{"id":196756,"date":"2020-04-07T06:15:14","date_gmt":"2020-04-06T22:15:14","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=196756"},"modified":"2020-04-06T21:15:25","modified_gmt":"2020-04-06T13:15:25","slug":"%e7%94%a8%e4%ba%8e%e9%ab%98%e7%ba%a7%e7%94%b5%e5%8c%96%e5%ad%a6%e5%82%a8%e8%83%bd%e7%9a%84%e7%a2%b3%e5%9f%ba%e7%ba%a4%e7%bb%b4%e8%ae%be%e5%a4%87%e4%ba%86%e8%a7%a3%e4%b8%80%e4%b8%8b%ef%bc%81","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=196756","title":{"rendered":"\u7528\u4e8e\u9ad8\u7ea7\u7535\u5316\u5b66\u50a8\u80fd\u7684\u78b3\u57fa\u7ea4\u7ef4\u8bbe\u5907\u4e86\u89e3\u4e00\u4e0b\uff01"},"content":{"rendered":"<p>\u5148\u8fdb\u7684\u7535\u5316\u5b66\u50a8\u80fd\u88c5\u7f6e(EESDs)\u53ef\u4ee5\u6709\u6548\u5730\u50a8\u5b58\u7535\u80fd\uff0c\u540c\u65f6\u53c8\u5177\u6709\u5fae\u578b\/\u67d4\u6027\/\u53ef\u7a7f\u6234\/\u627f\u91cd\u7684\u7279\u70b9\uff0c\u56e0\u6b64\uff0c\u4ece\u67d4\u6027\/\u53ef\u7a7f\u6234\/\u4fbf\u643a\u5f0f\u7535\u5b50\u4ea7\u54c1\u5230\u8f7b\u578b\u7535\u52a8\u6c7d\u8f66\/\u822a\u7a7a\u822a\u5929\u8bbe\u5907\uff0c\u5404\u79cd\u5e94\u7528\u90fd\u9700\u8981\u5b83\u3002\u7136\u800c\uff0c\u4f20\u7edf\u7684EESDs\u4f53\u79ef\u5e9e\u5927\u4e14\u521a\u6027\u597d\uff0c\u80fd\u91cf\/\u529f\u7387\u5bc6\u5ea6\u4f4e\uff0c\u4e0d\u9002\u5408\u627f\u8f7d\u3002\u56e0\u6b64\uff0c\u5f00\u53d1\u5148\u8fdb\u7684EESDs\u6210\u4e3a\u6ee1\u8db3\u8fd9\u4e9b\u65b0\u9700\u6c42\u7684\u8feb\u5207\u9700\u8981\uff0c\u5e76\u5728\u5f88\u5927\u7a0b\u5ea6\u4e0a\u4f9d\u8d56\u4e8e\u5148\u8fdb\u7684\u80fd\u6e90\u6750\u6599\u548c\u5668\u4ef6\u7ed3\u6784\u7684\u65b0\u8bbe\u8ba1\u3002\u78b3\u57fa\u7ea4\u7ef4(CFs)\u56e0\u5176\u8f7b\u8d28\u3001\u9ad8\u5bfc\u7535\u6027\u3001\u4f18\u5f02\u7684\u673a\u68b0\u5f3a\u5ea6\u3001\u67d4\u97e7\u6027\u548c\u53ef\u8c03\u7684\u7535\u5316\u5b66\u6027\u80fd\uff0c\u5728\u8fd9\u4e9b\u5148\u8fdb\u7684EESDs(\u5982\u8d85\u7ea7\u7535\u5bb9\u5668\u548c\u7535\u6c60)\u7684\u53d1\u5c55\u4e2d\u5177\u6709\u5de8\u5927\u7684\u6f5c\u529b\u3002\u5728\u6b64\u6211\u4eec\u4ecb\u7ecd\u4e00\u4e0b\u78b3\u57fa\u7ea4\u7ef4\u7684\u5236\u5907\u6280\u672f\uff0c\u4ee5\u53ca\u63d0\u9ad8\u5176\u673a\u68b0\u3001\u7535\u6c14\u548c\u7535\u5316\u5b66\u6027\u80fd\u7684\u5404\u79cd\u65b9\u6cd5\uff0c\u4ee5\u53ca\u6765\u81ea\u8fd9\u4e9b\u78b3\u57fa\u7ea4\u7ef4\u7684EESDs\u9ad8\u7ea7\u7684\u8bbe\u8ba1\u3001\u88c5\u914d\u548c\u6f5c\u5728\u7684\u5e94\u7528\u3002\u5206\u4eab\u78b3\u57fa\u7ea4\u7ef4\u5728\u9ad8\u7ea7\u7535\u6c89\u79ef\u4e2d\u7684\u5e94\u7528\u524d\u666f\u548c\u9762\u4e34\u7684\u6311\u6218\u3002<\/p>\n<p><strong><b>1<\/b><\/strong><strong><b>\u00a0EESDs<\/b><\/strong><strong><b>\u548cC<\/b><\/strong><strong><b>F<\/b><\/strong><strong><b>s\u4ecb\u7ecd<\/b><\/strong><\/p>\n<p>\u7535\u5316\u5b66\u50a8\u80fd\u88c5\u7f6e(EESDs)\u5305\u62ec\u8d85\u7ea7\u7535\u5bb9\u5668\u548c\u53ef\u5145\u7535\u7535\u6c60\uff0c\u7531\u6b63\u8d1f\u7535\u6781\u3001\u5206\u79bb\u5668\u548c\u6db2\u6001\u6216\u51dd\u80f6\u6001\u7684\u7535\u89e3\u8d28\u7ec4\u6210\u3002\u5de5\u4f5c\u7535\u6781\u901a\u5e38\u7531\u4e00\u5c42\u542b\u6709\u6d3b\u6027\u6750\u6599\u3001\u805a\u5408\u7269\u7c98\u5408\u5242\u548c\u5bfc\u7535\u5242\u7684\u91d1\u5c5e\u7b94\u6216\u6ce1\u6cab\u4f5c\u4e3a\u7535\u6d41\u6536\u96c6\u5668\u3002\u6709\u65f6\uff0c\u9ad8\u5bfc\u7535\u6027\u6d3b\u6027\u5c42\u53ef\u4ee5\u4f5c\u4e3a\u72ec\u7acb\u7535\u6781\uff1b\u78b3\u7eb3\u7c73\u7ba1\u548c\u77f3\u58a8\u70ef\u7b49\u6d3b\u6027\u6750\u6599\u4e5f\u53ef\u4ee5\u7ec4\u88c5\u6210\u72ec\u7acb\u7684\u5bfc\u7535\u8584\u819c\u3001\u6ce1\u6cab\u6216\u7ea4\u7ef4\u7535\u6781\uff0c\u56e0\u6b64\u7c98\u5408\u5242\u548c\u5bfc\u7535\u5242\u88ab\u6dd8\u6c70\u3002\u901a\u8fc7\u7535\u5316\u5b66\u8fc7\u7a0b\u4ee5\u53ef\u9006\u3001\u9ad8\u6548\u3001\u65b9\u4fbf\u7684\u65b9\u5f0f\u50a8\u5b58\u548c\u91ca\u653e\u7535\u80fd\uff0c\u5e7f\u6cdb\u5e94\u7528\u4e8e\u4fbf\u643a\u5f0f\u7535\u5b50\u3001\u7535\u52a8\u6c7d\u8f66\u548c\u822a\u7a7a\/\u822a\u5929\u8bbe\u5907\u7b49\u9886\u57df\u3002<\/p>\n<p>\u57fa\u4e8eCF\u7684\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u5178\u578b\u914d\u7f6e<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196758 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72471-35.png\" alt=\"\" width=\"700\" height=\"298\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72471-35.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72471-35-300x128.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe\u7247\u6765\u6e90\uff1aDOI:\u00a010.1021\/acs.chemrev.9b00466<\/p>\n<p>\u78b3\u57fa\u7ea4\u7ef4(CFs)\u88ab\u8ba4\u4e3a\u662f\u4ee5\u78b3\u4e3a\u4e3b\u8981\u6210\u5206\u7684\u957f(\u4e00\u822c\u4e3a&gt;1 mm)\u7ea4\u7ef4\u3002\u78b3\u7ea4\u7ef4\u7684\u76f4\u5f84\u901a\u5e38\u5728\u51e0\u5341\u7eb3\u7c73\u5230\u51e0\u5341\u5fae\u7c73\u4e4b\u95f4\uff0c\u8fd9\u4f7f\u5f97\u5b83\u4eec\u53ef\u4ee5\u88ab\u5212\u5206\u4e3a\u78b3\u7eb3\u7c73\u7ea4\u7ef4(CNFs,\u76f4\u5f84&lt; 1\u03bcm)\u548c\u78b3\u8d85\u7ec6\u7ea4\u7ef4(CMFs,\u76f4\u5f84&gt; 1\u03bcm)\u3002CFs\u8f83\u957f\uff0c\u673a\u68b0\u5f3a\u5ea6\u5f3a\uff0c\u67d4\u97e7\u6027\u597d\uff0c\u5e76\u5177\u6709\u826f\u597d\u7684\u5bfc\u7535\u6027\u548c\u7535\u5316\u5b66\u6027\u80fd\u3002\u8fd9\u4e9b\u7279\u6027\u610f\u5473\u7740CFs\u53ca\u5176\u7ec7\u7269\u53ef\u4ee5\u4f5c\u4e3a\u7406\u60f3\u7684\u65e0\u7c98\u7ed3\u5242\u3001\u81ea\u7acb\u3001\u575a\u56fa\u548c\u7075\u6d3b\u7684\u7535\u6781\uff0c\u5b83\u4eec\u53ef\u4ee5\u7ec4\u88c5\u6210\u7ebf\u72b6\u548c\u7eba\u7ec7\u7684EESDs\uff0c\u53ef\u4ee5\u4f5c\u4e3a\u5c0f\u578b\/\u67d4\u6027\/\u53ef\u7a7f\u6234\u7535\u5b50\u8bbe\u5907\u548c\u667a\u80fd\u670d\u88c5\u7684\u7279\u6b8a\u7535\u6e90\u3002\u8fd9\u4e9b\u5148\u8fdb\u7684EESDs\u6709\u5229\u4e8e\u5f00\u53d1\u4fbf\u643a\u5f0f\u7535\u5b50\u3001\u7535\u52a8\u6c7d\u8f66\u3001\u822a\u7a7a\u548c\u822a\u5929\u8bbe\u5907\uff0c\u5177\u6709\u663e\u8457\u7684\u51cf\u91cd\u548c\u5ef6\u957f\u7eed\u822a\u80fd\u529b\u3002\u56e0\u6b64\uff0cCFs\u662f\u4e00\u79cd\u5f88\u6709\u524d\u9014\u7684\u5148\u8fdbEESDs\u6750\u6599\u3002<\/p>\n<p>\u9ad8\u7ea7\u7535\u5316\u5b66\u50a8\u80fd\u7684\u78b3\u57fa\u7ea4\u7ef4\u53ca\u6f5c\u5728\u5e94\u7528<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196759 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72472-30.png\" alt=\"\" width=\"700\" height=\"590\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72472-30.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72472-30-300x253.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe\u7247\u6765\u6e90\uff1aDOI:\u00a010.1021\/acs.chemrev.9b00466<\/p>\n<p><strong><b>2<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>C<\/b><\/strong><strong><b>F<\/b><\/strong><strong><b>s<\/b><\/strong><strong><b>\u7684\u5236\u5907<\/b><\/strong><strong><b>\u53ca\u6027\u80fd\u6539\u5584<\/b><\/strong><\/p>\n<p>CFs\u53ef\u4ee5\u901a\u8fc7\u4e24\u79cd\u4e3b\u8981\u7684\u65b9\u6cd5\u4ea7\u751f\uff1a\u539f\u4e1d\u78b3\u5316\u548c\u7531\u78b3\u7eb3\u7c73\u6750\u6599\u7eba\u4e1d<\/p>\n<p>\u539f\u4e1d\u78b3\u5316\uff0c\u524d\u9a71\u7ea4\u7ef4\u4ece\u81ea\u7136\u8d44\u6e90\u4e2d\u83b7\u5f97\uff0c\u7531\u805a\u5408\u7269\u6216\u6ca5\u9752\u7eba\u6210\uff0c\u6216\u7531\u5c0f\u5206\u5b50\u5408\u6210\uff0c\u7136\u540e\u7ecf\u53d7\u9ad8\u6e29(&gt;500\u2103\uff0c\u901a\u5e38\u4e3a\u223c1000\u2103)\u78b3\u5316\u3002\u78b3\u7eb3\u7c73\u6750\u6599\u7eba\u4e1d\uff0c\u78b3\u7eb3\u7c73\u7ba1\u548c\u77f3\u58a8\u70ef(\u6c27\u5316\u7269)\u7b49\u7eb3\u7c73\u78b3\u5316\u7269\u662f\u901a\u8fc7\u5316\u5b66\u6c14\u76f8\u6c89\u79ef\u6cd5(CVD)\u6216\u5316\u5b66\u5265\u79bb\u5408\u6210\uff0c\u7136\u540e\u7531\u6c14\u6eb6\u80f6\u3001\u6e7f\u5206\u6563\u4f53\u6216\u56fa\u4f53\u9635\u5217\/\u819c\u7eba\u6210\u7ea4\u7ef4\u3002<\/p>\n<p>\u6c14\/\u6db2\/\u56fa\u76f8\u7ec4\u88c5\u7684\u5178\u578b\u65b9\u6cd5<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196760 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-29.png\" alt=\"\" width=\"700\" height=\"532\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-29.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-29-300x228.