{"id":195811,"date":"2020-02-20T06:46:56","date_gmt":"2020-02-19T22:46:56","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=195811"},"modified":"2020-02-19T16:26:49","modified_gmt":"2020-02-19T08:26:49","slug":"%e5%b7%b2%e6%a0%a1%e7%a8%bf%e4%bb%b6-%e8%8b%8f%e5%b7%9e%e5%a4%a7%e5%ad%a6-adv-funct-mater-%e9%80%9a%e8%bf%87%e7%95%8c%e9%9d%a2%e5%b0%91%e6%95%b0%e8%bd%bd%e6%b5%81%e5%ad%90%e8%b0%83%e5%88%b6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=195811","title":{"rendered":"\u82cf\u5dde\u5927\u5b66 Adv. Funct. Mater: \u901a\u8fc7\u754c\u9762\u5c11\u6570\u8f7d\u6d41\u5b50\u8c03\u5236\u7684\u4fc4\u6b47\u6548\u5e94\u8f85\u52a9\u9499\u949b\u77ff\u7535\u81f4\u53d1\u5149"},"content":{"rendered":"<p style=\"text-align: left;\"><strong>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011<\/strong><\/p>\n<p>\u4fc4\u6b47\u6548\u5e94\uff08Auger effect\uff09\u662f\u4f7f\u539f\u5b50\u3001\u5206\u5b50\u6210\u4e3a\u9ad8\u9636\u79bb\u5b50\u7684\u7269\u7406\u73b0\u8c61\uff0c\u4f34\u968f\u4e00\u4e2a\u7535\u5b50\u80fd\u91cf\u964d\u4f4e\u7684\u540c\u65f6\uff0c\u53e6\u4e00\u4e2a\uff08\u6216\u591a\u4e2a\uff09\u7535\u5b50\u80fd\u91cf\u5c06\u589e\u9ad8\u3002\u529f\u80fd\u5c42\u754c\u9762\u662f\u5f71\u54cd\u8bbe\u5907\u6027\u80fd\u548c\u529f\u80fd\u6027\u7684\u91cd\u8981\u56e0\u7d20\u3002\u5176\u4e2d\uff0c\u7531\u4e8e\u5f02\u8d28\u63a5\u89e6\u3001\u6ce8\u5165\u80fd\u91cf\u504f\u79fb\u548c\u4ecb\u7535\u635f\u8017\u5f15\u8d77\u7684\u5bc4\u751f\u754c\u9762\u6548\u5e94\u901a\u5e38\u662f\u4e0d\u5229\u7684\u3002\u7136\u800c\uff0c\u754c\u9762\u5904\u4e09\u8f7d\u6d41\u5b50\u76f8\u4e92\u4f5c\u7528\u7684\u4fc4\u6b47\u6548\u5e94\uff08IAE\uff09\u53ef\u4ee5\u663e\u8457\u8c03\u5236\u53d1\u5149\u4e8c\u6781\u7ba1\uff08LEDs\uff09\u7684\u5bfc\u901a\u548c\u9a71\u52a8\u7535\u538b\u4f7f\u5f97\u4f4e\u80fd\u91cf\u7684\u8f7d\u6d41\u5b50\u8db3\u4ee5\u514b\u670d\u6ce8\u5165\u52bf\u5792\uff0c\u4ece\u800c\u5b9e\u73b0\u4e9a\u5e26\u9699\u7535\u538b\u7535\u81f4\u53d1\u5149\uff08EL\uff09\u3002\u8fd9\u79cd\u7406\u60f3\u7684\u754c\u9762\u6548\u5e94\u53ef\u4ee5\u4f5c\u4e3a\u5185\u7f6e\u7684\u5347\u538b\u5668\u5e76\u964d\u4f4e\u5404\u529f\u80fd\u5c42\u4e2d\u7684\u538b\u964d\uff0c\u4f46\u662f\u5176\u96be\u4ee5\u6349\u6478\u7684\u673a\u7406\uff0c\u5728\u8be5\u9886\u57df\u4ecd\u7136\u7f3a\u4e4f\u6df1\u5165\u7684\u4e86\u89e3\u3002<\/p>\n<p>\u9499\u949b\u77ff\u6750\u6599\u5728\u7535\u81f4\u53d1\u5149\u9886\u57df\u5f97\u5230\u5e7f\u6cdb\u5173\u6ce8\uff0c\u4f46\u662f\u5b83\u4eec\u7684\u79bb\u5b50\u6027\u7279\u70b9\u4ee5\u53ca\u6613\u88ab\u7834\u574f\u7684\u6676\u683c\u7ed3\u6784\u5c24\u5176\u662f\u5728\u5927\u504f\u538b\u4e0b\u7684\u52a0\u901f\u964d\u89e3\u662f\u5bfc\u81f4\u5668\u4ef6\u8870\u9000\u7684