{"id":198174,"date":"2020-03-24T06:15:15","date_gmt":"2020-03-23T22:15:15","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=198174"},"modified":"2020-03-23T23:08:35","modified_gmt":"2020-03-23T15:08:35","slug":"%e8%a5%bf%e5%b7%a5%e5%a4%a7%e6%9d%90%e6%96%99%e5%ad%a6%e9%99%a2%e3%80%81%e5%87%9d%e5%9b%ba%e6%8a%80%e6%9c%af%e5%9b%bd%e5%ae%b6%e9%87%8d%e7%82%b9%e5%ae%9e%e9%aa%8c%e5%ae%a4%e6%9d%8e%e6%96%87%e4%ba%9a","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=198174","title":{"rendered":"\u897f\u5de5\u5927\u6750\u6599\u5b66\u9662\u3001\u51dd\u56fa\u6280\u672f\u56fd\u5bb6\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u674e\u6587\u4e9a\u6559\u6388Prog. Mater. Sci. \u7efc\u8ff0\uff1a\u51b7\u55b7\u6d82\u56fa\u6001\u6210\u5f62\u949b\u53ca\u949b\u5408\u91d1"},"content":{"rendered":"<p><strong><b>\u3010<\/b><\/strong><strong><b>\u80cc\u666f\u4ecb\u7ecd<\/b><\/strong><strong><b>\u3011<\/b><\/strong><\/p>\n<p>\u949b\u53ca\u949b\u5408\u91d1\u56e0\u5176\u9ad8\u7684\u6bd4\u5f3a\u5ea6\u3001\u4f18\u826f\u7684\u8010\u8680\u6027\u53ca\u751f\u7269\u76f8\u5bb9\u6027\uff0c\u5e7f\u6cdb\u5e94\u7528\u4e8e\u822a\u7a7a\u3001\u822a\u5929\u3001\u5316\u5de5\u3001\u533b\u5b66\u7b49\u9886\u57df\u3002\u7136\u800c\u56e0\u949b\u53ca\u949b\u5408\u91d1\u7684\u6d3b\u6027\u9ad8\uff0c\u6613\u6c27\u5316\uff0c\u4f20\u7edf\u7684\u5236\u5907\u5de5\u827a\uff08\u94f8\u9020\u3001\u7535\u5b50\u675f\u710a\u63a5\u548c\u771f\u7a7a\u7b49\u79bb\u5b50\u55b7\u6d82\u7b49\uff09\u987b\u5728\u771f\u7a7a\u6216\u8005\u60f0\u6027\u6c14\u4f53\u7684\u4fdd\u62a4\u4e0b\uff0c\u65e0\u7591\u589e\u52a0\u4e86\u5236\u9020\u6210\u672c\u3002\u8fd1\u51e0\u5e74\uff0c\u589e\u6750\u5236\u9020\u6280\u672f\u53d6\u5f97\u4e86\u5de8\u5927\u8fdb\u5c55\uff0c\u5728\u4f20\u7edf\u589e\u6750\u5236\u9020\uff08\u6fc0\u5149\u589e\u6750\u3001\u7535\u5b50\u675f\u589e\u6750\u548c\u7535\u5f27\u589e\u6750\uff09\u8fc7\u7a0b\u4e2d\uff0c\u7c89\u672b\u6216\u8005\u4e1d\u6750\u7ecf\u5386\u7194\u5316-\u51dd\u56fa\u8fc7\u7a0b\uff0c\u8fd1\u51c0\u6210\u5f62\u96f6\u90e8\u4ef6\uff0c\u4e3a\u949b\u53ca\u949b\u5408\u91d1\u7684\u6210\u5f62\u5236\u9020\u5f00\u8f9f\u4e86\u4e00\u4e2a\u65b0\u65b9\u5411\u3002\u7136\u800c\u9ad8\u6e29\u7684\u5de5\u827a\u8fc7\u7a0b\u4ecd\u5e26\u6765\u51b6\u91d1\u7f3a\u9677\uff0c\u6bd4\u5982\u5fae\u88c2\u7eb9\u3001\u6b8b\u4f59\u5e94\u529b\u548c\u53d8\u5f62\u7b49\u3002<\/p>\n<p>\u51b7\u55b7\u6d82\uff08Cold Spraying\uff0cCS\uff09\uff0c\u662f\u4e00\u79cd\u57fa\u4e8e\u5fae\u7c73\u7ea7\u9897\u7c92\u9ad8\u901f\u56fa\u6001\u78b0\u649e\u800c\u7ed3\u5408\u7684\u6210\u5f62\u6280\u672f\uff08\u7ed3\u5408\u673a\u7406\u4e0e\u7206\u70b8\u710a\u63a5\u7c7b\u4f3c\uff0c\u4e5f\u53ef\u79f0\u4f5c\u5fae\u578b\u56fa\u76f8\u710a\u63a5\uff09\uff0c\u81ea20\u4e16\u7eaa80\u5e74\u4ee3\u4e2d\u671f\u53d1\u73b0\u4ee5\u6765\uff0c\u53d7\u5230\u56fd\u5185\u5916\u5b66\u8005\u7684\u5e7f\u6cdb\u5173\u6ce8\u3002\u5176\u5de5\u4f5c\u539f\u7406\u662f\u5c06\u9ad8\u538b\u6c14\u4f53\uff08He\u3001N<sub>2<\/sub>\u3001\u7a7a\u6c14\u6216\u5b83\u4eec\u7684\u6df7\u5408\u6c14\u4f53\uff