{"id":197579,"date":"2020-03-06T06:45:11","date_gmt":"2020-03-05T22:45:11","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=197579"},"modified":"2020-03-05T16:50:00","modified_gmt":"2020-03-05T08:50:00","slug":"materials-today%ef%bc%9a%e5%a4%a7%e9%9d%a2%e7%a7%af%e5%88%b6%e5%a4%87%e4%ba%8c%e7%bb%b4%e9%9d%9e%e6%99%b6%e5%90%88%e9%87%91%e4%bb%a5%e5%8f%8a%e4%ba%8c%e7%bb%b4%e9%ab%98%e7%86%b5%e5%90%88%e9%87%91","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=197579","title":{"rendered":"Materials Today\uff1a\u5927\u9762\u79ef\u5236\u5907\u4e8c\u7ef4\u975e\u6676\u5408\u91d1\u4ee5\u53ca\u4e8c\u7ef4\u9ad8\u71b5\u5408\u91d1"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u8fd1\u5341\u51e0\u5e74\u6765\uff0c\u77f3\u58a8\u70ef\u3001\u4e8c\u786b\u5316\u94bc\u7b49\u4e8c\u7ef4\u6750\u6599\u56e0\u5176\u72ec\u7279\u7684\u7eb3\u7c73\u7ed3\u6784\u53ca\u4f4e\u7ef4\u7279\u6027\u5728\u6750\u6599\u9886\u57df\u5f15\u8d77\u4e86\u5e7f\u6cdb\u5173\u6ce8\u3002\u5b66\u8005\u4eec\u4e0d\u65ad\u63a2\u7d22\u4e8c\u7ef4\u6750\u6599\u6240\u7279\u6709\u7684\u7269\u7406\u548c\u5316\u5b66\u6027\u8d28\uff0c\u5e76\u5f00\u62d3\u4e86\u5176\u5728\u9ad8\u7075\u654f\u5ea6\u4f20\u611f\u5668\uff0c\u67d4\u6027\u7535\u5b50\uff0c\u5316\u5b66\u50ac\u5316\u7b49\u9886\u57df\u7684\u5e94\u7528\u6f5c\u529b\u3002\u9664\u8fd9\u4e9b\u5177\u6709\u5c42\u72b6\u7ed3\u6784\u7684\u672c\u5f81\u4e8c\u7ef4\u6750\u6599\u4ee5\u5916\uff0c\u5982\u4f55\u964d\u4f4e\u91d1\u5c5e\u6750\u6599\u7684\u7ef4\u5ea6\u5e76\u5236\u5907\u51fa\u8d85\u8584\u65e0\u57fa\u5e95\u91d1\u5c5e\u8584\u819c\uff0c\u4e5f\u5c31\u662f\u4e8c\u7ef4\u91d1\u5c5e\uff0c\u4ea6\u6210\u4e3a\u4e86\u79d1\u7814\u4eba\u5458\u5173\u6ce8\u7684\u70ed\u70b9\u3002\u91d1\u5c5e\u6750\u6599\u7684\u672c\u5f81\u7ed3\u6784\u51b3\u5b9a\u4e86\u5176\u5b58\u5728\u5f62\u5f0f\u503e\u5411\u4e8e\u4e09\u7ef4\u800c\u975e\u4e8c\u7ef4\uff0c\u56e0\u6b64\u4e8c\u7ef4\u91d1\u5c5e\u7684\u5236\u5907\u8fc7\u7a0b\u4e5f\u76f8\u5bf9\u7e41\u7410\u548c\u56f0\u96be\u3002\u73b0\u6709\u7684\u4e8c\u7ef4\u91d1\u5c5e\u5236\u5907\u65b9\u6cd5\u4ee5\u6eb6\u6db2\u73af\u5883\u4e0b\u7684\u5316\u5b66\u5408\u6210\u4e3a\u4e3b\uff0c\u5176\u5236\u5907\u65b9\u6cd5\u901a\u5e38\u9488\u5bf9\u7279\u5b9a\u5355\u4e00\u91d1\u5c5e\u5355\u8d28\uff0c\u91d1\u5c5e\u7684\u751f\u957f\u8fc7\u7a0b\u4e5f\u901a\u5e38\u8f83\u4e3a\u7f13\u6162\u3002\u56e0\u800c\u5176\u6240\u80fd\u5236\u5907\u7684\u4e8c\u7ef4\u91d1\u5c5e\u7684\u5316\u5b66\u6210\u5206\u8f83\u4e3a\u5355\u4e