{"id":201470,"date":"2020-07-06T06:56:45","date_gmt":"2020-07-05T22:56:45","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=201470"},"modified":"2020-07-05T20:45:09","modified_gmt":"2020-07-05T12:45:09","slug":"%e5%85%89%e8%87%b4%e5%8f%91%e5%85%89%e6%9d%90%e6%96%99-%e9%bb%84%e7%bb%b4%e9%99%a2%e5%a3%ab%e3%80%81chihaya-adachi%e3%80%81%e6%9d%a8%e6%9c%9d%e9%be%99%ef%bc%8c%e6%bd%98%e6%a2%85%e8%af%be%e9%a2%98","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=201470","title":{"rendered":"\u5149\u81f4\u53d1\u5149\u6750\u6599&#8211;\u9ec4\u7ef4\u9662\u58eb\u3001Chihaya Adachi\u3001\u6768\u671d\u9f99\uff0c\u6f58\u6885\u8bfe\u9898\u7ec4\u6210\u679c\u901f\u9012"},"content":{"rendered":"<p style=\"text-align: center;\"><strong><b>\u9ec4\u7ef4\u9662\u58eb\u8bfe\u9898\u7ec4<\/b><\/strong><\/p>\n<p><strong><b>\u4e9a\u5355\u5143\u4e92\u9501\u5b9e\u73b0\u805a\u5408\u7269\u4e2d\u957f\u5bff\u547d\u7684\u6709\u673a\u5ba4\u6e29\u78f7\u5149\u7684\u7814\u7a76<\/b><\/strong><\/p>\n<p>\u957f\u5bff\u547d\u7684\u5ba4\u6e29\u78f7\u5149\uff08LRTP\uff09\u662f\u4e00\u79cd\u5728\u6709\u673a\u7535\u5b50\u548c\u5149\u5b50\u5b66\u4e2d\u5f15\u4eba\u6ce8\u76ee\u7684\u5149\u5b66\u73b0\u8c61\u3002\u5c3d\u7ba1\u8fd1\u4e9b\u5e74\u6765\u53d1\u5c55\u5341\u5206\u8fc5\u901f\uff0c\u4f46\u5728\u65e0\u5b9a\u5f62\u805a\u5408\u7269\u4e2d\u83b7\u5f97LRTP\u7684\u901a\u7528\u65b9\u6cd5\u4ecd\u5b58\u5728\u6311\u6218\u3002\u9488\u5bf9\u6b64\u95ee\u9898\uff0c\u897f\u5317\u5de5\u4e1a\u5927\u5b66\u9ec4\u7ef4\u9662\u58eb\u8bfe\u9898\u7ec4\u57fa\u4e8e\u4f20\u7edf\u7684\u805a\u4e59\u70ef\u884d\u751f\u7269\uff0c\u63d0\u51fa\u4e86\u4e00\u79cd\u901a\u8fc7\u79bb\u5b50\u952e\u4ea4\u8054\u805a\u5408\u7269\u7684\u5316\u5b66\u7b56\u7565\u6765\u5b9e\u73b0\u8d85\u957f\u78f7\u5149\u7684\u65b9\u6cd5\u3002\u5728\u81ea\u7136\u73af\u5883\u6761\u4ef6\u4e0b\uff0c\u65e0\u5b9a\u5f62\u805a\u5408\u7269\u7684LRTP\u5bff\u547d\u8fbe\u5230\u521b\u7eaa\u5f55\u76842.1 s\u3002\u6b64\u5916\uff0c\u8fd8\u53d1\u73b0\u53ef\u4ee5\u901a\u8fc7\u8c03\u8282\u5355\u7ec4\u5206\u805a\u5408\u7269\u6750\u6599\u4e2d\u7684\u6fc0\u53d1\u6ce2\u957f\u6765\u83b7\u5f97\u591a\u8272\u957f\u5bff\u547d\u78f7\u5149\u53d1\u5c04\u3002\u8fd9\u4e9b\u7ed3\u679c\u6982\u8ff0\u4e86\u6784\u9020\u5e26\u6709LRTP\u805a\u5408\u7269\u6750\u6599\u7684\u57fa\u672c\u539f\u7406\uff0c\u8d4b\u4e88\u4f20\u7edf\u805a\u5408\u7269\u65b0\u7684\u7279\u5f81\u3002<sup>[1<\/sup><sup>]<\/sup>\u76f8\u5173\u7814\u7a76\u4ee5\u201cEnabling long-lived organic room temperature phosphorescence in polymers by subunit interlocking\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728Nature Communications\u3002<\/p>\n<p><strong><b>\u56fe1<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>PAANa\uff0cPMANa\u548cPMANa-co-PSSNa\u805a\u5408\u7269\u7684\u5149\u5316\u5b66\u7269\u7406\u6027\u8d28\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-201471 