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196761 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-1-1.png\" alt=\"\" width=\"700\" height=\"612\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-1-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-1-1-300x262.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196762 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-2-1.png\" alt=\"\" width=\"700\" height=\"652\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-2-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72473-2-1-300x279.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe\u7247\u6765\u6e90\uff1aDOI:\u00a010.1021\/acs.chemrev.9b00466<\/p>\n<p>CFs\u7535\u5316\u5b66\u6027\u80fd\u7684\u6539\u5584<\/p>\n<p>CFs\u7684\u7535\u5316\u5b66\u6027\u80fd\u5728\u5f88\u5927\u7a0b\u5ea6\u4e0a\u662f\u7531\u5176\u7ed3\u6784\u51b3\u5b9a\u7684\uff0c\u5176\u673a\u7535\u6027\u80fd\u4e5f\u662f\u5982\u6b64\u3002<\/p>\n<p>\u7535\u5316\u5b66\u6027\u80fd\u6539\u5584\u65b9\u6cd5<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196763 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72474-28.png\" alt=\"\" width=\"625\" height=\"499\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72474-28.png 625w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72474-28-300x240.png 300w\" sizes=\"(max-width: 625px) 100vw, 625px\" \/><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196764 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72474-1-1.png\" alt=\"\" width=\"700\" height=\"648\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72474-1-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72474-1-1-300x278.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe\u7247\u6765\u6e90\uff1aDOI:\u00a010.1021\/acs.chemrev.9b00466<\/p>\n<p><strong><b>3<\/b><\/strong><strong><b>\u00a0CFs<\/b><\/strong><strong><b>\u57fa\u8d85\u7ea7\u7535\u5bb9\u5668<\/b><\/strong><\/p>\n<p>CFs\u7684\u7535\u5316\u5b66\u6027\u80fd\u5728\u5f88\u5927\u7a0b\u5ea6\u4e0a\u662f\u7531\u5176\u7ed3\u6784\u51b3\u5b9a\u7684\uff0c\u5176\u673a\u7535\u6027\u80fd\u4e5f\u662f\u5982\u6b64\u3002\u63d0\u9ad8CF\u7535\u6781\u7684\u6bd4\u7535\u5bb9\u662f\u9ad8\u6027\u80fd\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u5173\u952e\u95ee\u9898\u3002<\/p>\n<p><strong><b>\u63d0\u9ad8CF<\/b><\/strong><strong><b>\u57fa<\/b><\/strong><strong><b>\u8d85\u7ea7\u7535\u5bb9\u5668\u80fd\u91cf\u548c\u529f\u7387\u5bc6\u5ea6\u7684\u65b9\u6cd5<\/b><\/strong><\/p>\n<ul>\n<li><b><\/b>\u4f7f\u7528\u975e\u5bf9\u79f0\u914d<strong><b>\u7f6e<\/b><\/strong><\/li>\n<\/ul>\n<p>\u91c7\u7528\u975e\u5bf9\u79f0\u7ed3\u6784\u53ef\u4ee5\u6709\u6548\u5730\u63d0\u9ad8\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u5de5\u4f5c\u7535\u538b\u548c\u80fd\u91cf\u3001\u529f\u7387\u5bc6\u5ea6\uff0c\u5373\u5728\u6b63\u8d1f\u7535\u6781\u4e0a\u4f7f\u7528\u4e0d\u540c\u7684PWs\u6d3b\u6027\u6750\u6599\uff0c\u6216\u5728\u4e24\u4e2a\u7535\u6781\u4e0a\u4f7f\u7528\u76f8\u540c\u7684\u6d3b\u6027\u6750\u6599\uff0c\u4f46\u8d28\u91cf\u6bd4\u4e0d\u540c\u3002\u5e38\u7528\u7684\u6b63\u6781\u6d3b\u6027\u6750\u6599\u6709\u91d1\u5c5e\u6c27\u5316\u7269\/\u6c22\u6c27\u5316\u7269\/\u786b\u5316\u7269\u5c42\u72b6\u53cc\u6c22\u6c27\u5316\u7269\u3001\u5bfc\u7535\u805a\u5408\u7269\u3001\u78b3\u7eb3\u7c73\u6750\u6599\u3002\u8be5\u8d1f\u6781\u6d3b\u6027\u6750\u6599\u53ef\u4ee5\u662f\u78b3\u7eb3\u7c73\u6750\u6599\u91d1\u5c5e\u6c27\u5316\u7269\u3001\u6c2e\u5316\u7269\u3001\u78f7\u5316\u7269\u7b49\u6570\u767e\u79cd\u6b63\u6781\u548c\u8d1f\u6781\u6750\u6599\u7684\u7ec4\u5408\u53ef\u7528\u4e8e\u914d\u7f6e\u975e\u5bf9\u79f0\u8d85\u7ea7\u7535\u5bb9\u5668\u3002<\/p>\n<p>\u6bd4\u5982\uff1a<\/p>\n<p><strong><b>\u53ef\u62c9\u4f38\u7ebf\u5f62\u975e\u5bf9\u79f0\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u8bbe\u8ba1<\/b><\/strong><\/p>\n<p>\u4e1c\u534e\u5927\u5b66\u4fde\u5efa\u52c7\u6559\u6388\u3001\u674e\u53d1\u5b66\u526f\u6559\u6388\u4e0e\u7f8e\u56fd\u7279\u62c9\u534e\u5927\u5b66\u90b9\u7956\u709c\u6559\u6388\u5408\u4f5c\uff0c\u5728ACS Nano\u4e0a\u53d1\u8868\u9898\u4e3a\u201cStretchable Wire-Shaped Asymmetric Supercapacitors Based on Pristine and MnO<sub>2<\/sub>\u00a0Coated Carbon Nanotube Fibers\u201d\u7684\u8bba\u6587\uff0c\u5c06\u975e\u5bf9\u79f0\u7684\u7ed3\u6784\u5e94\u7528\u5728\u7ebf\u5f62\u8d85\u7ea7\u7535\u5bb9\u5668\u4e2d\uff0c\u4f7f\u8d85\u7ea7\u7535\u5bb9\u5668\u7535\u538b\u8303\u56f4\u4ece0.8 V\u6269\u5c55\u52301.5V\uff0c\u4e14\u88c5\u7f6e\u7684\u80fd\u91cf\u5bc6\u5ea6\u548c\u529f\u7387\u5bc6\u5ea6\u5206\u522b\u662f\u5bf9\u5e94\u975e\u5bf9\u79f0\u8d85\u7ea7\u7535\u5bb9\u5668\u4e09\u500d\u548c\u4e24\u500d\u3002\u975e\u5bf9\u79f0\u7ebf\u5f62\u8d85\u7ea7\u7535\u5bb9\u5668\u7531\u4f5c\u4e3a\u6b63\u6781\u7684MnO<sub>2<\/sub>\/CNT\u590d\u5408\u7ea4\u7ef4\uff0c\u4f5c\u4e3a\u8d1f\u6781\u7684\u6c14\u51dd\u80f6CNT\u7ea4\u7ef4\u4ee5\u53ca\u4f5c\u4e3a\u7535\u89e3\u8d28\u7684KOH-PVA\u51dd\u80f6\u7ec4\u6210\u3002\u5229\u7528Dow XLA\u5f39\u6027\u7ea4\u7ef4\u4f5c\u4e3a\u57fa\u4f53\u4ee5\u53ca\u201c\u5148\u9884\u62c9\u4f38-\u540e\u5c48\u66f2\u201d\u7684\u65b9\u6cd5\uff0c\u8d4b\u4e88\u4e86\u5176100%\u53ef\u62c9\u4f38\u6027\u3002\u8fd9\u4e2a\u975e\u5bf9\u79f0\u7684\u53ef\u62c9\u4f38\u8d85\u7ea7\u7535\u5bb9\u5668\u5177\u6709\u8f83\u9ad8\u7684\u6bd4\u7535\u5bb9157.53 \u00b5F cm-1\u00a0(\u626b\u63cf\u901f\u7387\u4e3a\u00a050 mV s<sup>-1<\/sup>\u65f6\uff09\uff0c\u8f83\u9ad8\u7684\u80fd\u91cf\u5bc6\u5ea6\uff0817.26\u201346.59 nWh cm<sup>-1<\/sup>\uff09\u548c\u529f\u7387\u5bc6\u5ea6\uff087.63\u201361.55 \u00b5W cm<sup>-1<\/sup>\uff09\u3002\u5f15\u4eba\u6ce8\u610f\u7684\u662f\uff0c\u9ad8\u8fbe100%\u7684\u5faa\u73af\u62c9\u4f38\u5e94\u53d8\u4ec5\u5b83\u7684\u7535\u5316\u5b66\u6027\u80fd\u9020\u6210\u4e86\u5fae\u5c0f\u5f71\u54cd\u3002\u53e6\u5916\uff0c\u7ecf\u8fc710000\u6b21\u7684\u6052\u7535\u6d41\u5145\u653e\u7535\u5faa\u73af\uff0c\u6bd4\u7535\u5bb9\u4ecd\u7136\u4fdd\u6301\u4e8699%\u4ee5\u4e0a\uff0c\u8868\u660e\u826f\u597d\u7684\u957f\u671f\u5faa\u73af\u7a33\u5b9a\u6027\u3002\u975e\u5bf9\u79f0\u7684\u7ed3\u6784\u88ab\u8bc1\u660e\u662f\u4e00\u79cd\u4f18\u5f02\u7684\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u7ed3\u6784\uff0c\u7528\u4ee5\u8fbe\u5230\u8f83\u9ad8\u7684\u5de5\u4f5c\u7535\u538b\u548c\u9ad8\u80fd\u91cf\u5bc6\u5ea6\uff0c\u800c\u4e0d\u727a\u7272\u529f\u7387\u53ca\u5faa\u73af\u7a33\u5b9a\u6027\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1021\/acsnano.5b01244\u00a0<\/p>\n<p><strong><b>\u67d4\u6027\u5168\u56fa\u6001\u975e\u5bf9\u79f0\u8d85\u7ea7\u7535\u5bb9\u5668<\/b><\/strong><strong><b>\u7684\u8bbe\u8ba1<\/b><\/strong><\/p>\n<p>\u8fd1\u5e74\u6765\uff0c\u7ea4\u7ef4\u578b\u67d4\u6027\u8d85\u7ea7\u7535\u5bb9\u5668\u56e0\u5176\u5728\u53ef\u7a7f\u6234\u7535\u5b50\u9886\u57df\u7684\u6f5c\u5728\u5e94\u7528\u800c\u53d7\u5230\u5e7f\u6cdb\u5173\u6ce8\u3002\u7136\u800c\uff0c\u6709\u9650\u7684\u80fd\u91cf\u5bc6\u5ea6\u4ecd\u7136\u662f\u5236\u7ea6\u5176\u5b9e\u9645\u5e94\u7528\u7684\u4e25\u91cd\u74f6\u9888\u3002\u4e1c\u534e\u5927\u5b66\u6731\u7f8e\u82b3\u6559\u6388\u56e2\u961f\u5728Carbon\u4e0a\u53d1\u8868\u9898\u4e3a\u201cFlexible all-solid-state asymmetric supercapacitor based on transition metal oxide nanorods\/reduced graphene oxide hybrid fibers with high energy density\u201d\u7684\u8bba\u6587\uff0c\u901a\u8fc7\u4e00\u79cd\u7b80\u4fbf\u3001\u53ef\u6269\u5c55\u7684\u6e7f\u7eba\u65b9\u6cd5\u5236\u5907\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269\u7eb3\u7c73\u68d2\/\u8fd8\u539f\u6c27\u5316\u77f3\u58a8\u70ef(rGO)\u6df7\u5408\u7ea4\u7ef4\u3002\u7531\u4e8e\u8fc7\u6e21\u91d1\u5c5e\u6c27\u5316\u7269\u7eb3\u7c73\u68d2\u4e0e\u8fd8\u539f\u6c27\u5316\u77f3\u58a8\u70ef\u7684\u534f\u540c\u4f5c\u7528\uff0c\u4f7f\u6742\u5316\u7ea4\u7ef4\u7684\u7535\u5316\u5b66\u6027\u80fd\u5f97\u5230\u4e86\u5f88\u5927\u7684\u6539\u5584\u3002\u4ee5MnO<sub>2<\/sub>\u7eb3\u7c73\u68d2\/rGO\u6742\u5316\u7ea4\u7ef4\u4e3a\u6b63\u6781\uff0cMoO<sub>3<\/sub>\u7eb3\u7c73\u68d2\/rGO\u6742\u5316\u7ea4\u7ef4\u4e3a\u8d1f\u6781\uff0cH<sub>3<\/sub>PO<sub>4<\/sub>\/\u805a\u4e59\u70ef\u9187(PVA)\u4e3a\u7535\u89e3\u6db2\uff0c\u6784\u5efa\u4e86\u5168\u56fa\u6001\u975e\u5bf9\u79f0\u8d85\u7ea7\u7535\u5bb9\u5668\u3002\u6839\u636eMnO<sub>2<\/sub>\u548cMoO<sub>3<\/sub>\u4e4b\u95f4\u4e0d\u540c\u7684\u5de5\u4f5c\u7535\u4f4d\u7a97\u53e3\uff0c\u4f18\u5316\u540e\u7684\u975e\u5bf9\u79f0\u8d85\u7ea7\u7535\u5bb9\u5668\u53ef\u4ee5\u57281.6 