09\u5bfc\u5165\u7279\u6b8a\u8bbe\u8ba1\u7684\u62c9\u74e6\u5c14\uff08Laval\uff09\u55b7\u5634\uff0c\u5229\u7528\u9ad8\u538b\u6c14\u4f53\u5728\u8f83\u4f4e\u7684\u6e29\u5ea6\u4e0b\uff08\u4f4e\u4e8e\u55b7\u6d82\u6750\u6599\u7684\u7194\u70b9\uff09\u52a0\u901f\u5fae\u7c73\u5c3a\u5ea6\u7684\u9897\u7c92\uff0c\u4f7f\u5176\u5728\u56fa\u6001\u4e0b\u4ee5\u8f83\u9ad8\u7684\u901f\u5ea6\u649e\u51fb\u57fa\u4f53\uff0c\u901a\u8fc7\u9897\u7c92\/\u57fa\u4f53\u53d1\u751f\u5267\u70c8\u7684\u5851\u6027\u53d8\u5f62\u800c\u6c89\u79ef\u4e8e\u57fa\u4f53\u8868\u9762\u5f62\u6210\u6d82\u5c42\u3002\u8fc4\u4eca\u4e3a\u6b62\uff0c\u51b7\u55b7\u6d82\u6280\u672f\u80fd\u591f\u7528\u6765\u5236\u5907\u5927\u90e8\u5206\u91d1\u5c5e\u53ca\u5176\u5408\u91d1\uff08Al\u3001Cu\u3001Ag\u3001Mg\u3001Sn\u3001Zn\u3001Ti\u3001Ni\u3001Fe\u3001Ta\u3001\u4e0d\u9508\u94a2\u3001Ti<sub>6<\/sub>Al4V\u3001\u9ad8\u6e29\u5408\u91d1\u3001\u9ad8\u71b5\u5408\u91d1\u7b49\uff09\uff1b\u91d1\u5c5e-\u91d1\u5c5e\u590d\u5408\u6750\u6599\uff08Al-Cu\u3001Al-Ti\u3001Al-Ni\u3001W-Cu\u7b49\uff09\u3001\u91d1\u5c5e-\u9676\u74f7\u590d\u5408\u6750\u6599\uff08Al-Al<sub>2<\/sub>O<sub>3<\/sub>\u3001Al-SiC\u3001Al-TiN\u3001Ti-SiC\u7b49\uff09\uff1b\u751a\u81f3\u975e\u6676\uff08NiTiZrSiSn\u3001Al\u57fa\u3001Fe\u57fa\u7b49\uff09\u3001\u7eb3\u7c73\u7ed3\u6784\u91d1\u5c5e\u6750\u6599\uff08nano-Al\u3001Ni\u3001Cu\u7b49\uff09\u3002\u8fd1\u5e74\u6765\uff0c\u51b7\u55b7\u6d82\u4ece\u6d82\u5c42\u5236\u5907\u6269\u5c55\u5230\u6210\u5f62\u5236\u9020\u4e0e\u4fee\u590d\u518d\u5236\u9020\u9886\u57df\uff0c\u5373\u51b7\u55b7\u6d82\u56fa\u6001\u589e\u6750\u5236\u9020\u6280\u672f\u3002\u4f5c\u4e3a\u589e\u6750\u5236\u9020\u5bb6\u65cf\u7684\u65b0\u6210\u5458\uff0c\u51b7\u55b7\u6d82\u5728\u5236\u9020\u4e1a\u4e2d\u8868\u73b0\u51fa\u4e86\u5de8\u5927\u7684\u6f5c\u529b\uff0c\u5f15\u8d77\u4e86\u5168\u4e16\u754c\u91cd\u8981\u5de5\u4e1a\u9886\u57df\u7684\u5173\u6ce8\u3002<\/p>\n<p>\u4f5c\u4e3a\u4ee3\u8868\u6027\u6750\u6599\u4e4b\u4e00\uff0c\u949b\u53ca\u949b\u5408\u91d1\u7684\u9ad8\u8d28\u91cf\u51b7\u55b7\u6d82\u6210\u5f62\u9762\u4e34\u5de8\u5927\u6311\u6218\uff0c\u5907\u53d7\u56fd\u9645\u540c\u884c\u5173\u6ce8\u3002\u672c\u6587\u9996\u5148\u7cfb\u7edf\u5730\u63a2\u8ba8\u4e86\u51b7\u55b7\u6d82\u949b\u53ca\u949b\u5408\u91d1\u6c89\u79ef\u4f53\u7684\u6c89\u79ef\u7279\u6027\u53ca\u5176\u5de5\u827a\u5f71\u54cd\u56e0\u7d20\u3002\u9897\u7c92\u662f\u5982\u4f55\u6c89\u79ef\u7684\uff1f\u6c89\u79ef\u4f53\u7684\u7ec4\u7ec7\u548c\u6027\u80fd\u5982\u4f55\uff1f\u5de5\u827a\u53c2\u6570-\u7ec4\u7ec7-\u6027\u80fd\u76f8\u5173\u6027\uff1f\u5176\u6b21\uff0c\u73b0\u6709\u7814\u7a76\u8868\u660e\u949b\u53ca\u949b\u5408\u91d1\u7684\u7ed3\u5408\u673a\u7406\u4e0e\u94dc\u3001\u94dd\u7b49\u5b58\u5728\u5f88\u5927\u5dee\u522b\uff0c\u56e0\u6b64\u7406\u89e3\u949b\u53ca\u949b\u5408\u91d1\u7684\u7ed3\u5408\u673a\u7406\u53d8\u5f97\u5c24\u5176\u91cd\u8981\u3002\u6700\u540e\uff0c\u949b\u53ca\u949b\u5408\u91d1\u6c89\u79ef\u4f53\u7684\u529b\u5b66\u6027\u80fd\u4e9f\u9700\u63d0\u9ad8\uff0c\u5982\u4f55\u6709\u6548\u5730