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72471-13.png\" alt=\"\" width=\"749\" height=\"446\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72471-13.png 749w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72471-13-300x179.png 300w\" sizes=\"(max-width: 749px) 100vw, 749px\" \/><\/p>\n<p><strong><b>\u989c\u8272\u53ef\u8c03\u8d85\u957f\u6709\u673a\u78f7\u5149\u7684\u5355\u7ec4\u5206\u5206\u5b50\u6676\u4f53\u7684\u7814\u7a76<\/b><\/strong><\/p>\n<p>\u5177\u6709\u8d85\u957f\u5bff\u547d\u7684LED\u53d1\u5149\u6750\u6599\u5728\u663e\u793a\uff0c\u4fe1\u606f\u52a0\u5bc6\u548c\u751f\u7269\u6210\u50cf\u9886\u57df\u5177\u6709\u5f88\u5927\u7684\u5e94\u7528\u4ef7\u503c\u3002\u56e0\u6b64\uff0c\u897f\u5317\u5de5\u4e1a\u5927\u5b66\u9ec4\u7ef4\u9662\u58eb\u8bfe\u9898\u7ec4\u5236\u5907\u51fa\u51e0\u79cd\u63d0\u4f9b\u989c\u8272\u53ef\u8c03\uff0c\u8d85\u957f\u6709\u673a\u78f7\u5149\uff08UOP\uff09\u7684\u6709\u673a\u78f7\u5149\u4f53\u6750\u6599\u3002\u8fd9\u4e9b\u6750\u6599\u53ef\u4ee5\u901a\u8fc7\u6539\u53d8\u6fc0\u53d1\u6ce2\u957f\u6765\u5b9e\u73b0\u4ece\u7d2b\u8272\u5230\u7eff\u8272\u6240\u6709\u53ef\u89c1\u5149\u8c31\u4e2d\u53d1\u5c04\u989c\u8272\u7684\u53d8\u5316\u3002\u7ed3\u679c\u8868\u660e\uff1a\u8fd9\u4e9b\u6709\u673a\u78f7\u5149\u4f53\u5177\u67092.45\u00b5s\u7684\u8d85\u957f\u5bff\u547d\u548c31.2\uff05\u7684\u6700\u5927\u78f7\u5149\u6548\u7387\u3002\u8fd9\u4e9b\u6750\u6599\u5728\u5728\u591a\u8272\u663e\u793a\u5668\u548c300\u81f3360 nm\u8303\u56f4\u5185\u7684\u7d2b\u5916\u7ebf\u53ef\u89c6\u68c0\u6d4b\u4e2d\u663e\u793a\u51fa\u826f\u597d\u7684\u5e94\u7528\u6548\u679c\uff0c\u4e3a\u5f00\u53d1\u5177\u6709\u52a8\u6001\u63a7\u5236\u78f7\u5149\u7684\u667a\u80fd\u53d1\u5149\u6750\u6599\u548c\u4f20\u611f\u5668\u63d0\u4f9b\u4e86\u673a\u4f1a\u3002<sup>[2<\/sup><sup>]<\/sup>\u76f8\u5173\u7814\u7a76\u4ee5\u201cColour-tunable ultra-long organic phosphorescence of a single-component molecular crystal\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728nature photonics\u3002<\/p>\n<p><strong><b>\u56fe2<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u5355\u7ec4\u5206\u6676\u4f53\u4e2d\u989c\u8272\u53ef\u8c03\u7684<\/b><\/strong><strong><b>UOP<\/b><\/strong><strong><b>\u7684\u673a\u7406\u7814\u7a76\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-201472 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72472-12.png\" alt=\"\" width=\"663\" height=\"429\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72472-12.png 663w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72472-12-300x194.png 300w\" sizes=\"(max-width: 663px) 100vw, 