00\u4e14\u9762\u79ef\u8f83\u5c0f\u3002\u5bf9\u4e8e\u6210\u4efd\u548c\u7ed3\u6784\u66f4\u4e3a\u590d\u6742\u7684\u591a\u7ec4\u5143\u5408\u91d1\u6750\u6599\uff0c\u4f8b\u5982\u5e7f\u4e3a\u4eba\u77e5\u7684\u91d1\u5c5e\u73bb\u7483\u4ee5\u53ca\u8fd1\u4e9b\u5e74\u53d1\u5c55\u8fc5\u731b\u7684\u9ad8\u71b5\u5408\u91d1\uff0c\u73b0\u6709\u7684\u5408\u6210\u65b9\u6cd5\u675f\u624b\u65e0\u7b56\u3002\u800c\u4f5c\u4e3a\u6253\u5f00\u591a\u7ec4\u5143\u5408\u91d1\u5728\u4f4e\u7ef4\u5ea6\u4e0b\u6027\u8d28\u7814\u7a76\u7684\u4e00\u4e2a\u7a81\u7834\u53e3\uff0c\u5bf9\u4e8c\u7ef4\u590d\u6742\u91d1\u5c5e\u5236\u5907\u65b9\u6cd5\u7684\u63a2\u7d22\u4e0e\u6539\u826f\u6210\u4e3a\u8feb\u5207\u9700\u8981\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\u6768\u52c7\u6559\u6388\uff08\u901a\u8baf\u4f5c\u8005\uff09\u56e2\u961f\u5728\u590d\u6742\u4e8c\u7ef4\u91d1\u5c5e\u5236\u5907\u65b9\u6cd5\u7684\u63a2\u7d22\u4e0a\u5b9e\u73b0\u4e86\u65b0\u7684\u7a81\u7834\uff0c\u5229\u7528\u65b0\u5f00\u53d1\u7684\u65b9\u6cd5\u6210\u529f\u5236\u5907\u4e86\u591a\u79cd\u65e0\u57fa\u5e95\u4e8c\u7ef4\u91d1\u5c5e\u53ca\u9676\u74f7\u8584\u819c\uff0c\u5305\u62ecTi\uff0c ZrCuAlNi\u975e\u6676\u5408\u91d1, FeCoNiCrNb\u9ad8\u71b5\u5408\u91d1\u4ee5\u53ca\u975e\u6676\u7845\uff0cSiC \u9676\u74f7\uff0cAg-C \u590d\u5408\u6750\u6599\u7b49\u3002\u65b0\u5236\u5907\u65b9\u6cd5\u8868\u73b0\u51fa\u4e86\u5bf9\u591a\u79cd\u6750\u6599\u7684\u5e7f\u6cdb\u9002\u7528\u6027\u3002\u6240\u5236\u5907\u51fa\u7684\u4e8c\u7ef4\u91d1\u5c5e\u548c\u9676\u74f7\u4ea6\u5728\u9762\u79ef\u5c3a\u5ea6\u4e0a\u5b9e\u73b0\u4e86\u7a81\u7834\uff1a\u4ee5\u4e8c\u7ef4Ti\u4e3a\u4f8b\uff0c\u5728\u539a\u5ea6\u7ef4\u6301\u572820nm \u7684\u5c3a\u5bf8\u4e0b\uff0c\u5176\u6a2a\u5411\u5c3a\u5bf8\u53ef\u4ee5\u5ef6\u4f38\u81f3\u5398\u7c73\u7684\u5b8f\u89c2\u5c3a\u5ea6\uff0c\u8fb9\u957f\u4e0e\u539a\u5ea6\u7684\u6a2a\u7eb5\u6bd4\u8fbe\u5230\u4e8610<sup>6<\/sup> \u91cf\u7ea7\uff1b\u4e8c\u7ef4TiO2\u7684\u539a\u5ea6\u751a\u81f3\u53ef\u4f4e\u81f35nm\uff0c\u800c\u6a2a\u5411\u5c3a\u5bf8\u4e5f\u5728\u5398\u7c73\u5c3a\u5ea6\u3002\u5236\u5907\u65b9\u6cd5\u4ee5\u70ed\u538b\u6539\u826f\u7684\u805a\u4e59\u70ef\u9187\uff08PVA\uff09\u805a\u5408\u7269\u4e3a\u57fa\u5e95\uff0c\u4ee5\u78c1\u63a7\u6e85\u5c04\u7b49\u5e38\u89c4\u7269\u7406\u6c14\u76f8\u6c89\u79ef\u4e3a\u8584\u819c\u5f62\u6210\u624b\u6bb5\uff0c\u5229\u7528\u91d1\u5c5e-\u805a\u5408\u7269\u754c\u9762\u5728\u5e94\u529b\u4f5c\u7528\u4e0b\u7684\u8868\u9762\u4e0d\u7a33\u5b9a\u6027\u4f5c\u4e3a\u9a71\u52a8\u529b\uff08polymer