\u63d0\u5347\u5176\u529b\u5b66\u6027\u80fd\u662f\u53e6\u4e00\u4e2a\u91cd\u8981\u96be\u9898\u3002\u76ee\u524d\uff0c\u901a\u8fc7\u4e0e\u5176\u4ed6\u52a0\u5de5\u6280\u672f\u590d\u5408\u6765\u6539\u5584\u949b\u53ca\u949b\u5408\u91d1\u6c89\u79ef\u4f53\u7684\u529b\u5b66\u6027\u80fd\uff0c\u79f0\u4e4b\u4e3a\u201c\u51b7\u55b7\u6d82\u590d\u5408\u6280\u672f\u201d\u3002<\/p>\n<p>\u60f3\u6df1\u5165\u4e86\u89e3\u51b7\u55b7\u6d82\u6280\u672f\uff0c\u7279\u522b\u662f\u51b7\u55b7\u6d82\u949b\u5408\u91d1\u6c89\u79ef\u4f53\u7684\u7ec4\u7ec7\u548c\u6027\u80fd\u7279\u6027\u4ee5\u53ca\u5f3a\u5851\u5316\u63d0\u9ad8\u6280\u672f\u7684\u79d1\u7814\u8fbe\u4eba\uff0c\u8fd8\u5728\u7b49\u4ec0\u4e48\u5462\uff1f<\/p>\n<p>\u8be5\u6210\u679c\u53d7\u5230<strong><b>\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1(51875471)<\/b><\/strong>\u7684\u8d44\u52a9\uff0c\u4ee5\u53ca<strong><b>\u51dd\u56fa\u6280\u672f\u56fd\u5bb6\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u81ea\u4e3b\u8bfe\u9898(2019-QZ-01)<\/b><\/strong>\u7684\u5927\u529b\u652f\u6301\u3002<\/p>\n<p><strong><b>\u3010<\/b><\/strong><strong><b>\u6210\u679c\u7b80\u4ecb<\/b><\/strong><strong><b>\u3011<\/b><\/strong><\/p>\n<p>\u897f\u5317\u5de5\u4e1a\u5927\u5b66\u51dd\u56fa\u6280\u672f\u56fd\u5bb6\u91cd\u70b9\u5b9e\u9a8c\u5ba4\u674e\u6587\u4e9a\u6559\u6388\uff08\u7b2c\u4e00\u4f5c\u8005\u548c\u901a\u8baf\u4f5c\u8005\uff09\u3001\u66f9\u806a\u806a\u5728\u8bfb\u535a\u58eb\u548c\u7231\u5c14\u5170\u90fd\u67cf\u6797\u5927\u5b66\u7684\u6bb7\u7855\u52a9\u7406\u6559\u6388\uff0c\u5728<strong><b>\u6750\u6599\u79d1\u5b66\u9876\u7ea7\u671f\u520a\u300aProgress in Materials Science\u300b\uff08\u5f71\u54cd\u56e0\u5b50IF2018 = 23.725\uff0c5\u5e74\u5f71\u54cd\u56e0\u5b50IF = 33.01<\/b><\/strong>\uff09\u4e0a\u53d1\u8868\u9898\u4e3a\u201cSolid-state cold spraying of Ti and its alloys: a literature review\u201d\u7684\u957f\u7bc7\u7efc\u8ff0\uff0c\u4ee5\u4f5c\u8005\u591a\u5e74\u7684\u7814\u7a76\u6210\u679c\u4e3a\u4e3b\u7ebf\uff0c\u6df1\u5165\u63a2\u8ba8\u4e86\u51b7\u55b7\u6d82\u949b\u53ca\u949b\u5408\u91d1\u6c89\u79ef\u4f53\u7684\u5f71\u54cd\u56e0\u7d20\u548c\u7ed3\u5408\u673a\u5236\uff0c\u5e76\u603b\u7ed3\u4e86\u51b7\u55b7\u6d82\u4e0e\u5176\u4ed6\u52a0\u5de5\u5de5\u827a\u7684\u590d\u5408\u6280\u672f\uff0c\u65e8\u5728\u63d0\u5347\u6c89\u79ef\u4f53\u5f3a\u5851\u6027\uff0c\u968f\u540e\u603b\u7ed3\u4e86\u6c89\u79ef\u4f53\u7684\u5e94\u7528\uff0c\u6700\u540e\u5bf9\u6c89\u79ef\u4f53\u7684\u7ed3\u5408\u673a\u5236\u5b8c\u5584\u3001\u5f3a\u5851\u6027\u7684\u63d0\u5347\u3001\u5728\u589e\u6750\u5236\u9020\u548c\u4fee\u590d\u518d\u5236\u9020\u9886\u57df\u7684\u5e94\u7528\u7b49\u63d0\u51fa\u4e86\u5c55\u671b\u3002\u7efc\u8ff0\u5168\u65872\u4e075\u5343\u4f59\u5b57\uff0c\u5206\u4e3a7\u4e2a\u5927\u7ae0\u8282\uff0c\u5171\u542b9\u4e2a\u91cd\u8981\u8868\u683c\u548c87\u5f20\u91cd\u8981\u56fe\u7247\uff0c\u5f15\u7528\u4e86160\u4f59\u7bc7\u53c2\u8003\u6587\u732e\uff0c\u5185\u5bb9\u6db5\u76d6\u4e86\u51b7\u55b7\u6d82\u53d1\u73b0\u81f3\u4eca30\u591a\u5e74\u6765\u51e0\u4e4e\u6240\u6709\u5173\u4e8e\u51b7\u55b7\u6d82\u949b\u53ca\u949b\u5408\u91d1\u7684\u7814\u7a76\u6210\u679c\u3002<\/p>\n<p><strong><b>\u3010<\/b><\/strong><strong><b>\u56fe\u6587\u5bfc\u8bfb<\/b><\/strong><strong><b>\u3011<\/b><\/strong><\/p>\n<p>\u56fe1 \u51b7\u55b7\u6d82\u539f\u7406\u793a\u610f\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198175 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72471-15.png\" alt=\"\" width=\"700\" height=\"350\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72471-15.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72471-15-300x150.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe2 \u5178\u578b\u51b7\u55b7\u6d82Ti\u53caTi<sub>6<\/sub>Al4V\u6a2a\u622a\u9762\u7ec4\u7ec7<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198176 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72472-13.png\" alt=\"\" width=\"606\" height=\"459\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72472-13.png 606w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72472-13-300x227.png 300w\" sizes=\"(max-width: 606px) 100vw, 606px\" \/><\/p>\n<p>(a)\u548c(c)\u4e3a\u51b7\u55b7\u6d82Ti\u6c89\u79ef\u4f53\uff0c(b)\u548c(d)\u4e3a\u51b7\u55b7\u6d82Ti<sub>6<\/sub>Al4V\u6c89\u79ef\u4f53<\/p>\n<p>\u56fe3 Ti\u7c92\u5b50\u649e\u51fb\u901f\u5ea6\u3001\u6c89\u79ef\u4f53\u5b54\u9699\u7387\u548c\u663e\u5fae\u786c\u5ea6\u7684\u5173\u7cfb<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-198677\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/hehe.png\" alt=\"\" width=\"562\" height=\"428\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/hehe.png 562w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/hehe-300x228.png 300w\" sizes=\"(max-width: 562px) 100vw, 562px\" \/><\/p>\n<p>(a)\u4e3aTi\u7c92\u5b50\u649e\u51fb\u901f\u5ea6\u548c\u6c89\u79ef\u4f53\u5b54\u9699\u7387\u7684\u5173\u7cfb\uff0c(b)\u4e3aTi\u7c92\u5b50\u649e\u51fb\u901f\u5ea6\u548c\u6c89\u79ef\u4f53\u663e\u5fae\u786c\u5ea6\u7684\u5173\u7cfb\uff0c(c)\u4e3aTi\u6c89\u79ef\u4f53\u5b54\u9699\u7387\u548c\u663e\u5fae\u786c\u5ea6\u7684\u5173\u7cfb<\/p>\n<p>\u56fe4 \u51b7\u55b7\u6d82Ti\u53caTi<sub>6<\/sub>Al4V\u589e\u6750\u5236\u9020\u7684\u4e3b\u8981\u5de5\u827a\u53c2\u6570<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198178 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72474-12.png\" alt=\"\" width=\"700\" height=\"343\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72474-12.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72474-12-300x147.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe5 Ti\u7c92\u5b50\u649e\u51fb\u901f\u5ea6\u4e0e\u6c89\u79ef\u6548\u7387\u7684\u5173\u7cfb<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198179 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72475-11.png\" alt=\"\" width=\"572\" height=\"424\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72475-11.png 572w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72475-11-300x222.png 300w\" sizes=\"(max-width: 572px) 100vw, 572px\" \/><\/p>\n<p>\u56fe6 Ti<sub>6<\/sub>A<sub>l<\/sub>4V\u7c92\u5b50\u649e\u51fb\u5230Ti\u57fa\u677f\u4e0a\u5265\u79bb\u540e\u7684\u5fae\u89c2\u5f62\u8c8c<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198180 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72476-11.png\" alt=\"\" width=\"700\" height=\"250\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72476-11.