V\u7684\u9ad8\u538b\u4e0b\u8fdb\u884c\u53ef\u9006\u5faa\u73af\uff0c\u5e76\u572876.4 mW cm<sup>&#8211;<\/sup><sup>3<\/sup>\u7684\u529f\u7387\u5bc6\u5ea6\u4e0b\u63d0\u4f9b18.2 mWh cm<sup>&#8211;<\/sup><sup>3<\/sup>\u7684\u4f18\u8d8a\u4f53\u79ef\u80fd\u91cf\u5bc6\u5ea6\u3002\u6b64\u5916\uff0c\u975e\u5bf9\u79f0\u8d85\u7ea7\u7535\u5bb9\u5668\u8fd8\u5177\u6709\u663e\u8457\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u548c\u826f\u597d\u7684\u67d4\u6027\u548c\u673a\u68b0\u7a33\u5b9a\u6027\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1016\/j.carbon.2016.11.051\u00a0<\/p>\n<ul>\n<li><b><\/b><strong><b>\u4f7f\u7528<\/b><\/strong><strong><b>\u9ad8\u538b\u7535\u89e3\u8d28<\/b><\/strong><\/li>\n<\/ul>\n<p>\u7535\u89e3\u6db2\u662f\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u53e6\u4e00\u4e2a\u91cd\u8981\u7ec4\u6210\u90e8\u5206\uff0c\u5b83\u4e3b\u8981\u51b3\u5b9a\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u5de5\u4f5c\u7535\u538b\u3002\u8d85\u7ea7\u7535\u5bb9\u5668\u6700\u5e7f\u6cdb\u4f7f\u7528\u7684\u7535\u89e3\u8d28\u662f\u6c34\u6eb6\u6db2\uff0c\u7531\u4e8e\u5b83\u4eec\u7684\u9ad8\u79bb\u5b50\u7535\u5bfc\u7387\u3001\u4f4e\u79bb\u5b50\u534a\u5f84\u3001\u73af\u5883\u53cb\u597d\u6027\u548c\u4e0d\u53ef\u71c3\u6027\uff0c\u4f7f\u7528\u9ad8\u538b\u7535\u89e3\u6db2\u662f\u63d0\u9ad8CF\u578b\u8d85\u7ea7\u7535\u5bb9\u5668\u80fd\u91cf\u548c\u529f\u7387\u5bc6\u5ea6\u7684\u6709\u6548\u9014\u5f84\u3002<\/p>\n<p>\u6bd4\u5982\uff1a<\/p>\n<p><strong><b>\u4e09\u7ef4\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u79bb\u5b50\u6db2\u4f53\u8d85\u7ea7\u7535\u5bb9\u5668\u7535\u6781<\/b><\/strong><\/p>\n<p>\u5fb7\u96f7\u585e\u5c14\u5927\u5b66\u7684Vibha Kalra\u6559\u6388\u7b49\u4eba\u5728Chem.\u00a0Commun.\u4e0a\u53d1\u8868\u9898\u4e3a\u201cBinder-free three-dimensional high energy density electrodes for ionic-liquid supercapacitors\u201d\u7684\u8bba\u6587\uff0c\u6f14\u793a\u4e86\u4e00\u79cd\u7b80\u4fbf\u7684\u65b9\u6cd5\u6765\u5236\u4f5c\u65e0\u7c98\u7ed3\u5242\u591a\u5b54\u78b3\u7eb3\u7c73\u7ea4\u7ef4\u7535\u6781\u7528\u4e8e\u5ba4\u6e29\u79bb\u5b50\u6db2\u4f53\u8d85\u7ea7\u7535\u5bb9\u5668\u3002\u7814\u7a76\u4e86\u65e0\u7c98\u7ed3\u5242\u7535\u7eba\u78b3\u7eb3\u7c73\u7ea4\u7ef4\u5728\u5ba4\u6e29\u79bb\u5b50\u6db2\u4f53\u8d85\u7ea7\u7535\u5bb9\u5668\u4e2d\u7684\u7535\u5316\u5b66\u884c\u4e3a\u3002\u6837\u54c1\u7684\u6bd4\u7535\u5bb9\u9ad8\u8fbe180 F g<sup>&#8211;<\/sup><sup>1<\/sup>\uff0c\u80fd\u91cf\u5bc6\u5ea6\u4e3a80W h kg<sup>&#8211;<\/sup><sup>1<\/sup>\u3002\u540c\u65f6\u5728\u626b\u63cf\u901f\u7387\u4e3a200mV s<sup>&#8211;<\/sup><sup>1<\/sup>\u65f6\uff0c\u6837\u54c1\u8868\u73b0\u51fa\u8fd1\u4e4e\u7406\u60f3\u7684CV\u66f2\u7ebf\u3002\u8868\u660e\u4e86\u5feb\u901f\u52a8\u529b\u5b66\u548c\u9ad8\u529f\u7387\u5904\u7406\u80fd\u529b\u3002\u7ed3\u679c\u8868\u660e\uff0c\u57285000\u4e2a\u5145\u653e\u7535\u5faa\u73af\u4e2d\uff0c\u6837\u54c1\u662f\u7a33\u5b9a\u7684\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1039\/c5cc04359j<\/p>\n<p><strong><b>\u57fa\u4e8e<\/b><\/strong><strong><b>\u79bb\u5b50\u51dd\u80f6\u548c\u591a\u5b54\u78b3\u7eb3\u7c73\u7ea4\u7ef4\u7535\u6781<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u9ad8\u5ea6\u8010<\/b><\/strong><strong><b>\u7528<\/b><\/strong><strong><b>\u56fa\u6001\u8d85\u7ea7\u7535\u5bb9\u5668<\/b><\/strong><\/p>\n<p>\u5fb7\u96f7\u585e\u5c14\u5927\u5b66\u7684Vibha Kalra\u6559\u6388\u5728ACS Appl. Mater. Interfaces\u4e0a\u53d1\u8868\u9898\u4e3a\u201cHighly Durable, Self-Standing Solid-State Supercapacitor Based on an Ionic Liquid-Rich Ionogel and Porous Carbon Nanofiber Electrodes\u201d\u7684\u8bba\u6587\uff0c\u5c06\u542b\u670995%\u7684IL(1-\u4e59\u57fa-3-\u7532\u57fa\u54aa\u5511\u53cc\u4e9a\u80fa)\u548c5%\u7684\u7532\u57fa\u7ea4\u7ef4\u7d20(\u4e00\u79cd\u805a\u5408\u7269\u57fa\u8d28)\u7684\u79bb\u5b50\u6db2\u4f53(IL)\u7684\u79bb\u5b50\u51dd\u80f6\u4e0e\u9ad8\u5ea6\u4e92\u8054\u76843D\u6d3b\u6027\u70ad\u7eb3\u7c73\u7ea4\u7ef4(CNF)\u7535\u6781\u76f8\u7ed3\u5408\uff0c\u5236\u5907\u51fa\u9ad8\u6027\u80fd\u7684\u56fa\u6001\u8d85\u7ea7\u7535\u5bb9\u5668\u3002\u8be5\u79bb\u5b50\u51dd\u80f6\u5177\u6709\u5f88\u5f3a\u7684\u673a\u68b0\u6027\u80fd\uff0c\u5176\u50a8\u5b58\u6a21\u91cf\u4e3a5 MPa\uff0c\u572825\u2103\u4e0b\u7684\u9ad8\u79bb\u5b50\u7535\u5bfc\u7387\u4e3a5.7 mS cm<sup>\u22121<\/sup>\u3002\u901a\u8fc7\u9759\u7535\u7eba\u4e1d\u6280\u672f\u83b7\u5f97\u7684\u9ad8\u8868\u9762\u79efCDF\u57fa\u7535\u6781(2282 m<sup>2<\/sup>\u00a0g<sup>\u22121<\/sup>)\uff0cCNF\u7535\u6781\u7684\u591a\u5b54\u7ed3\u6784\u6709\u5229\u4e8e\u67d4\u8f6f\u4f46\u673a\u68b0\u8010\u7528\u7684\u79bb\u5b50\u51dd\u80f6\u819c\u7684\u8f7b\u677e\u6e17\u900f\uff0c\u4ece\u800c\u4f7f\u591a\u5b54\u7eb3\u7c73\u7ea4\u7ef4\u548c\u51dd\u80f6\u7535\u89e3\u8d28\u754c\u9762\u4e4b\u95f4\u7684\u4eb2\u5bc6\u63a5\u89e6\u6210\u4e3a\u53ef\u80fd\u3002\u8d85\u7ea7\u7535\u5bb9\u5668\u663e\u793a\u51fa\u826f\u597d\u7684\u7535\u5bb9\u7279\u6027\uff0c\u5305\u62ec153 F g<sup>\u22121<\/sup>\u7684\u91cd\u91cf\u7535\u5bb9\uff0c65 W h kg<sup>\u22121<\/sup>\u7684\u9ad8\u6bd4\u80fd\u5bc6\u5ea6\uff0c\u9ad8\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\u57281A g<sup>\u22121<\/sup>\u76842\u4e07\u6b21\u5145\u653e\u7535\u5faa\u73af\u540e\uff0c\u7535\u5bb9\u8870\u51cf\u4ec5\u4e3a4%\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1021\/acsami.7b07479\u00a0<\/p>\n<ul>\n<li><b><\/b><strong><b>\u4f7f\u7528<\/b><\/strong><strong><b>\u6c27\u5316\u8fd8\u539f\u6d3b\u6027\u7535\u89e3\u8d28<\/b><\/strong><\/li>\n<\/ul>\n<p>\u8003\u8651\u5230\u7535\u89e3\u8d28\u5360\u76f8\u5f53\u5927\u7684\u8d28\u91cf\/\u4f53\u79ef\u5206\u6570\uff0c\u4ee5CF\u4e3a\u57fa\u7840\u7684\u8d85\u7ea7\u7535\u5bb9\u5668\uff0c\u901a\u8fc7\u52a0\u5165\u4e00\u4e9b\u6c27\u5316\u8fd8\u539f\u6d3b\u6027\u6dfb\u52a0\u5242\u6765\u589e\u52a0\u80fd\u91cf\u5bc6\u5ea6\u662f\u6709\u6548\u7684\u3002\u6c27\u5316\u8fd8\u539f\u6dfb\u52a0\u5242\u5e94\u5728\u7535\u89e3\u8d28\u4e2d\u5177\u6709\u826f\u597d\u7684\u6eb6\u89e3\u5ea6\uff0c\u6216\u80fd\u5438\u9644\u5728\u7535\u6781\u4e0a\uff0c\u5e76\u80fd\u5728\u5faa\u73af\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u53d1\u751f\u53ef\u9006\u7684\u8fd8\u539f\/\u6c27\u5316\u53cd\u5e94\u3002<\/p>\n<p>\u6bd4\u5982\uff1a<\/p>\n<p><strong><b>\u53cc\u6c27\u5316\u8fd8\u539f\u79bb\u5b50\u6db2\u4f53\u7528\u4e8e\u9ad8\u6bd4\u80fd\u8d85\u7ea7\u7535\u5bb9\u5668<\/b><\/strong><\/p>\n<p>\u8499\u5f7c\u5229\u57c3\u7b2c\u4e00\u5927\u5b66 Olivier Fontaine\u6559\u6388\u7b49\u4eba\u5728Nature Materials\u4e0a\u53d1\u8868\u9898\u4e3a\u201cBiredox ionic liquids with solid-like redox density in the liquid state for high-energy supercapacitors\u201d\u7684\u8bba\u6587\uff0c\u4ecb\u7ecd\u4e86\u57fa\u4e8e\u53cc\u6c27\u5316\u8fd8\u539f\uff08biredox\uff09\u79bb\u5b50\u6db2\u4f53\uff0c\u5728\u7c7b\u6db2\u4f53\u5feb\u901f\u52a8\u529b\u5b66\u60c5\u51b5\u4e0b\u5b9e\u73b0\u7c7b\u56fa\u4f53\u6750\u6599\u6c27\u5316\u8fd8\u539f\u5bc6\u5ea6\u7684\u65b9\u6cd5\u3002\u8fd9\u4e9b\u53cc\u6c27\u5316\u8fd8\u539f\u79bb\u5b50\u6db2\u4f53\u7684\u9633\u79bb\u5b50\u548c\u9634\u79bb\u5b50\u5e26\u6709\u80fd\u8fdb\u884c\u5feb\u901f\u53ef\u9006\u6c27\u5316\u8fd8\u539f\u53cd\u5e94\u7684\u5206\u5b50\u3002\u8bc1\u660e\u5176\u7528\u4e8e\u9ad8\u5bb9\u91cf\/\u9ad8\u901f\u7387\u7535\u8377\u5b58\u50a8\u7684\u6f5c\u529b\uff0c\u5e76\u5728\u6c27\u5316\u8fd8\u539f\u8d85\u7ea7\u7535\u5bb9\u5668\u4e0a\u8fdb\u884c\u4e86\u6f14\u793a\u3002\u8fd9\u4e9b\u79bb\u5b50\u6db2\u4f53\u80fd\u591f\u901a\u8fc7\u5728\u7535\u6781\u7684\u5b54\u4e2d\u5b58\u50a8\u5927\u91cf\u7535\u8377\u6765\u5c06\u7535\u8377\u5b58\u50a8\u4e0e\u79bb\u5b50\u901a\u8fc7\u7684\u7535\u6781\u8868\u9762\u53bb\u8026\u5408\uff0c\u4ee5\u4f7f\u7531\u4e8e\u5c06\u6c27\u5316\u8fd8\u539f\u7269\u8d28\u4fdd\u7559\u5728\u5b54\u4e2d\u800c\u5bfc\u81f4\u7684\u81ea\u653e\u7535\u548c\u6cc4\u6f0f\u7535\u6d41\u6700\u5c0f\u5316\uff0c\u5e76\u7531\u5b83\u4eec\u8f83\u5bbd\u7684\u7535\u5316\u5b66\u7a97\u53e3\u6765\u63d0\u9ad8\u5de5\u4f5c\u7535\u538b\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1038\/nmat4808\u00a0<\/p>\n<p><strong><b>\u5f15\u5165\u53cc\u6781\u6027\u6709\u673a\u6c27\u5316\u8fd8\u539f\u81ea\u7531\u57fa\u6fc0\u53d1<\/b><\/strong><strong><b>\u53cc<\/b><\/strong><strong><b>\u7535\u5c42\u7535\u5bb9\u5668<\/b><\/strong><\/p>\n<p>\u78b3\u57fa\u7535\u5316\u5b66\u53cc\u5c42\u7535\u5bb9\u5668(EDLCs)\u901a\u5e38\u5177\u6709\u9ad8\u529f\u7387\u548c\u957f\u5bff\u547d\uff0c\u4f46\u80fd\u91cf\u5bc6\u5ea6\/\u7535\u5bb9\u8f83\u4f4e\u3002\u78b3\u6750\u6599\u7684\u5b54\/\u5f62\u6001\u4f18\u5316\u548c\u5047\u7535\u5bb9\u6750\u6599\u4fee\u9970\u5df2\u88ab\u7528\u6765\u63d0\u9ad8\u7535\u6781\u7535\u5bb9\u3002\u5728\u7535\u89e3\u6db2\u4e2d\u52a0\u5165\u53ef\u6eb6\u6027\u6c27\u5316\u8fd8\u539f\u4ecb\u8d28\u662f\u63d0\u9ad8\u7535\u6781\u7535\u5bb9\u7684\u4e00\u4e2a\u6709\u524d\u9014\u7684\u9009\u62e9\u3002\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u7684\u674e\u4f1a\u5de7\u6559\u6388\u548c\u590d\u65e6\u5927\u5b66\u7684\u738b\u6c38\u521a\u6559\u6388\u56e2\u961f\u5728Angew.