surface buckling enabled exfoliation, PSBEE\uff09, \u6210\u529f\u5b9e\u73b0\u4e86\u91d1\u5c5e\u548c\u9676\u74f7\u8584\u819c\u7684\u5265\u79bb\u3002\u5728\u8fdb\u4e00\u6b65\u7684\u7814\u7a76\u4e2d\uff0c\u56e2\u961f\u53d1\u73b0\u8be5\u5236\u5907\u65b9\u6cd5\u4ea6\u5177\u6709\u826f\u597d\u7684\u53ef\u8c03\u63a7\u6027\u3002\u91d1\u5c5e\u8584\u819c\u5728\u542b\u6c34\u91cf\uff0c\u5f39\u6027\u6a21\u91cf\u4e0d\u540c\u7684PVA\u57fa\u5e95\u4e0a\u7684\u5265\u79bb\u884c\u4e3a\u8868\u73b0\u51fa\u4e86\u4ece\u5fae\u7c73\u5377\u5230\u5927\u9762\u79ef\u819c\u7684\u8f6c\u53d8\u3002\u5b9e\u9a8c\u7ed3\u679c\u4ea6\u8868\u660e\uff0c\u9540\u819c\u63a9\u6a21\u677f\u7684\u5f15\u5165\u53ef\u6709\u6548\u63a7\u5236\u4e8c\u7ef4\u91d1\u5c5e\u7684\u5f62\u6001\u4e0e\u5927\u5c0f\u3002\u76f8\u5173\u7814\u7a76\u6210\u679c\u4ee5\u9898\u4e3a\u201cThe Controlled Large-Area Synthesis of Two Dimensioanl Metals\u201d\u53d1\u8868\u5728\u4e86Materials Today\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p>\u56fe1. \u57fa\u4e8ePSBEE\u7684\u4e8c\u7ef4\u91d1\u5c5e\u5236\u5907\u65b9\u6cd5\u793a\u610f\u56fe\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/1-17.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-197583\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/1-17.jpg\" alt=\"\" width=\"700\" height=\"407\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/1-17.jpg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/1-17-300x174.jpg 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/a><\/p>\n<p>a)\u4ee5PVA \u4e3a\u57fa\u5e95\u7684\u57fa\u4e8ePSBEE\u7684\u4e8c\u7ef4\u91d1\u5c5e\u5236\u5907\u6d41\u7a0b\u56fe\u3002<\/p>\n<p>b)3D\u6253\u5370\u51fa\u7684PVA\u677f\u5b9e\u62cd\u7167\u7247\u3002<\/p>\n<p>c)3D\u6253\u5370\u51fa\u7684PVA\u8868\u9762\u5f62\u8c8c\u3002<\/p>\n<p>d)\u70ed\u538b\u540e\u7684PVA\u57fa\u677f\u5b9e\u62cd\u7167\u7247\u3002<\/p>\n<p>e)\u70ed\u538b\u540e\u7684PVA\u8868\u9762\u5f62\u8c8c\u3002<\/p>\n<p>f)\u8868\u9762\u6c89\u79efTi\u819c\u540e\u7684PVA\u57fa\u677f\u5b9e\u62cd\u7167\u7247\u3002<\/p>\n<p>g)\u6c89\u79efTi\u819c\u540e\u7684PVA\u8868\u9762\u5f62\u8c8c\u3002<\/p>\n<p>h)<strong>\u2013 <\/strong>i)\u4ecePVA\u57fa\u677f\u4e0a\u5265\u79bb\u540e\u60ac\u6d6e\u5728\u6c34\u4e2d\u7684\u65e0\u57fa\u5e95Ti\u8584\u819c\u3002<\/p>\n<p>\u56fe2. \u57fa\u4e8e\u672c\u6587\u65b9\u6cd5\u5236\u5907\u51fa\u7684\u4e8c\u7ef4\u91d1\u5c5e\u7684\u7ed3\u6784\u548c\u51e0\u4f55\u8868\u5f81\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/2-14.