663px\" \/><\/p>\n<p><strong><b>\u9ad8\u6027\u80fd\u9499\u949b\u77ff\u53d1\u5149\u4e8c\u6781\u7ba1\u7684\u5206\u5b50\u949d\u5316\u7814\u7a76<\/b><\/strong><\/p>\n<p>\u9677\u9631\u4ecb\u5bfc\u7684\u975e\u8f90\u5c04\u635f\u8017\u662f\u9650\u5236\u6eb6\u6db2\u5904\u7406\u7684\u9499\u949b\u77ff\u5149\u7535\u5668\u4ef6\uff08\u4f8b\u5982\u53d1\u5149\u4e8c\u6781\u7ba1\uff09\u53d1\u5149\u6548\u7387\u7684\u4e3b\u8981\u56e0\u7d20\u3002\u901a\u5e38\u6765\u8bf4\uff0c\u4f7f\u7528\u6709\u673a\u5206\u5b50\u7684\u7f3a\u9677\u949d\u5316\u88ab\u8ba4\u4e3a\u662f\u89e3\u51b3\u8be5\u95ee\u9898\u7684\u6700\u6709\u5438\u5f15\u529b\u7684\u65b9\u6cd5\u3002\u7136\u800c\uff0c\u7531\u4e8e\u7f3a\u4e4f\u5bf9\u5206\u5b50\u7ed3\u6784\u5982\u4f55\u5f71\u54cd\u949d\u5316\u6548\u679c\u7684\u6df1\u5165\u4e86\u89e3\uff0c\u5f71\u54cd\u4e86\u8be5\u65b9\u6cd5\u7684\u5b9e\u65bd\u3002\u897f\u5317\u5de5\u4e1a\u5927\u5b66\u9ec4\u7ef4\u9662\u58eb\u8bfe\u9898\u7ec4\u8bc1\u660e\u4e86\u957f\u4e45\u4ee5\u6765\u88ab\u5ffd\u7565\u7684\u6c22\u952e\u5728\u5f71\u54cd\u949d\u5316\u6548\u679c\u4e2d\u8d77\u7740\u5173\u952e\u4f5c\u7528\u3002\u5176\u901a\u8fc7\u524a\u5f31\u949d\u5316\u529f\u80fd\u90e8\u5206\u548c\u9499\u949b\u77ff\u4e2d\u6709\u673a\u9633\u79bb\u5b50\u4e4b\u95f4\u7684\u6c22\u952e\uff0c\u663e\u7740\u589e\u5f3a\u4e86\u4e0e\u7f3a\u9677\u4f4d\u70b9\u7684\u76f8\u4e92\u4f5c\u7528\uff0c\u5e76\u6700\u5927\u7a0b\u5ea6\u5730\u51cf\u5c11\u4e86\u975e\u8f90\u5c04\u91cd\u7ec4\u635f\u5931\u3002\u56e0\u6b64\u5236\u5907\u51fa\u5177\u670921.6\uff05\u7684\u8d85\u9ad8\u5916\u90e8\u91cf\u5b50\u6548\u7387\u7684\u8fd1\u7ea2\u5916\u9499\u949b\u77ff\u53d1\u5149\u4e8c\u6781\u7ba1\u3002\u800c\u4e14\uff0c\u6240\u5236\u5907\u51fa\u7684\u949d\u5316\u9499\u949b\u77ff\u53d1\u5149\u4e8c\u6781\u7ba1\u5728200 mA cm<sup>\u2212<\/sup><sup>2<\/sup>\u7684\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\u4fdd\u630120.1\uff05\u7684\u9ad8\u5916\u90e8\u91cf\u5b50\u6548\u7387\u548c11.0\uff05\u7684\u7535\u5149\u8f6c\u5316\u6548\u7387\u3002<sup>[3<\/sup><sup>]<\/sup>\u76f8\u5173\u7814\u7a76\u4ee5\u201cRational molecular passivation for high-performance perovskite light-emitting diodes\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728nature photonics\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>3<\/b><\/strong><strong><b>\u6c22\u952e\u949d\u5316\u5bf9EL\u6027\u80fd\u5f71\u54cd\u6d4b\u8bd5\u56fe<\/b><\/strong><\/p>\n<p>&nbsp;<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-201473 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72473-12.png\" alt=\"\" width=\"894\" height=\"414\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72473-12.png 894w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72473-12-300x139.png 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72473-12-768x356.png 768w\" sizes=\"(max-width: 894px) 100vw, 894px\" \/><\/p>\n<p style=\"text-align: center;\"><strong><b>Chihaya