\u4e0a\u53d1\u8868\u9898\u4e3a\u201cEnergize Electrochemical Double Layer Capacitor by Introducing an Ambipolar Organic Redox Radical in Electrolyte\u201d\u7684\u8bba\u6587\uff0c\u5c06\u4e00\u4e2a\u53cc\u6781\u6027\u6709\u673a\u81ea\u7531\u57faTEMPO\uff082, 2, 6,6-tetramethylpiperidinyloxyl\uff09\u5f15\u5165\u7535\u89e3\u6db2\u4e2d\uff0c\u901a\u8fc7\u6b63\u6781\u7684\u6c27\u5316\u548c\u8d1f\u6781\u7684\u8fd8\u539f\uff0c\u53ef\u4ee5\u663e\u8457\u5730\u589e\u52a0\u8d5d\u7535\u5bb9\u3002\u5e26\u6709TEMPO\u4ecb\u8d28\u7684EDLC\u7684\u80fd\u91cf\u5bc6\u5ea6\u9ad8\u8fbe51 Wh kg-1\uff0c\u662f\u4e0d\u542bTEMPO\u4ecb\u8d28\u7684\u7535\u5bb9\u5668\u76842.4\u500d\uff0c\u8be5\u7535\u5bb9\u5668\u4e5f\u8868\u73b0\u51fa\u4e86\u4f18\u5f02\u7684\u5faa\u73af\u7a33\u5b9a\u6027\uff0c\u957f\u5468\u671f\u7a33\u5b9a\u6027\u8d85\u8fc74000\u4e2a\u5468\u671f\u3002\u6240\u83b7\u5f97\u7684\u7ed3\u679c\u53ef\u80fd\u4e3a\u63d0\u9ad8EDLCs\u7684\u80fd\u91cf\u5bc6\u5ea6\u63d0\u4f9b\u65b0\u7684\u9014\u5f84\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI:\u00a010.1002\/anie.201804582\u00a0<\/p>\n<ul>\n<li><b><\/b><strong><b>\u4f7f\u7528<\/b><\/strong><strong><b>\u91d1\u5c5e\u7535\u6d41\u6536\u96c6\u5668<\/b><\/strong><\/li>\n<\/ul>\n<p>\u901a\u8fc7\u4f7f\u7528\u9ad8\u5bfc\u7535\u6027\u7684\u91d1\u5c5e\u7535\u6d41\u6536\u96c6\u5668\u53ef\u4ee5\u5feb\u901f\u5730\u5c06\u7535\u5b50\u4f20\u5bfc\u5230\u6d3b\u6027\u6750\u6599\u6216\u4ece\u6d3b\u6027\u6750\u6599\u4f20\u5bfc\u5230\u6d3b\u6027\u6750\u6599\uff0c\u663e\u7136\u53ef\u4ee5\u63d0\u9ad8\u901f\u7387\u6027\u80fd\u3002\u5728\u5e73\u9762\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u60c5\u51b5\u4e0b\uff0c\u901a\u5e38\u4f7f\u7528\u4e0d\u9508\u94a2\/\u94dd\/\u94c2\u7b94\/\u8584\u819c\u3002<\/p>\n<p>\u6bd4\u5982\uff1a<\/p>\n<p><strong><b>\u7eba\u7ec7\u54c1\u7528\u8d85\u9ad8\u901f\u5145\u653e\u7535<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u8d85\u7ea7\u7535\u5bb9\u5668<\/b><\/strong><\/p>\n<p>\u67d4\u6027\u3001\u53ef\u7a7f\u6234\u3001\u53ef\u690d\u5165\u5f0f\u548c\u6613\u4e8e\u91cd\u6784\u7684\u8d85\u7ea7\u7535\u5bb9\u5668\u4e3a\u7535\u5b50\u8bbe\u5907\u63d0\u4f9b\u4e86\u9ad8\u80fd\u91cf\u548c\u529f\u7387\u5bc6\u5ea6\u3002\u97e9\u56fd\u6c49\u9633\u5927\u5b66\u7684Seon Jeong Kim\u6559\u6388\u7b49\u4eba\u5728Nature\u00a0Commun.\u4e0a\u53d1\u8868\u9898\u4e3a\u201cUltrafast charge and discharge biscrolled yarn supercapacitors for textiles and microdevices\u201d\u7684\u8bba\u6587\uff0c\u6f14\u793a\u4e86\u53ef\u7f16\u7ec7\u3001\u53ef\u7f1d\u7eab\u3001\u53ef\u6253\u7ed3\u548c\u53ef\u7f16\u7ec7\u7684\u7eb1\u7ebf\uff0c\u5b83\u4eec\u662f\u6c27\u5316\u8fd8\u539f\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u9ad8\u6027\u80fd\u7535\u6781\u3002Biscrolling\u53ef\u4ee5\u5c06\u6570\u767e\u5c42\u5bfc\u7535\u805a\u5408\u7269\u6e17\u900f\u7684\u78b3\u7eb3\u7c73\u7ba1\u7247\u5377\u6210\u76f4\u5f84\u4e3a20um\u7684\u7eb1\u7ebf\u3002\u7528\u91d1\u5c5e\u7ebf\u96c6\u6d41\u5668\u8fde\u63a5\u53ccbiscrolled\u7eb1\u7ebf\u53ef\u4ee5\u63d0\u9ad8\u53d1\u7535\u80fd\u529b\u3002\u5bb9\u91cf\u9ad8(\u53ef\u8fbe179 F cm <sup>-3<\/sup>)\uff0c\u5bf9\u4e8e\u6db2\u4f53\u548c\u56fa\u4f53\u7535\u89e3\u8d28\uff0c\u5408\u80a1\u7ebf\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u653e\u7535\u7535\u6d41\u968f\u7535\u538b\u626b\u63cf\u7387\u7684\u589e\u5927\u800c\u7ebf\u6027\u589e\u5927.\u5b8c\u6574\u7684\u8d85\u7ea7\u7535\u5bb9\u5668\u5177\u6709\u6781\u9ad8\u7684\u80fd\u91cf\u5bc6\u5ea6\u548c\u529f\u7387\u5bc6\u5ea6\uff0c\u9ad8\u7684\u5faa\u73af\u5bff\u547d(\u5206\u522b\u4e3a92%\u548c99%\uff0c\u7ecf\u8fc710,000\u6b21\u5faa\u73af)\u5bf9\u7535\u5b50\u7eba\u7ec7\u54c1\u7684\u5e94\u7528\u5177\u6709\u91cd\u8981\u610f\u4e49\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1016\/j.jpowsour.2015.12.114\u00a0<\/p>\n<p><strong><b>\u57fa\u4e8e\u78b3\u7eb3\u7c73\u7ba1\/\u4e0d\u9508\u94a2\u82af<\/b><\/strong><strong><b>\u7eb1<\/b><\/strong><strong><b>\u7684\u53cc\u80a1\u7ebf\u8d85\u7ea7\u7535\u5bb9\u5668<\/b><\/strong><\/p>\n<p>\u7ebf\u6027\u8d85\u7ea7\u7535\u5bb9\u5668\u5728\u7535\u5b50\u7eba\u7ec7\u9886\u57df\u6709\u7740\u5de8\u5927\u7684\u53d1\u5c55\u6f5c\u529b\u3002\u7136\u800c\uff0c\u76ee\u524d\u62a5\u9053\u7684\u5927\u591a\u6570\u7eb1\u7ebf\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u80fd\u91cf\u5bc6\u5ea6\u4ecd\u7136\u5f88\u4f4e\uff0c\u5e76\u4e14\u968f\u7740\u8d85\u7ea7\u7535\u5bb9\u5668\u957f\u5ea6\u7684\u589e\u52a0\u800c\u663e\u8457\u964d\u4f4e\u3002\u534e\u5357\u7406\u5de5\u5927\u5b66\u7684Fenghua Su\u6559\u6388\u8054\u5408\u6fb3\u5927\u5229\u4e9aCSIRO\u7684Menghe Miao\u6559\u6388\u5728Journal of Power Sources\u53d1\u8868\u9898\u4e3a\u201cTwo-ply yarn supercapacitor based on carbon nanotube\/stainless steel core-sheath yarn electrodes and ionic liquid electrolyte\u201d\u7684\u8bba\u6587\uff0c\u62a5\u544a\u4e86\u4e00\u79cd\u57fa\u4e8e\u78b3\u7eb3\u7c73\u7ba1\/\u4e0d\u9508\u94a2\u5305\u82af\u7eb1\u7535\u6781\u548c\u79bb\u5b50\u6db2\u4f53\u7535\u89e3\u8d28\u7684\u53cc\u5c42\u8d85\u7ea7\u7535\u5bb9\u5668\u3002IL\u51dd\u80f6\u7535\u89e3\u8d28\u7684\u4f7f\u7528\u4f7f\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u7535\u4f4d\u7a97\u53e3\u4ece1.0 V\u6269\u5927\u52302.7 V\u3002\u78b3\u7eb3\u7c73\u7ba1\/\u4e0d\u9508\u94a2\u5305\u82af\u7eb1\u7ed3\u6784\u5927\u5927\u63d0\u9ad8\u4e86\u7535\u8377\u4f20\u8f93\u6548\u7387\uff0c\u5e76\u5141\u8bb8\u7ebf\u6027\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u957f\u5ea6\u5927\u5e45\u589e\u52a0\u3002\u6240\u5f97\u5230\u7684\u8d85\u7ea7\u7535\u5bb9\u5668\u5177\u6709\u5353\u8d8a\u7684\u7535\u5316\u5b66\u6027\u80fd\uff0c\u5176\u9ad8\u5bb9\u91cf\u7535\u5bb9\u4e3a263.31 F cm<sup>&#8211;<\/sup><sup>3<\/sup>\uff0c\u80fd\u91cf\u5bc6\u5ea6\u4e3a6.67\u217910<sup>&#8211;<\/sup><sup>2<\/sup>\u00a0Wh cm<sup>&#8211;<\/sup><sup>3<\/sup>\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1016\/j.jpowsour.2015.12.114\u00a0<\/p>\n<p><strong><b>4<\/b><\/strong><strong><b>\u00a0CF<\/b><\/strong><strong><b>s\u57fa<\/b><\/strong><strong><b>\u53ef\u5145\u7535\u7535\u6c60\u548c\u6df7\u5408\u7535\u6c60<\/b><\/strong><\/p>\n<p>\u4e0e\u8d85\u7ea7\u7535\u5bb9\u5668\u76f8\u6bd4\uff0c\u53ef\u5145\u7535\u7535\u6c60\u548c\u6df7\u5408\u7535\u6c60\u53ef\u4ee5\u63d0\u4f9b\u66f4\u9ad8\u7684\u80fd\u91cf\u5bc6\u5ea6\u3002\u5728\u8fd9\u4e9b\u91d1\u5c5e\u79bb\u5b50\u7535\u6c60\u548c\u6df7\u5408\u7535\u6c60\u4e2d\uff0c\u591a\u529f\u80fd\u7684CFs\u53ef\u4ee5\u4f5c\u4e3a\u672c\u8d28\u4e0a\u7684\u6d3b\u6027\u6b63\u8d1f\u6781\u6750\u6599\uff0c\u5bfc\u7535\u6dfb\u52a0\u5242\u548c\u529f\u80fd\u7535\u6d41\u6536\u96c6\u5668\u548c\u4e2d\u95f4\u5c42\u6dfb\u52a0\u5230\u5176\u4e2d\uff0c<\/p>\n<p>\u5176\u5177\u6709\u4ee5\u4e0b\u4f18\u70b9\uff1a\u5176\u5927\u5b54\u7ed3\u6784\u5177\u6709\u826f\u597d\u7684\u7535\u89e3\u8d28\u6e17\u900f\u548c\u79bb\u5b50\u6269\u6563\u52a8\u529b\u5b66\uff1b<\/p>\n<p>\u5b83\u4eec\u7684\u8fde\u7eed\u5bfc\u7535\u7f51\u7edc\u63d0\u4f9b\u4e86\u5feb\u901f\u7535\u8377(\u7535\u5b50\u6216\u7a7a\u7a74)\u5411\u6d3b\u6027\u6750\u6599\u548c\u91d1\u5c5e\u79bb\u5b50\u7684\u4f20\u8f93\uff1b<\/p>\n<p>\u4e0d\u9700\u8981\u805a\u5408\u7269\u7c98\u7ed3\u5242\u6216\u5bfc\u7535\u5242\uff0c\u53ef\u4f5c\u4e3a\u72ec\u7acb\u7684\u3001\u67d4\u6027\u7684\u3001\u8f7b\u8d28\u7684\u3001\u751a\u81f3\u7ed3\u6784\u7535\u6781\u4f7f\u7528\u3002<\/p>\n<ul>\n<li><b><\/b><strong><b>\u7eafCFs\u4f5c\u4e3a\u9633\u6781<\/b><\/strong><\/li>\n<\/ul>\n<p>\u53ef\u4f5c\u4e3a\u9502\u79bb\u5b50\u7535\u6c60\u548c\u7535\u5bb9\u5668\u7684\u9633\u6781\uff0c\u4f5c\u4e3a\u94a0\/\u94be\u79bb\u5b50\u7535\u6c60\u548c\u7535\u5bb9\u7684\u9633\u6781\u7b49\u3002<\/p>\n<p>\u6bd4\u5982\uff1a<\/p>\n<p><strong><b>\u6765\u81ea\u6728\u8d28\u7d20\u7684\u9ad8\u5f3a\u5ea6\u9502\u79bb\u5b50\u7535\u6c60\u9633\u6781<\/b><\/strong><\/p>\n<p>\u7f8e\u56fd\u6a61\u6811\u5cad\u56fd\u5bb6\u5b9e\u9a8c\u5ba4\u7684Wyatt