\u4e3b\u8981\u539f\u56e0\u3002\u5c31\u8fd9\u70b9\u800c\u8a00\uff0c\u8fd1\u7ea2\u5916\u9499\u949b\u77ffLEDs\uff08PeLEDs\uff09\u7531\u4e8e\u5176\u8f83\u4f4e\u7684\u9a71\u52a8\u7535\u538b\u800c\u8868\u73b0\u51fa\u826f\u597d\u7684\u5de5\u4f5c\u7a33\u5b9a\u6027\uff0c\u800c\u9700\u8981\u5927\u9a71\u52a8\u7535\u538b\u7684\u7eff\u8272\u548c\u84dd\u8272\u7684\u9499\u949b\u77ffLEDs\u7684\u5de5\u4f5c\u5bff\u547d\u76f8\u6bd4\u4e4b\u4e0b\u77ed\u5f88\u591a\u3002<\/p>\n<p style=\"text-align: left;\"><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u57fa\u4e8e\u6b64\uff0c\u82cf\u5dde\u5927\u5b66\u529f\u80fd\u7eb3\u7c73\u4e0e\u8f6f\u7269\u8d28\u7814\u7a76\u9662\u7684\u5ed6\u826f\u751f\u6559\u6388\u548c\u738b\u7167\u594e\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u62a5\u9053\u4e86PeLEDs\u4e2dIAE\u7684\u673a\u5236\u3002\u57fa\u4e8e\u754c\u9762\u7ba1\u7406\u65b9\u6cd5\u548c\u754c\u9762\u7535\u6d41\u8c03\u5236\uff0c\u4f5c\u8005\u63ed\u9732\u4e86IAE\u5148\u51b3\u6761\u4ef6\u548c\u6b21\u8981\u6761\u4ef6\uff0c\u5176\u4e2d\u4e9a\u5e26\u9699\u7684\u4e8c\u6781\u7ba1\u9608\u503c\u7535\u538b\uff08V<sub>th<\/sub>\uff09\u548c\u5408\u9002\u7684\u754c\u9762\u6ce8\u5165\u6bd4\u5bf9\u4e8e\u5b9e\u73b0IAE\u8f85\u52a9EL\u5fc5\u4e0d\u53ef\u5c11\u3002\u7814\u7a76\u53d1\u73b0IAE\u8fc7\u7a0b\u53ef\u4ee5\u7531\u754c\u9762\u5c11\u6570\u8f7d\u6d41\u5b50\u63a7\u5236\uff0c\u5728\u4fc4\u6b47\u754c\u9762\u4e0a\u8fc7\u91cf\u6216\u532e\u4e4f\u7684\u5c11\u6570\u8f7d\u6d41\u5b50\u6ce8\u5165\u5c06\u5bfc\u81f4\u754c\u9762\u591a\u6570\u8f7d\u6d41\u5b50\u7684\u8017\u5c3d\u6216IAE\u7387\u4f4e\u3002\u56e0\u6b64\uff0c\u57fa\u4e8e\u4e0a\u8ff0\u4f18\u70b9\uff0c\u5229\u7528IAE\u8f85\u52a9\u7684\u7eff\u8272PeLEDs\uff08\u53d1\u5c04\u5cf0\u5728512 nm\uff09\u5448\u73b0\u51fa\u8d85\u4f4e\u7684\u5de5\u4f5c\u7535\u538b\uff0c\u4ece\u800c\u6291\u5236\u4e86\u6eda\u8f6c\u5e76\u6539\u5584\u4e86\u5de5\u4f5c\u7a33\u5b9a\u6027\uff0c\u534a\u8870\u671f\u4e3a11.5 h\uff081000 cd m<sup>-2<\/sup>\u7684\u521d\u59cb\u4eae\u5ea6\uff09\uff0c\u6bd4\u53d7\u63a7\u5668\u4ef6\u957f\u51e0\u500d\u3002\u8be5\u7814\u7a76\u6210\u679c\u4ee5\u9898\u4e3a<strong>\u201cAuger Effect Assisted Perovskite Electroluminescence Modulated by Interfacial Minority Carriers\u201d<\/strong>\u53d1\u5e03\u5728\u56fd\u9645\u8457\u540d\u671f\u520a<strong>Adv. Funct. Mater.<\/strong>\u4e0a\uff0c<strong>\u535a\u58eb\u751f\u82d1\u5e05\u3001\u5218\u5e86\u536b\u4e3a\u672c\u5de5\u4f5c\u5171\u540c\u7b2c\u4e00\u4f5c\u8005<\/strong>\u3002<\/p>\n<p style=\"text-align: left;\"><strong>\u3010\u56fe\u6587\u89e3\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00\u3001\u57fa\u4e8e\u4e0d\u7528\u7535\u5b50\u4f20\u8f93\u5c42PeLEDs\u7684\u57fa\u672c\u7ed3\u6784\u4e0e\u7535\u5b66\u7279\u6027<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-195812\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/1-17.jpg\" alt=\"\" width=\"600\" height=\"809\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/1-17.