Adachi<\/b><\/strong><strong><b>\u8bfe\u9898\u7ec4<\/b><\/strong><\/p>\n<p><strong><b>\u7535\u8377\u8f6c\u79fb\u4e0e\u5c40\u90e8\u6fc0\u53d1\u6001\u4e4b\u95f4\u7684\u80fd\u9699\u5bf9\u6709\u673a\u957f\u4f59\u8f89\u53d1\u5149\u5f71\u54cd\u7684\u7814\u7a76<\/b><\/strong><\/p>\n<p>\u6709\u673a\u957f\u4f59\u8f89\u53d1\u5149\u6750\u6599\uff08LPL\uff09\u662f\u4e00\u79cd\u53ef\u5c06\u5b58\u50a8\u7684\u6fc0\u5b50\u80fd\u91cf\u7f13\u6162\u91ca\u653e\u4e3a\u5149\u7684\u6709\u673a\u53d1\u5149\u7cfb\u7edf\u3002\u76f8\u6bd4\u8f83\u4e8e\u4f20\u7edf\u7684\u65e0\u673a\u957f\u4f59\u8f89\u53d1\u5149\u6750\u6599\uff0c\u6709\u673a\u957f\u4f59\u8f89\u53d1\u5149\u6750\u6599\u5728\u529f\u80fd\u6027\uff0c\u67d4\u97e7\u6027\uff0c\u900f\u660e\u6027\u548c\u6eb6\u6db2\u52a0\u5de5\u6027\u65b9\u9762\u5177\u6709\u663e\u8457\u7684\u4f18\u52bf\u3002\u4f46\u662f\uff0c\u5173\u4e8e\u6709\u673a\u957f\u4f59\u8f89\u53d1\u5149\u6750\u6599\u7684\u5206\u5b50\u9009\u62e9\u7b56\u7565\u4ecd\u7136\u4e0d\u6e05\u695a\u3002\u8fd1\u65e5\uff0c\u65e5\u672c\u8457\u540d\u6709\u673a\u5316\u5b66\u3001\u6750\u6599\u5316\u5b66\u5bb6\uff0c\u4e5d\u5dde\u5927\u5b66Chihaya Adachi\u6559\u6388\u8bfe\u9898\u7ec4\u53d1\u73b0\u4e86\u6fc0\u57fa\u590d\u5408\u7269\u7cfb\u7edf\u4e2d\u6700\u4f4e\u7684\u5c40\u90e8\u4e09\u91cd\u6fc0\u53d1\u6001\u548c\u6700\u4f4e\u7684\u5355\u91cd\u7535\u8377\u8f6c\u79fb\u6fc0\u53d1\u6001\u4e4b\u95f4\u7684\u80fd\u9699\u5bf9LPL\u6027\u80fd\u5f71\u54cd\u7684\u673a\u7406\u3002\u7cfb\u7edf\u7814\u7a76\u4e86\u4e09\u79cd\u4e0d\u540c\u7684\u80fd\u9699\u4f9b\u4f53\u6750\u6599\u7684LPL\u6301\u7eed\u65f6\u95f4\u548c\u5149\u8c31\u7279\u6027\u53d8\u5316\u89c4\u5f8b\u3002\u7ed3\u679c\u53d1\u73b0\uff1a\u5f53\u6700\u4f4e\u7684\u5c40\u90e8\u4e09\u91cd\u6fc0\u53d1\u6001\u7684\u80fd\u7ea7\u6bd4\u7535\u8377\u8f6c\u79fb\u6fc0\u53d1\u6001\u7684\u80fd\u7ea7\u4f4e\u5f97\u591a\u65f6\uff0c\u8be5\u7cfb\u7edf\u7684LPL\u6301\u7eed\u65f6\u95f4\u77ed\uff0c\u5e76\u4e14\u6e05\u9664\u4e86\u7531\u6fc0\u57fa\u590d\u5408\u7269\u8367\u5149\u548c\u4f9b\u4f53\u78f7\u5149\u5f15\u8d77\u7684\u4e24\u4e2a\u4e0d\u540c\u7684\u53d1\u5c04\u7279\u5f81\u3002<sup>[<\/sup><sup>4<\/sup><sup>]<\/sup>\u76f8\u5173\u7814\u7a76\u4ee5\u201cInfluence of energy gap between charge-transfer and locally excited states on organic long persistence luminescence\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728Nature Communications\u3002<\/p>\n<p><strong><b>\u56fe4<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u6709\u673a\u957f\u4f59\u8f89\u53d1\u5149\u6750\u6599\u53d1\u5149\u673a\u7406\u793a\u610f\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-201474 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72474-11.png\" alt=\"\" width=\"757\" height=\"372\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72474-11.png 757w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72474-11-300x147.png 