E. Tenhaeff\u6559\u6388\u7b49\u4eba\u5728AFM\u4e0a\u53d1\u8868\u4e3a\u9898\u201cHighly Robust Lithium Ion Battery Anodes from Lignin: An Abundant, Renewable, and Low-Cost Material\u201d\u7684\u8bba\u6587\uff0c\u62a5\u9053\u4e86\u4e00\u79cd\u5b8c\u5168\u7531\u5929\u7136\u548c\u53ef\u518d\u751f\u8d44\u6e90\u5236\u6210\u7684\u4f4e\u6210\u672c\u7535\u6c60\u7535\u6781\u7684\u5408\u6210\u3001\u52a0\u5de5\u548c\u6027\u80fd\u3002\u8fd9\u79cd\u9633\u6781\u6750\u6599\u5177\u6709\u53ef\u8c03\u7684\u7535\u5316\u5b66\u6027\u80fd\uff0c\u9002\u7528\u4e8e\u9ad8\u529f\u7387\u548c\u9ad8\u80fd\u91cf\u7684\u5e94\u7528\u3002\u63d0\u51fa\u4e86\u4e00\u79cd\u80fd\u76f4\u63a5\u4ea7\u751f\u7535\u4e92\u8fde\u4e09\u7ef4\u7ed3\u6784\u7684\u5408\u6210\u65b9\u6cd5\uff0c\u5176\u4e2d\u78b3\u6846\u67b6\u4f5c\u4e3a\u96c6\u7535\u4f53\u548c\u9502\u63d2\u5165\u6750\u6599\uff0c\u6d88\u9664\u4e86\u4f20\u7edf\u8bbe\u8ba1\u4e2d\u60f0\u6027\u6750\u6599\u7684\u989d\u5916\u8d28\u91cf\u548c\u8d39\u7528\u3002\u7ea4\u7ef4\u72b6\u78b3\u7535\u6781\u6750\u6599\u662f\u5229\u7528\u53ef\u6269\u5c55\u7684\u7194\u4f53\u52a0\u5de5\u6280\u672f\u548c\u70ed\u8f6c\u6362\u65b9\u6cd5\u4ece\u8403\u53d6\u6728\u8d28\u7d20\u7684\u6eb6\u5242\u4e2d\u5f97\u5230\u7684\u3002\u6240\u5f97\u5230\u7684\u72ec\u7acb\u7535\u6781\u7684\u7535\u5316\u5b66\u6027\u80fd\u4e0e\u5546\u7528\u78b3\u57fa\u9633\u6781\u76f8\u5f53\uff0c\u800c\u6750\u6599\u548c\u52a0\u5de5\u6210\u672c\u4ec5\u4e3a\u540e\u8005\u7684\u51e0\u5206\u4e4b\u4e00\u3002\u7ec4\u5206\u548c\u7535\u5316\u5b66\u8868\u5f81\u8868\u660e\uff0c\u78b3\u5316\u6728\u8d28\u7d20\u5177\u6709\u65e0\u5e8f\u7684\u7eb3\u7c73\u6676\u7ed3\u6784\u3002\u5728\u4f20\u7edf\u7684\u975e\u8d28\u5b50\u578b\u6709\u673a\u7535\u89e3\u8d28\u4e2d\uff0c\u78b3\u5316\u6be1\u5faa\u73af\u53ef\u9006\uff0c\u5e93\u4ed1\u6548\u7387\u8d85\u8fc799.9%\u3002\u6b64\u5916\uff0c\u57282000\u2103\u78b3\u5316\u7684\u6728\u8d28\u7d20\u78b3\u7ea4\u7ef4\u57281M LiPF<sub>6<\/sub>\u7684\u78b3\u9178\u4e19\u70ef\u916f\u4e2d\u53ef\u4ee5\u53ef\u9006\u5faa\u73af\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1002\/adfm.201301420\u00a0<\/p>\n<p><strong><b>\u5bcc\u6c2eC<\/b><\/strong><strong><b>F<\/b><\/strong><strong><b>\u57fa\u94a0<\/b><\/strong><strong><b>\u7535\u5bb9\u5668\u9633\u6781<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u7535\u8377\u5b58\u50a8\u673a\u5236<\/b><\/strong><\/p>\n<p>\u9a6c\u514b\u65af\u00b7\u666e\u6717\u514b\u80f6\u4f53\u548c\u754c\u9762\u7814\u7a76\u6240\u7684Martin Oschatz\u6559\u6388\u7b49\u4eba\u5728 AFM\u4e0a\u53d1\u8868\u9898\u4e3a\u201cUnderstanding the Charge Storage Mechanism to Achieve High Capacity and Fast Ion Storage in Sodium-Ion Capacitor Anodes by Using Electrospun Nitrogen-Doped Carbon Fibers\u201d\u7684\u8bba\u6587\uff0c\u4ee5\u516d\u6c2e\u6742\u82ef\u4e8c\u8148(HAT-CN)\u548c\u805a\u4e59\u70ef\u5421\u54af\u70f7\u916e\u4e3a\u539f\u6599\uff0c\u901a\u8fc7\u7535\u7eba\u4e1d\u7684\u65b9\u6cd5\u5236\u5907\u5fae\u5b54\u5bcc\u6c2e\u70ad\u7ea4\u7ef4(HAT-CNFs)\u3002\u7ed3\u952e\u52a8\u673a\u3001\u7535\u5b50\u7ed3\u6784\u3001\u6c2e\u6742\u539f\u5b50\u542b\u91cf\u3001\u5b54\u9699\u7387\u3001\u78b3\u5806\u79ef\u7a0b\u5ea6\u7b49\u90fd\u53ef\u4ee5\u901a\u8fc7\u51b7\u51dd\u6e29\u5ea6\u6765\u63a7\u5236\u3002HAT-CNFs\u5177\u6709\u663e\u8457\u7684\u53ef\u9006\u5bb9\u91cf(0.1 A g<sup>\u22121<\/sup>\u65f6\u4e3a395 mAh g<sup>\u22121<\/sup>)\u548c\u901f\u7387\u80fd\u529b(10 A g<sup>\u22121<\/sup>\u65f6\u4e3a106 mAh g<sup>\u22121<\/sup>)\uff0c\u53ef\u4f5c\u4e3a\u94a0\u50a8\u5b58\u7684\u6b63\u6781\u6750\u6599\uff0cHAT-CNFs\u8fd8\u4f5c\u4e3a\u4e00\u7cfb\u5217\u6a21\u578b\u5316\u5408\u7269\uff0c\u7528\u4e8e\u7814\u7a76\u63d2\u5c42\u548c\u4ee5\u4e0d\u540c\u901f\u7387\u53ef\u9006\u7ed3\u5408\u5728\u6c2e\u4f4d\u70b9\u4e0a\u5bf9\u94a0\u50a8\u5b58\u7684\u8d21\u732e\u3002\u4ee5HAT-CNF\u4e3a\u9633\u6781\uff0c\u4ee5\u76d0\u6a21\u538b\u591a\u5b54\u78b3\u4e3a\u9634\u6781\u7684\u6df7\u5408\u5f0f\u94a0\u79bb\u5b50\u7535\u5bb9\u5168\u7535\u6c60\uff0c\u57280.5-4.0 V\u7684\u7535\u538b\u8303\u56f4\u5185\u5177\u6709\u663e\u8457\u7684\u6027\u80fd\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1002\/adfm.201902858\u00a0<\/p>\n<ul>\n<li><b><\/b><strong><b>\u5ba2<\/b><\/strong><strong><b>\u8f7d\u7684CFs\u4f5c\u4e3a\u9633\u6781<\/b><\/strong><\/li>\n<\/ul>\n<p>\u591a\u79cd\u975e\u78b3\u8d1f\u6781\u6750\u6599\u53ef\u4ee5\u540c\u65f6\u63d0\u4f9b\u9ad8\u5bb9\u91cf\u548c\u826f\u597d\u7684\u5145\u653e\u7535\u5e73\u53f0\u3002\u56e0\u6b64,\u6742\u5316CFs\u4e0e\u8fd9\u4e9b\u7535\u5b50\u6750\u6599\u4e00\u8d77\uff0c\u540c\u65f6\u5f15\u5165\u5145\u7535\u5e73\u53f0\uff0c\u56e0\u6b64\u6709\u6548\u5730\u589e\u52a0\u4e86\u9502\/\u94a0\/\u94be\u79bb\u5b50\u7535\u6c60\u548c\u7535\u5bb9\u5668\u7684\u80fd\u91cf\u5bc6\u5ea6\u3002<\/p>\n<p>\u6bd4\u5982\uff1a<\/p>\n<p><strong><b>T-Nb<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>O<\/b><\/strong><strong><sub><b>5<\/b><\/sub><\/strong><strong><b>\/\u78b3\u7eb3\u7c73\u7ea4\u7ef4\u819c\u5b9e\u73b0\u67d4\u6027\u9ad8\u529f\u7387\u94a0\u79bb\u5b50\u7535\u5bb9\u5668<\/b><\/strong><\/p>\n<p>\u6df7\u5408\u94a0\u79bb\u5b50\u7535\u5bb9\u5668\u56e0\u5176\u517c\u5177\u7535\u6c60\u548c\u8d85\u7ea7\u7535\u5bb9\u5668\u7684\u4f18\u70b9\u4ee5\u53ca\u94a0\u8d44\u6e90\u7684\u4f4e\u6210\u672c\u800c\u5907\u53d7\u5173\u6ce8\u3002\u7136\u800c\uff0c\u9633\u6781\u4e2dNa<sup>+<\/sup>\u7684\u7f13\u6162\u6269\u6563\u963b\u788d\u4e86\u5176\u7684\u8fdb\u4e00\u6b65\u53d1\u5c55\u3002\u4e3a\u4e86\u5b9e\u73b0\u5feb\u901f\u6c27\u5316\u8fd8\u539f\u52a8\u529b\u5b66\uff0c\u534e\u4e2d\u79d1\u6280\u5927\u5b66\u80e1\u5148\u7f57\u6559\u6388\u8bfe\u9898\u7ec4\u5728Small\u4e0a\u53d1\u8868\u9898\u4e3a\u201cMesopore-Induced Ultrafast Na+-Storage in T-Nb<sub>2<\/sub>O<sub>5<\/sub>\/Carbon Nanofber Films toward Flexible High-Power Na-Ion Capacitors\u201d\u7684\u8bba\u6587\uff0c\u901a\u8fc7\u539f\u4f4dSiO<sub>2<\/sub>\u00a0\u523b\u8680\u6280\u672f\u7ec4\u88c5\u4e86\u4ecb\u5b54\u6b63\u4ea4Nb<sub>2<\/sub>O<sub>5<\/sub>-\u78b3\u7eb3\u7c73\u7ea4\u7ef4\u7f51\u7edc\u3002\u6240\u5f97\u7684\u4ecb\u5b54\u6750\u6599\u4e3aT-Nb<sub>2<\/sub>O<sub>5<\/sub>(m-Nb<sub>2<\/sub>O<sub>5<\/sub>)\/CNF\u819c\u662f\u673a\u68b0\u67d4\u6027\u7684\uff0c\u4e0d\u4f7f\u7528\u4efb\u4f55\u6dfb\u52a0\u5242\u3001\u7c98\u5408\u5242\u6216\u7535\u6d41\u6536\u96c6\u5668\u3002\u539f\u4f4d\u5f62\u6210\u7684\u4ecb\u5b54\u53ef\u4ee5\u6709\u6548\u5730\u63d0\u9ad8m-Nb<sub>2<\/sub>O<sub>5<\/sub>\/CNF\u7535\u6781\u7684Na<sup>+<\/sup>\u5b58\u50a8\u6027\u80fd\uff0c\u6bd4\u5982\u826f\u597d\u7684\u500d\u7387\u80fd\u529b(\u6700\u9ad8\u53ef\u8fbe150\u2103)\u548c\u51fa\u8272\u7684\u5faa\u73af\u80fd\u529b(100\u2103\u4e0b10000\u6b21\u5faa\u73af\u540e\u7684\u4fdd\u7559\u7387\u4e3a94%)\u3002\u57fa\u4e8em-Nb<sub>2<\/sub>O<sub>5<\/sub>\/CNF\u9633\u6781\u548c\u77f3\u58a8\u70ef\u6846\u67b6(GF)\/\u4ecb\u5b54\u78b3\u7eb3\u7c73\u7ba1(mCNF)\u9634\u6781\u7684\u67d4\u6027\u5668\u4ef6\uff0c\u572855Wh\/kg\u7684\u80fd\u91cf\u5bc6\u5ea6\u4e0b\u5177\u670960KW\/kg\u7684\u8d85\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1002\/smll.201804539<\/p>\n<p><strong><b>\u7845\/\u77f3\u58a8\u70ef\/\u78b3\u7eb3\u7c73\u7ebf\u4e09\u7ef4\u67d4\u6027\u7535\u6781<\/b><\/strong><\/p>\n<p>\u5f00\u53d1\u9ad8\u6027\u80fd\u3001\u957f\u5faa\u73af\u5bff\u547d\u7684\u7535\u6781\u6750\u6599\u662f\u9502\u79bb\u5b50\u7535\u6c60\u7684\u6838\u5fc3\u95ee\u9898\u3002\u6e56\u5357\u5927\u5b66\u7684\u9c81\u5175\u5b89\u6559\u6388\u8bfe\u9898\u7ec4\u5728ACS