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/1-17-222x300.jpg 222w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-b\uff09U-Pe\/\u9499\u949b\u77ff\/ETLs\u7684\u5668\u4ef6\u7ed3\u6784\u56fe\u548c\u5e73\u5e26\u80fd\u7ea7\uff1b<\/p>\n<p>\uff08c-d\uff09U-Pe\u8584\u819c\u548cU-Pe\/\u9499\u949b\u77ff\u5806\u53e0\u8584\u819c\u7684AFM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08e-f\uff09\u5177\u6709\u4e0d\u540c\u7535\u5b50\u4f20\u8f93\u5c42\u7684\u9499\u949b\u77ffLED\u7684J-V\u548cL-V\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08g\uff09J-V\u66f2\u7ebf\u7684\u8be6\u7ec6\u7535\u4fe1\u606f\uff0c\u5305\u62ecV<sub>th<\/sub>\u3001\u6f0f\u7535\u548c\u4f4e\u6ce8\u5165\u533a\u57df\uff1b<\/p>\n<p>\uff08h\uff09\u4e0d\u540c\u5668\u4ef6\u7684\u7406\u60f3\u56e0\u5b50\u3002<\/p>\n<p><strong>\u56fe\u4e8c\u3001PeLEDs\u7684\u754c\u9762\u63a2\u6d4b<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-195813\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/2-15.jpg\" alt=\"\" width=\"600\" height=\"604\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/2-15.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/2-15-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/2-15-298x300.jpg 298w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u7535\u5b50\u548c\u7a7a\u7a74\u7535\u6d41\u8def\u5f84\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u6f0f\u7535\u4f4d\u7f6e\u7684\u68c0\u6d4b\u65b9\u6cd5\uff1b<\/p>\n<p>\uff08c\uff09Ir(mdq)<sub>2<\/sub>acac\uff08MDQ\uff09\u3001TPBi\u548c\u6c2f\u5316\u80c6\u78b1\u4fee\u9970\u7684\u5668\u4ef6\u7684\u534a\u5bf9\u6570J-V\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08d\uff09MDQ\u4fee\u9970\u5668\u4ef6\u7684EL\u5149\u8c31\uff1b<\/p>\n<p>\uff08e\uff09PVK\u4fee\u9970\u540e\u7684\u5668\u4ef6\u548c\u53c2\u8003\u7684J-V-E\u66f2\u7ebf\u3002<\/p>\n<p>\uff08f\uff09ZnMgO\/ZrO<sub>2<\/sub>\/\u9499\u949b\u77ff\/ETLs\u7684\u7eaf\u7535\u5b50\u5668\u4ef6\u7684J-V\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe\u4e09\u3001\u754c\u9762\u4fc4\u6b47\u6548\u5e94\u7684\u89e6\u53d1\u6761\u4ef6\u7814\u7a76<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-195814\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/3-15.jpg\" alt=\"\" width=\"600\" height=\"351\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/3-15.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/3-15-300x176.