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72476-11-300x107.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe7 Ti\u53caTi<sub>6<\/sub>Al4V\u6c89\u79ef\u4f53\u4e0e\u57fa\u677f\u7684\u7ed3\u5408\u5f3a\u5ea6\u548c\u5b54\u9699\u7387<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198181 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72477-11.png\" alt=\"\" width=\"680\" height=\"457\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72477-11.png 680w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72477-11-300x202.png 300w\" sizes=\"(max-width: 680px) 100vw, 680px\" \/><\/p>\n<p>\u56fe8 Ti\u53caTi<sub>6<\/sub>Al4V\u6c89\u79ef\u4f53\u5185\u805a\u5f3a\u5ea6\uff08\u81ea\u8eab\u5f3a\u5ea6\uff09\u548c\u5b54\u9699\u7387<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198182 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72478-10.png\" alt=\"\" width=\"618\" height=\"447\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72478-10.png 618w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72478-10-300x217.png 300w\" sizes=\"(max-width: 618px) 100vw, 618px\" \/><\/p>\n<p>\u56fe9 \u540e\u70ed\u5904\u7406\u6539\u5584\u51b7\u55b7\u6d82Ti<sub>6<\/sub>Al4V\u6c89\u79ef\u4f53\u5185\u805a\u5f3a\u5ea6<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198183 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72479-8.png\" alt=\"\" width=\"646\" height=\"464\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72479-8.png 646w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u72479-8-300x215.png 300w\" sizes=\"(max-width: 646px) 100vw, 646px\" \/><\/p>\n<p>\u56fe10 \u539f\u4f4d\u55b7\u4e38\u8f85\u52a9\u51b7\u55b7\u6d82\u81f4\u5bc6\u5316\u6d82\u5c42\u539f\u7406\u793a\u610f\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198184 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724710-8.png\" alt=\"\" width=\"700\" height=\"636\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724710-8.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724710-8-300x273.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe11 \u6fc0\u5149\u8f85\u52a9\u51b7\u55b7\u6d82\u70ed\u8fc7\u7a0b\u793a\u610f\u56fe<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198185 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724711-4.png\" alt=\"\" width=\"661\" height=\"413\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724711-4.png 661w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724711-4-300x187.png 300w\" sizes=\"(max-width: 661px) 100vw, 661px\" \/><\/p>\n<p>\u56fe12 \u51b7\u55b7\u6d82Ti\u6c89\u79ef\u4f53\u7ecf\u8fc7\u70ed\u8f67\u5904\u7406\u540eOM\u5fae\u89c2\u7ec4\u7ec7<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198186 