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-197584\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/2-14.jpg\" alt=\"\" width=\"700\" height=\"707\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/2-14.jpg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/2-14-297x300.jpg 297w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/a><\/p>\n<p>a)\u2013 c)\u8f6c\u79fb\u81f3\u94dc\u7f51\u4e0a\u7684\u4e8c\u7ef4Ti, \u4e8c\u7ef4FeCoNiCrNb\uff0c\u4e8c\u7ef4ZrCuAlNi\u7684\u626b\u63cf\u7535\u955c\u56fe\u7247\u3002<\/p>\n<p>e)\u2013 f) \u4e8c\u7ef4Ti, \u4e8c\u7ef4FeCoNiCrNb\uff0c\u4e8c\u7ef4ZrCuAlNi\u7684\u9ad8\u5206\u8fa8\u7387\u900f\u5c04\u7535\u955c\u56fe\u7247\uff0c\u5176\u4e2d\u5185\u7f6e\u56fe\u7247\u4e3a\u5bf9\u5e94\u7684\u5feb\u901f\u5085\u91cc\u53f6\u53d8\u6362\u56fe\u3002<\/p>\n<p>g)\u2013 i) \u8f6c\u79fb\u81f3\u7845\u7247\u8868\u9762\u7684\u4e8c\u7ef4Ti, \u4e8c\u7ef4FeCoNiCrNb\uff0c\u4e8c\u7ef4ZrCuAlNi\u8fb9\u754c\u5904\u539f\u5b50\u529b\u663e\u5fae\u955c\u8868\u9762\u5f62\u8c8c\u56fe\uff0c\u5176\u4e2d\u5185\u7f6e\u66f2\u7ebf\u4e3a\u626b\u8fc7\u4e8c\u7ef4\u91d1\u5c5e\u8fb9\u754c\u7684\u9ad8\u5ea6\u56fe\u3002<\/p>\n<p>\u56fe3. \u5bf9\u8868\u9762\u8936\u76b1\u5f15\u8d77\u8131\u819c\u73b0\u8c61\u7684\u7406\u8bba\u63cf\u8ff0\u548c\u6709\u9650\u5143\u6a21\u62df\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/3-15.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-197585\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/3-15.jpg\" alt=\"\" width=\"700\" height=\"758\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/3-15.jpg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/3-15-277x300.jpg 277w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/a><\/p>\n<p>a)<strong>\u2013 <\/strong>c) \u6c34\u5206\u5b50\u6269\u6563\u8fdb\u5165\u91d1\u5c5e-PVA\u57fa\u5e95\u7cfb\u7edf\u4e2d\u5f15\u8d77\u8868\u9762\u4e0d\u7a33\u5b9a\u6027\u5e76\u4fc3\u4f7f\u8584\u819c\u5265\u79bb\u8fc7\u7a0b\u7684\u793a\u610f\u56fe<\/p>\n<p>d) \u5bf9\u8936\u76b1\u8868\u9762\u7684\u51e0\u4f55\u63cf\u8ff0\uff0c\u5305\u62ec\u8936\u76b1\u7684\u6ce2\u957f<em>l<\/em>\uff0c\u632f\u5e45<em>x<\/em> \u548c\u5728\u8584\u819c-\u57fa\u5e95\u754c\u9762\u5904\u5782\u76f4\u4e8e\u5e73\u9762\u65b9\u5411\u7684\u5e94\u529b<em>s<\/em><em><sub>z<\/sub><\/em>\u3002<\/p>\n<p>e) \u2013 g) <em>l<\/em>\/<em>h<sub>f <\/sub><\/em>\uff0c<em>x<\/em>\/<em>h<sub>f <\/sub><\/em>\u548c<em>s<\/em><em><sub>z<\/sub><\/em>\/<em>E<sub>s<\/sub><\/em> \u4ee5 <em>e<\/em><em><sub>cs<\/sub><\/em> \u4e0e <em>E<sub>f<\/sub><\/em>\/<em>E<sub>s<\/sub><\/em> \u4e3a\u81ea\u53d8\u91cf\u7684\u7b49\u9ad8\u7ebf\u56fe\u3002<\/p>\n<p>h) \u6709\u9650\u5143\u6a21\u62df\u53d7\u7ea6\u675f\u8584\u819c-\u57fa\u5e95\u7cfb\u7edf\u5728\u81a8\u80c0\u8fc7\u7a0b\u4e2d\u7fd8\u66f2\u754c\u9762\u5904\u7684\u88c2\u7f1d\u4ea7\u751f\u8fc7\u7a0b\u3002<\/p>\n<p>i) \u754c\u9762\u88c2\u7f1d\u5728\u6301\u7eed\u7684\u8584\u819c\u62c9\u626f\u8fc7\u7a0b\u4e2d\u751f\u957f\u6269\u5c55\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p>j) \u8868\u9762\u8936\u76b1\u7684\u51e0\u4f55\u5f62\u6001\u5bf9\u88c2\u7f1d\u6269\u5c55\u4e2d\u819c\u5185\u4e34\u754c\u5e94\u529b\u7684\u5f71\u54cd\u3002<\/p>\n<p>k) <em>s<\/em><em><sub>c<\/sub><\/em>\/<em>E<sub>s<\/sub><\/em>\u4ee5<em>E<sub>f<\/sub><\/em>\/<em>E<sub>s<\/sub><\/em>\u4e0e<em>x<\/em>\/<em>l<\/em>\u4e3a\u81ea\u53d8\u91cf\u7684\u7b49\u9ad8\u7ebf\u56fe\u3002<\/p>\n<p>\u56fe4. 2D FeCoNiCrNb\u7531\u7eb3\u7c73\u8584\u819c\u5411\u5fae\u7c73\u5377\u7684\u5f62\u6001\u8f6c\u53d8\u3002<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/4-15.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-197586\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/4-15.jpg\" alt=\"\" width=\"700\" height=\"605\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/4-15.jpg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/4-15-300x259.jpg 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/a><\/p>\n<p>a).\u8584\u819c\u5265\u79bb\u8fc7\u7a0b\u4e2d\u5728<em>e<\/em><em><sub>cs<\/sub><\/em> \u4e0e<em>E<sub>f<\/sub><\/em>\/<em>E<sub>s<\/sub><\/em>\u7684\u63a7\u5236\u4e0b\uff0c\u6700\u7ec8\u5f62\u6001\u7531\u7eb3\u7c73\u8584\u819c\u5411\u5fae\u7c73\u5377\u8f6c\u53d8\u7684\u793a\u610f\u56fe\u3002\u6ce8\u610f\u56fe\u4e2d\u7684\u8272\u5f69\u4ee3\u8868\u754c\u9762\u88c2\u7eb9\u4ea7\u751f\u7684\u96be\u6613\u7a0b\u5ea6\u3002<\/p>\n<p>b).\u8f6c\u79fb\u81f3Si\u4e0a\u7684FeCoNiCrNb\u5fae\u7c73\u5377\u5728\u626b\u63cf\u7535\u955c\u4e0b\u89c2\u5bdf\u5230\u7684\u5f71\u50cf\u3002<\/p>\n<p>c).