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u4ee5B4PYMPM\u4f5c\u4e3aETL\u7684\u7535\u5b50\u7535\u6d41\u8c03\u5236\u5668\u4ef6\u7684J-V\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08b\uff09\u5177\u6709\u4e0d\u540cETLs\u7684\u7535\u5b50\u7535\u6d41\u8c03\u5236\u5668\u4ef6\u7684J-V-L\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08c\uff09\u5168\u90e8\u8c03\u5236\u5668\u4ef6\u7684\u7535\u5b66\u53c2\u6570\u603b\u7ed3\uff0c\u5305\u62ec\u9608\u503c\u7535\u538b\u3001\u5f00\u542f\u7535\u538b\u4ee5\u53ca\u6709\u6e90\u5c42\u7684\u5149\u5b66\u5e26\u9699\uff1b<\/p>\n<p>\uff08d\uff09\u5bf9\u4e8eV<sub>th<\/sub>\u4f4e\u4e8eEAOB\/e\u7684\u5668\u4ef6\uff0c\u754c\u9762\u6ce8\u5165\u6bd4\u5b9a\u4e49\u4e3aI-MIN\/I-MAJ\u3002<\/p>\n<p>\n <strong>\u56fe\u56db\u3001IAE\u8f85\u52a9EL\u7684\u673a\u7406\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-195815\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/4-14.jpg\" alt=\"\" width=\"600\" height=\"418\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/4-14.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/4-14-300x209.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe\u4e94\u3001IAE\u673a\u7406\u5728\u5668\u4ef6\u4e2d\u7684\u8bc1\u660e<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-195816\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/5-9.jpg\" alt=\"\" width=\"600\" height=\"450\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/5-9.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/5-9-300x225.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-b\uff09\u5177\u6709MDQ\u754c\u9762\u63a2\u6d4b\u7684\u57fa\u4e8ePO-T2T\uff0850\u548c100 nm\uff09\u7684\u5668\u4ef6\u7684\u7535\u538b\u76f8\u5173EL\u5149\u8c31\uff1b<\/p>\n<p>\uff08c\uff09\u4e09\u79cd\u5178\u578b\u5668\u4ef6\u7684\u7535\u6d41\u6548\u7387\u589e\u76ca\u4e0e\u7535\u538b\u7684\u5173\u7cfb\uff1b<\/p>\n<p>\uff08d\uff09IAE\u5668\u4ef6\u7684\u6ce8\u5165\u6a21\u5f0f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u516d\u3001IAE\u5668\u4ef6\u548c\u666e\u901a\u5668\u4ef6\u7684\u6027\u80fd\u603b\u7ed3<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-195817\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/6-3.jpg\" alt=\"\" width=\"600\" height=\"448\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/6-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/6-3-300x224.