67b6\uff0c\u5e76\u52a0\u4ee5\u5fc5\u8981\u7684\u5b9e\u9a8c\u9a8c\u8bc1\uff0c\u4ee5\u66f4\u597d\u5730\u7406\u89e3\u51dd\u56fa\u504f\u6790\uff0c\u6539\u5584\u663e\u5fae\u7ec4\u7ec7\u5747\u5300\u6027\u3002<\/p>\n<p>2\uff09\u96be\u53d8\u6027\u80fd\u529b\u7684\u6311\u6218\uff1b\u5bf9\u4e8eTiAl \u8fd9\u6837\u7684\u96be\u53d8\u5f62\u5408\u91d1\uff0c\u91c7\u7528\u53d8\u5f62\u5de5\u827a\u610f\u5473\u7740\u6750\u6599\u5229\u7528\u7387\u5f88\u4f4e\uff0c\u6210\u672c\u5f88\u9ad8\uff0c\u8fd9\u662f\u81f3\u4eca\u53d8\u5f62\u5408\u91d1\u672a\u5b9e\u73b0\u5927\u6279\u91cf\u5e94\u7528\u7684\u4e3b\u8981\u539f\u56e0\u4e4b\u4e00\u3002 \u672a\u6765\u9700\u8981\u7cfb\u7edf\u8868\u5f81\u663e\u5fae\u7ec4\u7ec7\u548c\u7ec7\u6784\u968f\u53d8\u5f62\u5de5\u5e8f\u7684\u6f14\u53d8\u8fc7\u7a0b\uff0c\u5728\u6b64\u57fa\u7840\u4e0a\u4ee5\u6700\u5c11\u5de5\u5e8f\u83b7\u5f97\u6700\u4f73\u7ec4\u7ec7\uff0c\u4ee5\u964d\u4f4e\u6210\u672c\u3002<\/p>\n<p>\u5728\u5e94\u7528\u524d\u666f\u65b9\u9762\uff0c\u8fd1\u5e74\u6765\uff0c3D \u6253\u5370\u6280\u672f\u5feb\u901f\u53d1\u5c55\uff0c\u800c\u949b\u94dd\u5408\u91d1\u4e5f\u6210\u4e3a\u7814\u7a76\u7684\u4e3b\u8981\u5bf9\u8c61\u4e4b\u4e00\u3002\u6b27\u7f8e\u5bf9\u03b3-TiAl \u5408\u91d1\u5f00\u5c55\u4e86\u8f83\u5927\u6295\u5165\u7684\u7814\u7a76\u3002\u4f8b\u5982\uff0c\u7f8e\u56fd\u5fb7\u514b\u8428\u65af\u5927\u5b66\u548c\u52a0\u5dde\u5927\u5b66\u3001\u610f\u5927\u5229\u90fd\u7075\u6280\u672f\u5927\u5b66\u548c\u610f\u5927\u5229\u822a\u7a7a\u5de5\u4e1a\u96c6\u56e2\u3001\u745e\u5178Arcam \u516c\u53f8\u7b49\u5355\u4f4d\uff0c\u91c7\u7528\u7535\u5b50\u675f\u7c89\u672b\u5e8a\u6280\u672f\u5bf9\u5236\u5907\u591a\u79cd\u03b3-TiAl \u5408\u91d1\u53ca\u53f6\u7247\u3001\u53f6\u8f6e\u6a21\u62df\u4ef6\u5f00\u5c55\u4e86\u6df1\u5165\u7814\u7a76\uff1b\u8bb8\u591a\u53d1\u8fbe\u56fd\u5bb6\uff0c\u5305\u62ec\u6211\u56fd\u90fd\u5bf9\u8fd9\u4e00\u6280\u672f\u5728\u949b\u94dd\u5408\u91d1\u7684\u6210\u5f62\u4e0e\u5e94\u7528\u4e2d\u8fdb\u884c\u4e86\u4e00\u7cfb\u5217\u7814\u7a76\uff0c\u8fd9\u4e9b3D \u6253\u5370\u6280\u672f\u7528\u03b3-TiAl \u5408\u91d1\u5236\u5907\u5fc5\u5c06\u63a8\u52a8\u65b0\u4e00\u4ee3\u5236\u9020\u65b9\u6cd5\u7684\u8fdb\u6b65\u3002\u5c3d\u7ba1\u8fdb\u5c55\u8f83\u5feb\uff0c\u76ee\u524d\u4ecd\u6709\u5f88\u591a\u6280\u672f\u95ee\u9898\u6ca1\u6709\u89e3\u51b3\uff0c\u5982\u540c\u4e00\u5de5\u4ef6\u4e0d\u540c\u90e8\u4f4d\u6027\u80fd\u7684\u4e00\u81f4\u6027\u3001\u4e0d\u540c\u6279\u6b21\u95f4\u6027\u80fd\u7684\u4e00\u81f4\u6027\u3001\u6c89\u79ef\u8d28\u91cf\u4e0e\u5236\u9020\u6548\u7387\u7684\u77db\u76fe\u3001\u4ee5\u53ca\u5f53\u7535\u5b50\u675f\u626b\u63cf\u901f\u7387\u8f83\u9ad8\u65f6\u9020\u6210\u7684\u5c42\u95f4\u504f\u6790\u7b49\u95ee\u9898\u8fd8\u6709\u5f85\u6df1\u5165\u7814\u7a76\u3002<\/p>\n<p>\u6b27\u6d32\u79d1\u5b66\u57fa\u91d1\u4f1a\u57282013 \u5e74\u5e95\u51fa\u7248\u7684\u6750\u6599\u79d1\u5b66\u4e0e\u5de5\u7a0b\u5c55\u671b\u62a5\u544a\u5217\u51fa\u4e869 \u4e2a\u9700\u8981\u91cd\u70b9\u5173\u6ce8\u7684\u7814\u7a76\u4e3b\u9898\uff0c\u03b3 -TiAl \u5408\u91d1\u548c\u589e\u6750\u5236\u9020\u6280\u672f\u5206\u5217\u7b2c\u4e00\u548c\u7b2c\u4e8c\u3002\u800c\u5c06\u589e\u6750\u5236\u9020\u6280\u672f\u7528\u4e8e\u5236\u5907\u4f4e\u5851\u6027\u03b3-TiAl \u5408\u91d1\u90e8\u4ef6\u663e\u7136\u6311\u6218\u6027\u66f4\u5927\u3002\u5404\u79cd3D \u6253\u5370\u6280\u672f\u4ecd\u5728\u52a0\u901f\u53d1\u5c55\u4e2d\uff0c\u6709\u5f85\u6210\u719f\u3002\u6240\u4ee5\uff0c3D\u6253\u5370\u6280\u672f\u5728\u672a\u6765\u7684\u5e94\u7528\u524d\u666f\u53ef\u89c2\uff0c\u4f46\u662f\u9700\u8981\u89e3\u51b3\u82e5\u5e72\u5145\u6ee1\u6311\u6218\u7684\u96be\u9898\u3002<\/p>\n<h3>6 \u7ed3\u8bed<\/h3>\n<p>\u822a\u7a7a\u53d1\u52a8\u673a\u88ab\u8a89\u4e3a\u201c\u5de5\u4e1a\u4e4b\u82b1\u201d\u548c\u98de\u673a\u7684\u201c\u5fc3\u810f\u201d\uff0c\u4e5f\u662f\u5de5\u4e1a\u754c\u201c\u7687\u51a0\u4e0a\u7684\u660e\u73e0\u201d\u3002\u56e0\u6b64\uff0c\u822a\u7a7a\u53d1\u52a8\u673a\u6750\u6599\u5f25\u8db3\u73cd\u8d35\u3002\u800cTiAl\u5408\u91d1\u4f5c\u4e3a\u4e00\u79cd\u91cd\u8981\u7684\u822a\u7a7a\u53d1\u52a8\u673a\u6750\u6599\uff0c\u5e94\u7528\u524d\u666f\u975e\u5e38\u5e7f\uff0c\u662f\u76ee\u524d\u66ff\u4ee3\u954d\u57fa\u9ad8\u6e29\u5408\u91d1\u7684\u7406\u60f3\u6750\u6599\u3002\u5f00\u53d1\u9ad8\u6027\u80fd\u7684TiAl\u5408\u91d1\u5bf9\u822a\u7a7a\u53d1\u52a8\u673a\u7684\u751f\u4ea7\u610f\u4e49\u975e\u51e1\u3002\u5728\u540c\u6837\u7684\u6761\u4ef6\u4e0b\uff0c\u4f7f\u7528TiAl\u5408\u91d1\u4f5c\u4e3a\u53f6\u7247\uff0c\u53ef\u4ee5\u51cf\u91cd50%\u5de6\u53f3\uff0c\u8fd9\u6837\u53ef\u4ee5\u5927\u5927\u51cf\u5c11\u98de\u673a\u7684\u80fd\u8017\uff0c\u8fd8\u53ef\u4ee5\u51cf\u5c11CO<sub>2<\/sub>\u7684\u6392\u653e\uff0c\u66f4\u53ef\u4ee5\u8ba9\u98de\u673a\u975e\u5f97\u66f4\u9ad8\u66f4\u8fdc\u3002<\/p>\n<p>\u672c\u6587\u7531<strong>\u865a\u8c37\u7eb3\u7269<\/strong>\u4f9b\u7a3f\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u968f\u7740\u822a\u7a7a\u5de5\u4e1a\u7684\u5feb\u901f\u53d1\u5c55\uff0c\u5bf9\u6750\u6599\u7684\u8981\u6c42\u4e5f\u8d8a\u6765\u8d8a\u9ad8\uff0c\u76ee\u524d\uff0c\u5176\u7ed3\u6784\u6750\u6599\u6b63\u5728\u671d\u7740\u201c\u66f4\u5f3a\u66f4\u8f7b\u201d\u7684\u65b9\u5411\u53d1\u5c55\uff0c\u66f4\u8f7b\u7684\u6750\u6599\u610f\u5473\u7740\u98de\u673a\u80fd\u591f\u975e\u5f97\u66f4\u9ad8\u4e14\u53ef\u4ee5\u6709\u6548\u51cf\u5c11CO2\u7684\u6392\u653e\u3002\u91d1\u5c5e&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":182269,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-192198","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/192198"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=192198"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/192198\/revisions"}],"predecessor-version":[{"id":192922,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/192198\/revisions\/192922"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/182269"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=192198"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=192198"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=192198"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}