Nano\u4e0a\u53d1\u8868\u9898\u4e3a\u201cAtomic-Scale Control of Silicon Expansion<br \/>\n Space as Ultrastable Battery Anodes\u201d\u7684\u8bba\u6587\uff0c\u5229\u7528\u539f\u5b50\u5c42\u6c89\u79ef\u548c\u9759\u7535\u7eba\u4e1d\u76f8\u7ed3\u5408\u5236\u5907\u4e86\u7845\/\u77f3\u58a8\u70ef\/\u78b3\u7eb3\u7c73\u7ebf\u4e09\u7ef4\u67d4\u6027\u7535\u6781\u3002\u5229\u7528\u539f\u5b50\u5c42\u6c89\u79ef\u5de7\u5999\u5730\u5b9e\u73b0\u4e86\u7eb3\u7c73\u7845\u5728\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u7684\u81a8\u80c0\u7a7a\u95f4\u539f\u5b50\u7ea7\u522b\u7684\u63a7\u5236\u3002\u7845\u7eb3\u7c73\u9897\u7c92\u88ab\u7cbe\u786e\u548c\u53ef\u63a7\u7684\u7a7a\u9699\u7a7a\u95f4\u6240\u5305\u56f4\uff0c\u4ece\u800c\u4fdd\u8bc1\u4e86\u4f18\u5f02\u7684\u673a\u68b0\u5f3a\u5ea6\uff0c\u5e76\u63d0\u4f9b\u4e86\u8db3\u591f\u7684\u7a7a\u95f4\u6765\u514b\u670d\u7845\u7eb3\u7c73\u9897\u7c92\u5728\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u4f53\u79ef\u81a8\u80c0\u6240\u9020\u6210\u7684\u635f\u4f24\u3002\u540c\u65f6\u7531\u4e8e\u77f3\u58a8\u70ef\u548c\u78b3\u7ea4\u7ef4\u7684\u9ad8\u5bfc\u7535\u6027\u4f7f\u5f97\u7535\u6781\u6750\u6599\u5177\u6709\u826f\u597d\u7684\u500d\u7387\u6027\u80fd\uff0c\u5728700\u00a0mA\/g\u7684\u7535\u6d41\u5bc6\u5ea6\u5faa\u73af1050\u6b21\u540e\uff088\u4e2a\u6708\u5de6\u53f3\u65f6\u95f4\u6301\u7eed\u5faa\u73af\uff09\uff0c\u8be5\u7535\u6781\u6750\u6599\u4efb\u5c55\u73b0\u51fa2002\u00a0mAh\/g\u7684\u53ef\u9006\u5bb9\u91cf\uff08\u5e73\u5747\u6bcf\u4e2a\u5faa\u73af\u8870\u51cf0.006\uff05\uff09\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI:10.1021\/acsnano.6b04522<\/p>\n<ul>\n<li><b><\/b><strong><b>\u5ba2\u8f7dCFs\u4e3a\u9634\u6781<\/b><\/strong><\/li>\n<\/ul>\n<p>\u7531\u4e8eCFs\u5728\u666e\u901a\u7535\u89e3\u8d28\u7684\u7535\u4f4d\u7a97\u5185\u5bb9\u91cf\u8f83\u4f4e\uff0c\u56e0\u6b64\u5f88\u5c11\u88ab\u7814\u7a76\u4f5c\u4e3a\u672c\u8d28\u4e0a\u662f\u53ef\u5145\u7535\u7535\u6c60\u7684\u6d3b\u6027\u9634\u6781\u6750\u6599\u3002\u56e0\u6b64\uff0c\u6709\u5fc5\u8981\u5c06\u5bfc\u7535CFs\u4e0e\u9ad8\u5bb9\u91cf\u9634\u6781\u6750\u6599\u76f8\u7ed3\u5408\uff0c\u4f5c\u4e3a\u67d4\u6027\/\u53ef\u7a7f\u6234\/\u7ed3\u6784\u7535\u6c60\u7684\u9634\u6781\u3002<\/p>\n<p>\u6bd4\u5982\uff1a<\/p>\n<p><strong><b>\u4e00\u79cd\u7ebf\u72b6\u7684\u9502\u786b\u7535\u6c60<\/b><\/strong><\/p>\n<p>\u590d\u65e6\u5927\u5b66\u7684\u5f6d\u6167\u80dc\u6559\u6388\u5728AM\u4e0a\u53d1\u8868\u9898\u4e3a\u201cA Cable-Shaped Lithium Sulfur Battery\u201d\u7684\u8bba\u6587\uff0c\u62a5\u544a\u4e86\u4e00\u7ef4\u7ebf\u72b6\u7684\u9502\u786b\u7535\u6c60\u4f7f\u7528\u78b3\u7eb3\u7c73\u590d\u5408\u7ea4\u7ef4\u4f5c\u4e3a\u786b\u9634\u6781\u3002\u8fd9\u5f52\u529f\u4e8e\u4e8e\u78b3\u7eb3\u7c73\u7ba1(CNT)\u3001\u4ecb\u5b54\u78b3(MC)\u9897\u7c92\u548c\u6c27\u5316\u77f3\u58a8\u70ef(GO)\u5c42\u7684\u7efc\u5408\u4f18\u70b9\uff0c\u9634\u6781\u5177\u6709\u826f\u597d\u7684\u7269\u7406\u6027\u80fd\u548c\u8f83\u9ad8\u7684\u7535\u5316\u5b66\u6027\u80fd\u3002\u4ee5\u8be5\u590d\u5408\u7ea4\u7ef4\u4e3a\u786b\u9634\u6781\uff0c\u5236\u5907\u7ebf\u72b6\u9502\u786b\u7535\u6c60\u3002\u5b83\u5c55\u793a\u4e86\u6539\u8fdb\u7684\u5bff\u547d\u548c\u663e\u8457\u7684\u53d8\u5f62\u987a\u5e94\u6027\uff0c\u4f7f\u5b83\u8d85\u8d8a\u5176\u4ed6\u5149\u7ea4\u5f62\u7535\u6c60\u548c\u9886\u5148\u4e8e\u5176\u4ed6\u67d4\u6027\u80fd\u6e90\u8bbe\u5907\u3002\u8fd9\u9879\u5de5\u4f5c\u4e3a\u53ef\u7a7f\u6234\u8bbe\u5907\u7684\u9ad8\u6f0f\u78c1\u7387\u548c\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u4e4b\u95f4\u7684\u9e3f\u6c9f\u63d0\u4f9b\u4e86\u4e00\u4e2a\u901a\u7528\u7684\u89e3\u51b3\u65b9\u6848\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1002\/adma.201504241<\/p>\n<p><strong><b>\u5177\u6709\u4f18\u5f02\u7684\u7535\u5316\u5b66\u6027\u80fd<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u67d4\u6027\u591a\u5b54\u78b3\u7eb3\u7c73\u7ea4\u7ef4-\u7852\u9634\u6781<\/b><\/strong><\/p>\n<p>\u4e2d\u56fd\u79d1\u5b66\u6280\u672f\u5927\u5b66\u6731\u5f66\u6b66\u6559\u6388\u7b49\u4eba\u5728AEM\u4e0a\u53d1\u8868\u9898\u4e3a\u201cA Flexible Porous Carbon Nanofibers-Selenium Cathode with Superior Electrochemical Performance for Both Li-Se and Na-Se Batteries\u201d\u7684\u8bba\u6587\u5c06\u7852\u6e17\u900f\u5230\u4ecb\u5b54\u78b3\u7eb3\u7c73\u7ea4\u7ef4(PCNFs)\u4e2d\uff0c\u5236\u5907\u4e86\u4e00\u79cd\u67d4\u6027\u3001\u81ea\u7acb\u7684\u591a\u5b54\u78b3\u7eb3\u7c73\u7ea4\u7ef4\/\u7852\u590d\u5408\u7535\u6781(Se@PCNFs)\u3002\u5177\u6709\u4f18\u5316\u4ecb\u5b54\u5bb9\u7eb3\u7852\u7684\u591a\u5b54\u78b3\u53ef\u4ee5\u534f\u540c\u6291\u5236\u6d3b\u6027\u7269\u8d28\u7684\u6eb6\u89e3\uff0c\u63d0\u4f9b\u819c\u6240\u9700\u7684\u673a\u68b0\u7a33\u5b9a\u6027\u3002Se@PCNFs\u7535\u6781\u5728\u9502\u79bb\u5b50\u548c\u94a0\u79bb\u5b50\u5b58\u50a8\u65b9\u9762\u90fd\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u7535\u5316\u5b66\u6027\u80fd\u3002\u5bf9\u4e8e\u9502\u79bb\u5b50\u5b58\u50a8\u5668\uff0c\u7ecf\u8fc7900\u6b21\u5faa\u73af\u540e\uff0c\u5b83\u7684\u53ef\u9006\u5bb9\u91cf\u4e3a516mA g<sup>\u22121<\/sup>\uff0c\u800c\u57280.5 A g<sup>\u22121<\/sup>\u4e0b\u6ca1\u6709\u4efb\u4f55\u5bb9\u91cf\u635f\u5931\u3002\u5f53\u7528\u4e8e\u94a0-\u7852\u7535\u6c60\u65f6\uff0c\u8be5\u590d\u5408\u7535\u6781\u5728\u4ee50.05 Ag<sup>\u22121<\/sup>\u7684\u901f\u7387\u8fdb\u884c80\u6b21\u5faa\u73af\u540e\uff0c\u5176\u53ef\u9006\u5bb9\u91cf\u4e3a520 mAh g<sup>\u22121<\/sup>\uff0c1\u00a0A g<sup>\u22121<\/sup>\u901f\u7387\u4e3a230 mAh g<sup>\u22121<\/sup>\u3002\u7531\u4e8e\u7852\u5728PCNFs\u4e2d\u7684\u5747\u5300\u5206\u5e03\u4e0e\u4e09\u7ef4\u4e92\u8054\u7684PCNFs\u9aa8\u67b6\u7684\u534f\u540c\u4f5c\u7528\uff0c\u4f7f\u5f97\u7852\u5728PCNFs\u4e2d\u5177\u6709\u9ad8\u7684\u5bb9\u91cf\u3001\u826f\u597d\u7684\u5faa\u73af\u6027\u548c\u901f\u7387\u80fd\u529b\uff0c\u53ef\u4ee5\u7f13\u89e3\u591a\u7852\u5316\u5408\u7269\u4e2d\u95f4\u4f53\u5728\u5faa\u73af\u8fc7\u7a0b\u4e2d\u7684\u7a7f\u68ad\u53cd\u5e94\uff0c\u5e76\u5728\u6574\u4e2a\u7535\u6781\u4e2d\u4fdd\u6301\u826f\u597d\u7684\u5bfc\u7535\u6027\u3002\u901a\u8fc7\u5408\u7406\u3001\u7cbe\u5de7\u7684\u8bbe\u8ba1\uff0c\u8fd9\u79cd\u81ea\u652f\u6491\u7535\u6781\u6709\u671b\u6210\u4e3a\u9ad8\u529f\u7387\u3001\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u9502-\u7852\u7535\u6c60\u548c\u94a0-\u7852\u7535\u6c60\u7684\u53d1\u5c55\u65b9\u5411\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI:\u00a010.1002\/aenm.201401377\u00a0<\/p>\n<ul>\n<li><b><\/b><strong><b>CFs\u4f5c\u4e3a\u5bfc\u7535\u6dfb\u52a0\u5242<\/b><\/strong><strong><b>\u7b49<\/b><\/strong><\/li>\n<\/ul>\n<p>\u7531\u4e8eCFs\u7684\u9ad8\u7eb5\u6a2a\u6bd4\u548c\u826f\u597d\u7684\u5bfc\u7535\u6027\uff0c\u5b83\u5728\u63d0\u9ad8\u53ef\u5145\u7535\u7535\u6c60\u6d3b\u6027\u7535\u6781\u7684\u5bfc\u7535\u6027\u548c\u7535\u5316\u5b66\u6027\u80fd\u65b9\u9762\u4f18\u4e8e\u5176\u4ed6\u5bfc\u7535\u6dfb\u52a0\u5242\/\u4e2d\u95f4\u5c42\u3002<\/p>\n<p>\u6bd4\u5982\uff1a<\/p>\n<p><strong><b>\u6784\u5efa\u78b3\u7ea4\u7ef4\u4e09\u7ef4\u7f51\u7edc<\/b><\/strong><strong><b>\u5b9e\u73b0<\/b><\/strong><strong><b>Na<\/b><\/strong><strong><sub><b>3<\/b><\/sub><\/strong><strong><b>V<\/b><\/strong><strong><sub><b>2<\/b><\/sub><\/strong><strong><b>(PO<\/b><\/strong><strong><sub><b>4<\/b><\/sub><\/strong><strong><b>)<\/b><\/strong><strong><sub><b>3<\/b><\/sub><\/strong><strong><b>@\u78b3\u8d1f\u8f7d<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u8d85\u957f\u5faa\u73af\u5bff\u547d\u548c\u8d85\u9ad8\u901f\u94a0\u79bb\u5b50\u7535\u6c60<\/b><\/strong><\/p>\n<p>\u5927\u591a\u6570\u67d4\u6027\u7535\u6781\u4e2d\u6d3b\u6027\u6750\u6599\u7684\u8d28\u91cf\u8f7d\u8377\u8f83\u4f4e\uff0c\u8fd9\u5927\u5927\u963b\u788d\u4e86\u5b83\u4eec\u7684\u5b9e\u9645\u5e94\u7528\u3002\u5317\u4eac\u7406\u5de5\u5927\u5b66\u7684Minhua Cao\u8054\u5408\u97e9\u56fd\u6c49\u9633\u5927\u5b66Yang-Kook