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724712-2.png\" alt=\"\" width=\"623\" height=\"470\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724712-2.png 623w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724712-2-300x226.png 300w\" sizes=\"(max-width: 623px) 100vw, 623px\" \/><\/p>\n<p>\u56fe13 \u51b7\u55b7\u6d82Ti<sub>6<\/sub>Al4V\u6c89\u79ef\u4f53\u7ecf\u8fc7\u70ed\u7b49\u9759\u538b\u5904\u7406\u540e\u5de5\u7a0b\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198187 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724713-1.png\" alt=\"\" width=\"700\" height=\"252\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724713-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724713-1-300x108.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p>\u56fe14 \u51b7\u55b7\u6d82Ti<sub>6<\/sub>Al4V\u6c89\u79ef\u4f53\u7ecf\u8fc7\u6405\u62cc\u6469\u64e6\u52a0\u5de5\u5904\u7406\u540e\u7684\u5fae\u89c2\u7ec4\u7ec7<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-198188 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724714-1.png\" alt=\"\" width=\"700\" height=\"442\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724714-1.png 700w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/03\/\u56fe\u724714-1-300x189.png 300w\" sizes=\"(max-width: 700px) 100vw, 700px\" \/><\/p>\n<p><strong><b>\u8bba\u6587\u5df2\u5728\u7ebf\u53d1\u8868<\/b><\/strong><strong><b>\uff1a<\/b><\/strong><\/p>\n<p><strong><b>https:\/\/doi.org\/10.1016\/j.pmatsci.2019.100633\/<\/b><\/strong><\/p>\n<p><strong><b>\u539f\u6587\u94fe\u63a5\u5982\u4e0b\uff1a<\/b><\/strong><\/p>\n<p><strong><b>https:\/\/www.sciencedirect.com\/science\/article\/pii\/S007964251930115X<\/b><\/strong><\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011 \u949b\u53ca\u949b\u5408\u91d1\u56e0\u5176\u9ad8\u7684\u6bd4\u5f3a\u5ea6\u3001\u4f18\u826f\u7684\u8010\u8680\u6027\u53ca\u751f\u7269\u76f8\u5bb9\u6027\uff0c\u5e7f\u6cdb\u5e94\u7528\u4e8e\u822a\u7a7a\u3001\u822a\u5929\u3001\u5316\u5de5\u3001\u533b\u5b66\u7b49\u9886\u57df\u3002\u7136\u800c\u56e0\u949b\u53ca\u949b\u5408\u91d1\u7684\u6d3b\u6027\u9ad8\uff0c\u6613\u6c27\u5316\uff0c\u4f20\u7edf\u7684\u5236\u5907\u5de5\u827a\uff08\u94f8\u9020&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":198175,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-198174","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/198174"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=198174"}],"version-history":[{"count":9,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/198174\/revisions"}],"predecessor-version":[{"id":198702,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/198174\/revisions\/198702"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/198175"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=198174"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=198174"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=198174"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}