\u8f6c\u79fb\u5230\u94dc\u7f51\u4e0a\u7684FeCoNiCrNb\u65e0\u57fa\u5e95\u7eb3\u7c73\u8584\u819c\u5728\u626b\u63cf\u7535\u955c\u4e0b\u89c2\u5bdf\u5230\u7684\u5f71\u50cf\u3002<\/p>\n<p>\u56fe5. \u5bf9\u4ea7\u51fa2D\u91d1\u5c5e\u51e0\u4f55\u7684\u8c03\u63a7<\/p>\n<p><a href=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/5-12.jpg\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-197587\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/5-12.jpg\" alt=\"\" width=\"700\" height=\"651\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/5-12.jpg 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/5-12-300x279.jpg 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/a><\/p>\n<p>a)\u6709\u63a9\u6a21\u677f\u53c2\u4e0e\u7684\u8584\u819c\u6c89\u79ef\u8fc7\u7a0b\u793a\u610f\u56fe\u3002<\/p>\n<p>b)\u2013 e)\u63a9\u6a21\u677f\u7684\u5b9e\u62cd\u7167\u7247\uff0c\u5176\u4e2d\u5185\u7f6e\u56fe\u7247\u4e3a\u8f83\u9ad8\u500d\u5149\u5b66\u663e\u5fae\u955c\u56fe\u50cf\u3002<\/p>\n<p>f)- h) \u901a\u8fc7\u63a9\u6a21\u677f\u8584\u819c\u6c89\u79ef\u5236\u5907\u51fa\u7684\u5706\u5f62\uff0c\u65b9\u5f62\u53ca\u516d\u8fb9\u5f62\u4e8c\u7ef4FeCoNiCrNb\u7684\u626b\u63cf\u7535\u955c\u56fe\u7247\u3002<\/p>\n<p><strong>\u56fe\u6587\u94fe\u63a5\uff1a \u00a0<\/strong><a href=\"https:\/\/www.sciencedirect.com\/science\/article\/abs\/pii\/S1369702120300390?via%3Dihub\">https:\/\/www.sciencedirect.com\/science\/article\/abs\/pii\/S1369702120300390?via%3Dihub<\/a><\/p>\n<p><strong>\u8bfe\u9898\u7ec4\u7f51\u7ad9\uff1a <\/strong><\/p>\n<p>http:\/\/www.cityu.edu.hk\/stfprofile\/yonyang.htm<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u8fd1\u5341\u51e0\u5e74\u6765\uff0c\u77f3\u58a8\u70ef\u3001\u4e8c\u786b\u5316\u94bc\u7b49\u4e8c\u7ef4\u6750\u6599\u56e0\u5176\u72ec\u7279\u7684\u7eb3\u7c73\u7ed3\u6784\u53ca\u4f4e\u7ef4\u7279\u6027\u5728\u6750\u6599\u9886\u57df\u5f15\u8d77\u4e86\u5e7f\u6cdb\u5173\u6ce8\u3002\u5b66\u8005\u4eec\u4e0d\u65ad\u63a2\u7d22\u4e8c\u7ef4\u6750\u6599\u6240\u7279\u6709\u7684\u7269\u7406\u548c\u5316\u5b66\u6027\u8d28\uff0c\u5e76\u5f00\u62d3\u4e86\u5176\u5728&#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-197579","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/197579"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=197579"}],"version-history":[{"count":5,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/197579\/revisions"}],"predecessor-version":[{"id":197605,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/197579\/revisions\/197605"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=197579"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=197579"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=197579"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}