Sun\u6559\u6388\u7b49\u4eba\u5728Nano Energy\u4e0a\u53d1\u8868\u9898\u4e3a\u201cAchieving high mass loading of Na<sub>3<\/sub>V<sub>2<\/sub>(PO<sub>4<\/sub>)<sub>3<\/sub>@carbon on carbon cloth by constructing three-dimensional network between carbon fibers for ultralong cycle-life and ultrahigh rate sodium-ion batteries\u201d\u7684\u8bba\u6587\uff0c\u62a5\u544a\u4e86\u4e00\u79cd\u7b80\u5355\u7684\u7b56\u7565\u6765\u5b9e\u73b0\u9ad8\u8d28\u91cf\u8d1f\u8f7d\u7684Na<sub>3<\/sub>V<sub>2<\/sub>(PO4)<sub>3<\/sub>@\u78b3(NVP@C-CC)\u5728\u78b3\u5e03(NVP@C- CC)\u4e0a\uff0c\u901a\u8fc7\u4e24\u6b65\u6d82\u5c42\u548c\u9000\u706b\u5904\u7406\uff0c\u5f97\u5230\u7684NVP@C- cc\u819c\u53ef\u4ee5\u7528\u4f5c\u94a0\u79bb\u5b50\u7535\u6c60(SIBs)\u7684\u65e0\u7c98\u7ed3\u9634\u6781\u3002NVP@C\u4e0d\u4ec5\u5747\u5300\u5730\u56fa\u5b9a\u5728CC\u7684\u78b3\u7ea4\u7ef4\u8868\u9762\uff0c\u800c\u4e14\u78b3\u7ea4\u7ef4\u4e4b\u95f4\u4ee5\u4e92\u8054\u7684\u4e09\u7ef4(3D)\u5927\u5b54\u7ed3\u6784\u586b\u5145\u3002\u6b63\u662f\u56e0\u4e3a\u5145\u5206\u5229\u7528\u4e86\u78b3\u7ea4\u7ef4\u4e4b\u95f4\u7684\u7a7a\u9699\uff0c\u6211\u4eec\u5b9e\u73b0\u4e86\u9ad8\u7684NVP@C\u8d28\u91cf\u8d1f\u8f7d\u3002\u5145\u5206\u8bc4\u4f30\u7684\u7535\u6c60\u9634\u6781(\u9633\u6781\u4e3aNaTi<sub>2<\/sub>(PO<sub>4<\/sub>)<sub>3<\/sub>@C)\uff0c\u5b83\u4e5f\u8868\u73b0\u51fa\u4f18\u8d8a\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u548c\u901f\u7387\u6027\u80fd\u65f6\u3002\u672c\u7814\u7a76\u4e3a\u5b9e\u73b0\u67d4\u6027\u50a8\u80fd\u88c5\u7f6e\u4e2d\u67d4\u6027\u652f\u67b6\u4e0a\u6d3b\u6027\u6750\u6599\u7684\u9ad8\u8d28\u91cf\u8d1f\u8f7d\u63d0\u4f9b\u4e86\u4e00\u79cd\u65b0\u7684\u7b56\u7565\u3002\u901a\u8fc7\u5728\u78b3\u7ea4\u7ef4\u95f4\u5efa\u7acb\u4e09\u7ef4\u7f51\u7edc\uff0c\u5b9e\u73b0\u4e86\u9ad8\u8d28\u91cf\u8d1f\u8f7d\u7684NVP@C-CC\u7535\u6781\u3002NVP@C-CC\u7535\u6781\u5bf9\u94a0\u534a\u7535\u6c60\u548c\u5168\u7535\u6c60\u9634\u6781\u5747\u8868\u73b0\u51fa\u826f\u597d\u7684\u5faa\u73af\u6027\u80fd\u548c\u4f18\u8d8a\u7684\u901f\u7387\u5bb9\u91cf(\u9633\u6781\u4e3aNaTi<sub>2<\/sub>(PO<sub>4<\/sub>)<sub>3<\/sub>@C)\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1016\/j.nanoen.2017.12.038\u00a0<\/p>\n<p><strong><b>\u7528\u4e8e\u9ad8\u7a33\u5b9a\u94a0\u91d1\u5c5e\u9633\u6781\u76843D\u67d4\u6027\u78b3\u6be1\u4e3b\u4f53<\/b><\/strong><\/p>\n<p>\u5177\u6709\u9ad8\u7406\u8bba\u5bb9\u91cf\u548c\u6700\u4f4e\u7535\u5316\u5b66\u7535\u4f4d\u7684\u94a0\uff08Na\uff09\u91d1\u5c5e\u88ab\u8ba4\u4e3a\u662f\u7528\u4e8e\u94a0\u91d1\u5c5e\u7535\u6c60\u7684\u6709\u524d\u666f\u7684\u8d1f\u6781\u6750\u6599\u3002\u7136\u800c\uff0cNa\u7684\u679d\u6676\u751f\u957f\u548c\u5faa\u73af\u4e2d\u7684\u5927\u4f53\u79ef\u53d8\u5316\u4e25\u91cd\u963b\u788d\u4e86\u5176\u5b9e\u9645\u5e94\u7528\u3002\u5317\u4eac\u79d1\u6280\u5927\u5b66\u8303\u4e3d\u73cd\u6559\u6388\u7b49\u4eba\u5728AEM\u4e0a\u53d1\u8868\u9898\u4e3a\u201c3D Flexible Carbon Felt Host for Highly Stable Sodium Metal Anodes\u201d\u7684\u8bba\u6587\uff0c\u8868\u660e\u5df2\u7ecf\u5927\u89c4\u6a21\u5546\u4e1a\u5316\u76843D\u67d4\u6027\u78b3\uff08C\uff09\u6be1\u53ef\u4ee5\u7528\u4e8e\u901a\u8fc7\u7194\u878d\u6ce8\u5165\u7b56\u7565\u9884\u5b58Na\u7684\u4e3b\u4f53\uff0c\u901a\u8fc7\u8be5\u6ce8\u5165\u7b56\u7565\u83b7\u5f97Na\/C\u590d\u5408\u8d1f\u6781\u3002\u7531\u4e8e\u91d1\u5c5eNa\u88ab\u9650\u5236\u5728\u5bfc\u7535\u78b3\u6be1\u4e3b\u4f53\u4e2d\uff0c\u6240\u4ee5\u5f97\u5230\u7684\u8d1f\u6781\u5728\u5bf9\u79f0\u7535\u6c60\u4e2d\u7684\u78b3\u9178\u76d0\u57fa\u7535\u89e3\u8d28\u4e2d\u8868\u73b0\u51fa\u7a33\u5b9a\u7684\u7535\u538b\u5206\u5e03\u548c120\u6b21\u5faa\u73af\u7684\u5c0f\u6ede\u540e\uff0c\u8fd9\u589e\u52a0\u4e86Na<sup>+<\/sup>\u6c89\u79ef\u4f4d\u70b9\u4ee5\u964d\u4f4e\u6709\u6548\u7535\u6d41\u5bc6\u5ea6\u5e76\u4f7fNa\u5f62\u6838\u5747\u5300\uff0c\u4ece\u800c\u9650\u5236\u7535\u5316\u5b66\u5faa\u73af\u4e2d\u7684\u5c3a\u5bf8\u53d8\u5316\u3002\u66f4\u91cd\u8981\u7684\u662f\uff0c\u53ef\u4ee5\u6709\u6548\u6291\u5236\u94a0\u679d\u6676\u751f\u957f\u548c\u5927\u4f53\u79ef\u53d8\u5316\u3002\u5f53\u4e0eNa<sub>0.67<\/sub>Ni<sub>0.33<\/sub>Mn<sub>0.67<\/sub>O<sub>2<\/sub>\u6b63\u6781\u7ed3\u5408\u65f6\uff0cNa\/C\u590d\u5408\u6750\u6599\u5728\u5168\u7535\u6c60\u4e2d\u8868\u73b0\u51fa\u826f\u597d\u7684\u9002\u7528\u6027\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1002\/aenm.201702764\u00a0<\/p>\n<p><strong><b>5<\/b><\/strong><strong><b>\u00a0\u57fa\u4e8eCF<\/b><\/strong><strong><b>s<\/b><\/strong><strong><b>\u7684\u9ad8\u7ea7EESDs\u7684\u5e94\u7528<\/b><\/strong><\/p>\n<p><strong><b>\u9ad8\u5bb9\u91cf\u67d4\u6027\u9502\u79bb\u5b50\u7535\u6c60<\/b><\/strong><strong><b>\u7528\u4e8e<\/b><\/strong><strong><b>\u667a\u80fd\u5bfc\u7535\u7eba\u7ec7\u54c1<\/b><\/strong><\/p>\n<p>\u667a\u80fd\u5bfc\u7535\u7eba\u7ec7\u54c1\u5177\u6709\u56fa\u6709\u7684\u67d4\u6027\u3001\u7ea4\u7ef4\u7f51\u72b6\u3001\u8868\u9762\u7c97\u7cd9\u3001\u9644\u7740\u529b\u5f3a\u3001\u5bfc\u7535\u6027\u597d\u7b49\u4f18\u70b9\uff0c\u88ab\u7528\u4f5c\u67d4\u6027LIBs\u7684\u7535\u6d41\u6536\u96c6\u5668\u3002\u7eb3\u7c73\u5c3a\u5bf8\u7684\u6c27\u5316\u949b\u9502(LTO)\u548c\u78f7\u9178\u94c1\u9502(LFP)\u6d3b\u6027\u6750\u6599\u8fdb\u4e00\u6b65\u589e\u5f3a\u4e86\u5bfc\u7535\u6027\u548c\u67d4\u97e7\u6027\uff0c\u97e9\u56fd\u6c49\u9633\u5927\u5b66\u7684Yun Jung Lee\u6559\u6388\u7b49\u4eba\u5728Small\u4e0a\u53d1\u8868\u9898\u4e3a\u201cFlexible Lithium-Ion Batteries with High Areal Capacity Enabled by Smart Conductive Textiles\u201d\u7684\u8bba\u6587\uff0c\u8bbe\u8ba1\u5c06\u5b83\u4eec\u4e0e\u67d4\u6027\u7684\u4e8c\u7ef4\u77f3\u58a8\u70ef\u6df7\u5408\uff0c\u7531\u6b64\u4ea7\u751f\u7684LTO\/LFP\u5168\u7535\u6c60\u5177\u6709\u8f83\u9ad8\u7684\u9762\u79ef\u5bb9\u91cf\u548c\u7075\u6d3b\u6027\uff0c\u5e76\u80fd\u627f\u53d7\u673a\u68b0\u75b2\u52b3\u3002\u8be5\u7535\u6c60\u7684\u5bb9\u91cf\u8fbe\u52301.2 mA h cm<sup>\u22122<\/sup>\uff0c\u540c\u65f6\u8868\u73b0\u51fa\u826f\u597d\u7684\u7075\u6d3b\u6027\uff0c\u7535\u6c60\u572810 mm\u7684\u5f2f\u66f2\u534a\u5f84\u4e0b\u53cd\u590d\u5f2f\u66f21000\u6b21\u540e\u8868\u73b0\u51fa\u7a33\u5b9a\u7684\u5f00\u8def\u7535\u538b\u4fdd\u6301\u80fd\u529b\uff0c\u672a\u5f2f\u66f2\u7535\u6c60\u7684\u653e\u7535\u5bb9\u91cf\u5728\u5206\u522b\u4ee530\u300120\u548c10 mm\u7684\u5f2f\u66f2\u534a\u5f84\u5f2f\u66f2100\u6b21\u540e\u7684\u7535\u6c60\u4e2d\u5f97\u4ee5\u4fdd\u7559\uff0c\u8fd9\u8bc1\u5b9e\u4e86\u8fd9\u79cd\u7535\u6781\u914d\u7f6e\u53ef\u6210\u529f\u9632\u6b62\u91cd\u590d\u53d8\u5f62\u65f6\u7ed3\u6784\u635f\u574f\uff08\u5206\u5c42\u6216\u7834\u88c2\uff09\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI:10.1002\/smll.201703418<\/p>\n<p>\u5bfc\u7535\u78b3\u7d20\u7ec7\u7269\u7167\u7247\u53ca\u7535\u6781\u5236\u5907\u793a\u610f\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196765 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72475-27.png\" alt=\"\" width=\"700\" height=\"390\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72475-27.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72475-27-300x167.