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u7535\u6d41\u5bc6\u5ea6\u548c\u4eae\u5ea6\u4e0e\u7535\u538b\u7684\u5173\u7cfb\uff1b<\/p>\n<p>\uff08b\uff09\u4e0d\u540c\u504f\u538b\u4e0bIAE\u5668\u4ef6\u7684EL\u5149\u8c31\uff1b<\/p>\n<p>\uff08c\uff09\u5668\u4ef6EQE\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08d\uff09\u521d\u59cb\u4eae\u5ea6\u4e3a1000 cd m<sup>-2<\/sup>\u65f6\uff0c\u5668\u4ef6\u7684\u4f7f\u7528\u5bff\u547d\u5bf9\u6bd4\u3002<\/p>\n<p style=\"text-align: left;\"><strong>\u3010\u603b\u7ed3\u3011<\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u4f5c\u8005\u63a2\u8ba8\u4e86IAE\u7684\u673a\u7406\u5e76\u63d0\u51fa\u4e86IAE\u7684\u524d\u63d0\u548c\u6b21\u8981\u6761\u4ef6\u3002\u5bf9\u4e8e\u5e26\u9699\u4e3aV<sub>th<\/sub>\u7684\u5668\u4ef6\uff0cIAE\u8fc7\u7a0b\u7531\u754c\u9762\u5c11\u6570\u8f7d\u6ce2\u63a7\u5236\u3002\u5229\u7528IAE\u8f85\u52a9\u7684EL\uff0c\u9499\u949b\u77ffLEDs\u8868\u73b0\u51fa\u8d85\u4f4e\u7684\u5de5\u4f5c\u7535\u538b\uff0c\u57fa\u672c\u53ef\u5ffd\u7565\u7684\u6548\u7387\u6eda\u964d\u548c\u6539\u5584\u7684\u5de5\u4f5c\u7a33\u5b9a\u6027\uff0c\u8fd9\u4e3b\u8981\u662f\u7531\u4e8e\u5728\u529f\u80fd\u5c42\u4e2d\u663e\u8457\u964d\u4f4e\u7684\u7535\u573a\u5f3a\u5ea6\u3002\u603b\u4e4b\uff0c\u672c\u6587\u5f00\u53d1\u7684\u7b56\u7565\u4e3a\u589e\u5f3a\u9499\u949b\u77ffLEDs\u7684\u7a33\u5b9a\u6027\u63d0\u4f9b\u4e86\u4e00\u79cd\u53ef\u884c\u7684\u65b9\u6cd5\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adfm.201909222\" target=\"_blank\" rel=\"noopener\">Auger Effect Assisted Perovskite Electroluminescence Modulated by Interfacial Minority Carriers<\/a><\/strong>\uff08<em>Adv. Funct. Mater.<\/em>, <strong>2020<\/strong>, DOI: 10.1002\/adfm.201909222\uff09<\/p>\n<p>\u672c\u6587\u7531CQR\u7f16\u8bd1\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenvip.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011 \u4fc4\u6b47\u6548\u5e94\uff08Auger effect\uff09\u662f\u4f7f\u539f\u5b50\u3001\u5206\u5b50\u6210\u4e3a\u9ad8\u9636\u79bb\u5b50\u7684\u7269\u7406\u73b0\u8c61\uff0c\u4f34\u968f\u4e00\u4e2a\u7535\u5b50\u80fd\u91cf\u964d\u4f4e\u7684\u540c\u65f6\uff0c\u53e6\u4e00\u4e2a\uff08\u6216\u591a\u4e2a\uff09\u7535\u5b50\u80fd\u91cf\u5c06\u589e\u9ad8\u3002\u529f\u80fd\u5c42\u754c\u9762\u662f&#8230;<\/p>\n","protected":false},"author":7770,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[4309],"class_list":["post-195811","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-iae"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/195811"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7770"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=195811"}],"version-history":[{"count":5,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/195811\/revisions"}],"predecessor-version":[{"id":196394,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/195811\/revisions\/196394"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=195811"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=195811"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=195811"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}