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p><strong><b>\u57fa\u4e8e\u6539\u6027\u78b3\u7ea4\u7ef4\u7684\u591a\u529f\u80fd\u7ed3\u6784\u8d85\u7ea7\u7535\u5bb9\u5668\u590d\u5408\u6750\u6599<\/b><\/strong><\/p>\n<p>\u4f26\u6566\u5e1d\u56fd\u7406\u5de5\u5b66\u9662\u7684Milo S. P. Shaffer \u6559\u6388\u7b49\u4eba\u5728ACS Appl. Mater. Interfaces\u4e0a\u53d1\u8868\u9898\u4e3a\u201cMultifunctional Structural Supercapacitor Composites Based on Carbon Aerogel Modified High Performance Carbon Fiber Fabric\u201d\u7684\u8bba\u6587\uff0c\u8bbe\u8ba1\u4e86\u4e00\u79cd\u65b0\u578b\u591a\u529f\u80fd\u6750\u6599\uff0c\u5c06\u7ed3\u6784\u78b3\u7ea4\u7ef4\u7ec7\u7269\u5d4c\u5165\u78b3\u6c14\u51dd\u80f6\uff08CAG\uff09\u7684\u8fde\u7eed\u7f51\u7edc\u4e2d\uff0c\u5f62\u6210\u4e86\u4e00\u4e2a\u7c98\u7ed3\u4f46\u591a\u5b54\u7684\u6574\u4f53\uff0c\u53ef\u63d0\u4f9b\u51fa\u8272\u7684\u673a\u68b0\u6027\u80fd\uff0c\u540c\u65f6\u62e5\u6709\u9002\u5408\u7535\u5316\u5b66\u80fd\u91cf\u5b58\u50a8\u7684\u9ad8\u7535\u5316\u5b66\u8868\u9762\u79ef\u3002\u7ed3\u679c\u8868\u660e\uff0cCAG\u6539\u6027\u5de5\u827a\u5177\u6709\u53ef\u6269\u5c55\u6027\uff0c\u5e76\u4e14\u4e0e\u4e00\u7cfb\u5217\u5177\u6709\u4e0d\u540c\u8868\u9762\u7279\u6027\u7684\u78b3\u7ea4\u7ef4\u7ec7\u7269\u517c\u5bb9\u3002CAG\u7684\u52a0\u5165\u663e\u7740\u589e\u52a0\u4e86\u78b3\u7ea4\u7ef4\u7ec7\u7269\u7684\u8868\u9762\u79ef\uff0c\u56e0\u6b64\u4f7f\u7535\u5316\u5b66\u6027\u80fd\u63d0\u9ad8\u4e86\u7ea6100\u500d\u3002\u4f7f\u7528\u79bb\u5b50\u6db2\u4f53\uff08IL\uff09\u7535\u89e3\u8d28\uff0c\u5728\u5c06CAG\u5f15\u5165\u78b3\u7ea4\u7ef4\u7ec7\u7269\u540e\uff0c\u4f30\u8ba1\u7684\u80fd\u91cf\u5bc6\u5ea6\u4ece0.003\u589e\u81f31 Wh kg<sup>-1<\/sup>\u3002\u5c06\u4e24\u79cd\u6d78\u6709CAG\u7684\u78b3\u7ea4\u7ef4\u7ec7\u7269\u5939\u5728\u7edd\u7f18\u9694\u677f\u5468\u56f4\uff0c\u4ee5\u5f62\u6210\u529f\u80fd\u6b63\u5e38\u7684\u7ed3\u6784\u7535\u5316\u5b66\u53cc\u5c42\u7535\u5bb9\u5668\u590d\u5408\u6750\u6599\u3002 CAG\u6539\u6027\u4e0d\u4ec5\u6539\u5584\u4e86\u7535\u5316\u5b66\u8868\u9762\u79ef\uff0c\u800c\u4e14\u589e\u5f3a\u4e86\u4e00\u6b21\u7ea4\u7ef4\u5468\u56f4\u7684\u805a\u5408\u7269\u57fa\u4f53\uff0c\u4ece\u800c\u663e\u7740\u6539\u5584\u4e86\u57fa\u4f53\u4e3b\u5bfc\u7684\u590d\u5408\u6750\u6599\u7684\u6027\u80fd\u3002\u89c2\u5bdf\u5230\u9762\u5185\u526a\u5207\u5f3a\u5ea6\u548c\u6a21\u91cf\u63d0\u9ad8\u4e864.5\u500d\uff0c\u8fd9\u8868\u660eCAG\u6539\u6027\u7684\u7ed3\u6784\u78b3\u7ea4\u7ef4\u7ec7\u7269\u5728\u7ed3\u6784\u548c\u591a\u529f\u80fd\u50a8\u80fd\u5e94\u7528\u4e2d\u90fd\u6709\u5e0c\u671b\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1021\/am400947j\u00a0<\/p>\n<p>\u57fa\u4e8eCAG\u6539\u6027\u7684\u591a\u529f\u80fd\u7ed3\u6784\u8d85\u7ea7\u7535\u5bb9\u5668\u88c5\u7f6e\u6982\u5ff5\u793a\u610f\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196766 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72476-24.png\" alt=\"\" width=\"700\" height=\"394\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72476-24.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72476-24-300x169.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p><strong><b>\u7535\u81f4\u53d8\u8272\u7684\u7ea4\u7ef4<\/b><\/strong><strong><b>\u578b<\/b><\/strong><strong><b>\u8d85\u7ea7\u7535\u5bb9\u5668<\/b><\/strong><\/p>\n<p>\u667a\u80fd\u7535\u5b50\u4ea7\u54c1\u4ee3\u8868\u4e86\u73b0\u4ee3\u7535\u5b50\u5b66\u4e2d\u4e00\u4e2a\u5d2d\u65b0\u7684\uff0c\u6709\u5e0c\u671b\u7684\u65b9\u5411\u3002\u667a\u80fd\u7535\u5b50\u8bbe\u5907\uff08\u4f8b\u5982\u667a\u80fd\u624b\u673a\uff0c\u667a\u80fd\u624b\u73af\u548c\u773c\u955c\uff09\u7684\u666e\u53ca\uff0c\u91cd\u65b0\u5f15\u8d77\u4e86\u4eba\u4eec\u5bf9\u5176\u50a8\u80fd\u914d\u4ef6\u7684\u5174\u8da3\u3002 \u590d\u65e6\u5927\u5b66\u7684\u5f6d\u6167\u80dc\u56e2\u961f\u5728AM\u4e0a\u53d1\u8868\u9898\u4e3a\u201cElectrochromic Fiber-Shaped Supercapacitors\u201d\u7684\u8bba\u6587\uff0c\u901a\u8fc7\u5728\u5f39\u6027\u7ea4\u7ef4\u4e0a\u7f20\u7ed5\u53d6\u5411\u7684\u78b3\u7eb3\u7c73\u7ba1\/\u805a\u82ef\u80fa\u590d\u5408\u8584\u819c\u7535\u6781\uff0c\u5f00\u53d1\u4e86\u4e00\u79cd\u65b0\u578b\u7684\u7535\u81f4\u53d8\u8272\u3001\u67d4\u6027\u3001\u53ef\u62c9\u4f38\u7684\u7ea4\u7ef4\u578b\u8d85\u7ea7\u7535\u5bb9\u5668\u3002\u8fd9\u4e9b\u7ea4\u7ef4\u5f62\u72b6\u7684\u8d85\u7ea7\u7535\u5bb9\u5668\u5728\u4e0d\u540c\u7684\u5de5\u4f5c\u9636\u6bb5\u4e4b\u95f4\u8868\u73b0\u51fa\u5feb\u901f\u4e14\u53ef\u9006\u7684\u5f69\u8272\u8f6c\u6362\uff0c\u56e0\u6b64\u63d0\u4f9b\u4e86\u6709\u5173\u5176\u5de5\u4f5c\u72b6\u6001\u7684\u52a8\u6001\u4e14\u6709\u6548\u7684\u4fe1\u606f\u3002\u867d\u7136\u5728PANI\u7684\u57fa\u7840\u4e0a\u4e3b\u8981\u5c55\u793a\u4e86\u4e09\u79cd\u5178\u578b\u7684\u989c\u8272\uff0c\u5373\u6de1\u9ec4\u8272\u3001\u84dd\u8272\u548c\u7eff\u8272\uff0c\u4f46\u662f\u5176\u4ed6\u989c\u8272\u4e5f\u53ef\u4ee5\u6839\u636e\u540c\u6837\u7684\u7b56\u7565\u9009\u62e9\u5176\u4ed6\u805a\u5408\u7269\u6216\u91d1\u5c5e\u6c27\u5316\u7269\u7b49\u65e0\u673a\u6750\u6599\u6765\u5b9e\u73b0\u3002\u8fd9\u4e9b\u7535\u81f4\u53d8\u8272\u7684\u7ea4\u7ef4\u578b\u8d85\u7ea7\u7535\u5bb9\u5668\u5728\u5f2f\u66f2\u3001\u62c9\u4f38\u7b49\u53d8\u5f62\u6761\u4ef6\u4e0b\u4e5f\u8868\u73b0\u51fa\u826f\u597d\u7684\u7535\u5316\u5b66\u6027\u80fd\uff0c\u9664\u7528\u4e8e\u50a8\u80fd\u5916\uff0c\u8fd8\u53ef\u5e7f\u6cdb\u5e94\u7528\u4e8e\u663e\u793a\u9886\u57df\u3002\u8fd9\u9879\u5de5\u4f5c\u53ef\u4ee5\u4f5c\u4e3a\u901a\u8fc7\u63a2\u7d22\u9ad8\u6548\u7684\u94ec\u5408\u91d1\u6216\u5176\u4ed6\u667a\u80fd\u7535\u5b50\u8bbe\u5907\u6765\u5f00\u53d1\u663e\u793a\u4ea7\u54c1\u7684\u8d77\u70b9\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aDOI: 10.1002\/adma.201403243<\/p>\n<p>\u5145\u653e\u7535\u8fc7\u7a0b\u4e2d\u7684\u8272\u8f6c\u53d8<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-196767 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72477-18.png\" alt=\"\" width=\"700\" height=\"555\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72477-18.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/02\/\u56fe\u72477-18-300x238.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p><strong><b>\u6311\u6218\u4e0e\u5c55\u671b<\/b><\/strong><\/p>\n<p>\u5148\u524d\u7684\u7814\u7a76\u5df2\u7ecf\u8bc1\u660e\uff0cCFs\u662f\u6784\u5efa\u5e7f\u6cdb\u5e94\u7528\u7684\u9ad8\u7ea7EESDs\u7684\u4f18\u79c0\u5019\u9009\u3002\u7136\u800c\uff0c\u5728\u5b9e\u73b0\u5927\u89c4\u6a21\u5e94\u7528\u7a0b\u5e8f\u4e4b\u524d\uff0c\u5b83\u4eec\u4ecd\u7136\u9762\u4e34\u8bb8\u591a\u6311\u6218\uff1a\u57fa\u672c\u6784\u4ef6\u7684\u7ed3\u6784\u548c\u6027\u80fd\u9700\u8981\u5408\u6210\u5177\u6709\u7cbe\u786e\u7ed3\u6784\u7684\u524d\u9a71\u4f53\u548c\u7eb3\u7c73\u78b3\u5316\u7269\uff1b\u63a7\u5236\u7ea4\u7ef4\u7684\u5f62\u6210\u8fc7\u7a0b\u5bf9\u9002\u7528\u4e8e\u4e0d\u540c\u5e94\u7528\u7684\u9ad8\u7ea7EESD\uff0c\u9ad8\u6548\u4f4e\u6210\u672c\u5927\u89c4\u6a21\u751f\u4ea7CFs\u81f3\u5173\u91cd\u8981\uff1b\u6709\u6548\u5730\u8bbe\u8ba1\u548c\u7ec4\u88c5\u5177\u6709\u9ad8\u91cd\u91cf\/\u4f53\u79ef\u80fd\u91cf\u548c\u529f\u7387\u5bc6\u5ea6\u4e14\u4f7f\u7528\u5bff\u547d\u957f\u7684\u53ef\u9760EESDs\u3002\u7136\u800c\uff0cCF\u5bb6\u65cf\u7684\u65b0\u6210\u5458\u53ef\u80fd\u5728\u4e0d\u4e45\u7684\u5c06\u6765\u88ab\u5f00\u53d1\uff0c\u4f8b\u5982\uff0c\u77f3\u58a8\u70ef\u7ea4\u7ef4\u3001\u73bb\u78b3\u7ea4\u7ef4\u548c\u78b3\u7094\u7ea4\u7ef4\uff0c\u4e3a\u5148\u8fdb\u7684EESDs\u63d0\u4f9b\u4e86\u65b0\u7684\u5fae\u89c2\u7ed3\u6784\u3001\u65b0\u7684\u6027\u80fd\u548c\u65b0\u7684\u673a\u4f1a\u3002\u968f\u7740CFs\u751f\u4ea7\u6280\u672f\u7684\u7a81\u7834\u548cEESD\u7cfb\u7edf\u7684\u53d1\u5c55\uff0c\u6211\u4eec\u76f8\u4fe1CFs\u5c06\u5728\u5e2e\u52a9\u6211\u4eec\u7684\u65e5\u5e38\u751f\u6d3b\u548c\u5b9e\u73b0\u4e00\u4e2a\u6e05\u6d01\u80fd\u6e90\u7684\u4e16\u754c\u4e2d\u626e\u6f14\u91cd\u8981\u7684\u89d2\u8272\u3002<\/p>\n<p>\u672c\u6587\u7531Junas\u4f9b\u7a3f\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u5148\u8fdb\u7684\u7535\u5316\u5b66\u50a8\u80fd\u88c5\u7f6e(EESDs)\u53ef\u4ee5\u6709\u6548\u5730\u50a8\u5b58\u7535\u80fd\uff0c\u540c\u65f6\u53c8\u5177\u6709\u5fae\u578b\/\u67d4\u6027\/\u53ef\u7a7f\u6234\/\u627f\u91cd\u7684\u7279\u70b9\uff0c\u56e0\u6b64\uff0c\u4ece\u67d4\u6027\/\u53ef\u7a7f\u6234\/\u4fbf\u643a\u5f0f\u7535\u5b50\u4ea7\u54c1\u5230\u8f7b\u578b\u7535\u52a8\u6c7d\u8f66\/\u822a\u7a7a\u822a\u5929\u8bbe\u5907&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":196757,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-196756","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/196756"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=196756"}],"version-history":[{"count":7,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/196756\/revisions"}],"predecessor-version":[{"id":198604,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/196756\/revisions\/198604"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/196757"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=196756"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=196756"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=196756"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}