300w\" sizes=\"(max-width: 757px) 100vw, 757px\" \/><\/p>\n<p><strong><b>\u81ea\u53d1\u89e3\u79bb\u7684\u6709\u673a\u8367\u5149\u56e2\u6fc0\u5b50\u7f13\u6162\u91cd\u7ec4\u7684\u7814\u7a76<\/b><\/strong><\/p>\n<p>\u6709\u673a\u8367\u5149\u56e2\u4ee5\u53d1\u5149\u7684\u5f62\u5f0f\u6536\u96c6\u6fc0\u5b50\u6784\u6210\u4e86\u53d1\u5149\u5e94\u7528\u7684\u57fa\u7840\u3002\u5c3d\u7ba1\u9ad8\u7684\u5149\u81f4\u53d1\u5149\u91cf\u5b50\u4ea7\u7387\u5bf9\u4e8e\u6709\u6548\u7684\u53d1\u5149\u81f3\u5173\u91cd\u8981\uff0c\u4f46\u4f1a\u4f34\u968f\u7740\u53d1\u5c04\u6fc0\u5b50\u6d53\u5ea6\u4f9d\u8d56\u6027\u731d\u706d\u7684\u4e0d\u5229\u73b0\u8c61\u3002\u8fd1\u65e5\uff0c\u65e5\u672c\u8457\u540d\u6709\u673a\u5316\u5b66\u3001\u6750\u6599\u5316\u5b66\u5bb6\uff0c\u4e5d\u5dde\u5927\u5b66Chihaya Adachi\u6559\u6388\u8bfe\u9898\u7ec4\u53d1\u73b0\u6d53\u5ea6\u4f9d\u8d56\u6027\u7684\u201c\u957f\u5bff\u547d\u201d\uff08\u5373\u8d85\u8fc71\u5c0f\u65f6\uff09\u5149\u751f\u8f7d\u6d41\u5b50\u7684\u4ea7\u751f\u548c\u79ef\u7d2f\uff0c\u4ee5\u53ca\u5728\u5305\u542b\u6781\u6027\u8367\u5149\u56e2\u7684\u56fa\u6001\u819c\u4e2d\u7535\u81f4\u53d1\u5149\u80fd\u91cf\u7684\u8fde\u7eed\u91ca\u653e\u7b49\u73b0\u8c61\u3002\u5c3d\u7ba1\u4eba\u4eec\u8ba4\u4e3a\u8367\u5149\u56e2\u6fc0\u5b50\u662f\u7a33\u5b9a\u7684\uff0c\u4f46\u7814\u7a76\u7ed3\u679c\u8868\u660e\u5728\u6ca1\u6709\u5916\u90e8\u7535\u573a\u7684\u60c5\u51b5\u4e0b\uff0c\u67d0\u4e9b\u6fc0\u5b50\u5728\u56fa\u6001\u819c\u4e2d\u4e5f\u4f1a\u901a\u8fc7\u81ea\u53d1\u53d6\u5411\u6781\u5316\u53d1\u751f\u81ea\u53d1\u6027\u6fc0\u5b50\u89e3\u79bb\u3002\u8fd9\u4e9b\u7ed3\u679c\u5bfc\u81f4\u5bf9\u5305\u542b\u6781\u6027\u6709\u673a\u5206\u5b50\u56fa\u4f53\u819c\u7684\u201c\u53d1\u5149\u91cf\u5b50\u4ea7\u7387\u201d\u542b\u4e49\u7684\u65b0\u601d\u8003\u3002<sup>[5<\/sup><sup>]<\/sup>\u76f8\u5173\u7814\u7a76\u4ee5\u201cSlow recombination of spontaneously dissociated organic fluorophore excitons\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728Nature Communications\u3002<\/p>\n<p><strong><b>\u56fe5<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u542b\u6709\u6781\u6027\u8367\u5149\u56e2\u7684\u56fa\u4f53\u819c\u4e2d\u81ea\u53d1\u6fc0\u5b50\u89e3\u79bb\u548c\u91cd\u7ec4\u8fc7\u7a0b\u7684\u793a\u610f\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-201475 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72475-10.png\" alt=\"\" width=\"558\" height=\"217\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72475-10.png 558w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72475-10-300x117.png 300w\" sizes=\"(max-width: 558px) 100vw, 558px\" \/><\/p>\n<p style=\"text-align: center;\"><strong><b>\u6768\u671d\u9f99\u8bfe\u9898\u7ec4<\/b><\/strong><\/p>\n<p><strong><b>\u4e0e\u6fc0\u53d1\u6709\u5173\u7684\u957f\u5bff\u547d\u53d1\u5149\u805a\u5408\u7269\u7cfb\u7edf\u7684\u7814\u7a76<\/b><\/strong><\/p>\n<p>\u6709\u673a\u5ba4\u6e29\u53d1\u5149\u6750\u6599\u901a\u5e38\u5177\u6709\u957f\u5bff\u547d\u7684\u72ec\u7279\u78f7\u5149\u53d1\u5c04\u3002\u4f46\u5728\u53d7\u5230\u5916\u90e8\u523a\u6fc0\u65f6\uff0c\u8fd9\u4e9b\u6750\u6599\u4ec5\u53d1\u51fa\u5355\u4e00\u84dd\u5149\u6216\u7eff\u5149\uff0c\u56e0\u6b64\u5176\u989c\u8272\u53ef\u8c03\u6027\u53d7\u5230\u4e25\u683c\u9650\u5236\u3002\u91cd\u5e86\u7406\u5de5\u5927\u5b66\u6768\u671d\u9f99\u6559\u6388\u8bfe\u9898\u7ec4\u901a\u8fc7\u7b80\u5355\u7684pyrene\u884d\u751f\u7269\u63ba\u6742\u5230\u805a\u5408\u7269\u57fa\u4f53\u4e2d\uff0c\u5c06\u53d1\u5c04\u989c\u8272\u8303\u56f4\u4ece\u84dd\u8272\u6269\u5c55\u5230\u7ea2\u8272\u3002\u8fd9\u4e9b\u63ba\u6742\u5728\u805a\u5408\u7269\u8584\u819c\u4e2d\u7684pyrene\u5206\u5b50\u663e\u8457\u589e\u5f3a\u4e86\u7cfb\u7edf\u95f4\u7684\u7a7f\u8d8a\u9014\u5f84\uff0c\u964d\u4f4e\u4e86\u7cfb\u7edf\u7684\u7b2c\u4e00\u4e2a\u4e09\u91cd\u6001\u6c34\u5e73\uff0c\u5e76\u786e\u4fdd\u4e86\u819c\u5bf9\u6fc0\u53d1\u80fd\u5177\u6709\u654f\u611f\u7684\u54cd\u5e94\uff0c\u6700\u540e\u5728\u73af\u5883\u6761\u4ef6\u4e0b\u4ea7\u751f\u4f9d\u8d56\u4e8e\u6fc0\u53d1\u7684\u957f\u5bff\u547d\u53d1\u5149\u805a\u5408\u7269\u4f53\u7cfb\u3002\u8fd9\u4e9b\u6750\u6599\u53ef\u7528\u4f5c\u6784\u5efa\u5177\u6709\u591a\u8272\u4e92\u8f6c\u6362\u7684\u9632\u4f2a\u56fe\u6848\uff0c\u663e\u793a\u51fa\u5728\u4fe1\u606f\u9886\u57df\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u3002<sup>[<\/sup><sup>6]<\/sup>\u76f8\u5173\u7814\u7a76\u4ee5\u201cExcitation-Dependent Long-Life Luminescent Polymeric Systems under Ambient Conditions\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728Angewandte Chemie International Edition\u3002<\/p>\n<p><strong><b>\u56fe6<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>\u4e0d\u540c<\/b><\/strong><strong><b>pyrene<\/b><\/strong><strong><b>\u884d\u751f\u7269\u63ba\u6742\u7684P<\/b><\/strong><strong><b>VA<\/b><\/strong><strong><b>\u805a\u5408\u7269\u6fc0\u53d1-\u78f7\u5149\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-201476 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72476-9.png\" alt=\"\" width=\"684\" height=\"345\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72476-9.png 684w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72476-9-300x151.png 300w\" sizes=\"(max-width: 684px) 100vw, 684px\" \/><\/p>\n<p><strong><b>\u57fa\u4e8e\u805a\u78f7\u8148\u989c\u8272\u53ef\u8c03\u7684\u957f\u4f59\u8f89\u53d1\u5149\u805a\u5408\u7269\u7684\u7814\u7a76<\/b><\/strong><\/p>\n<p>\u6709\u673a\u957f\u4f59\u8f89\u53d1\u5149\uff08OLPL\uff09\u6750\u6599\u56e0\u5176\u4f18\u5f02\u7684\u5149\u5b66\u6027\u80fd\u5728\u751f\u7269\u6210\u50cf\uff0c\u4fe1\u606f\u5b89\u5168\uff0c\u663e\u793a\uff0c\u9632\u4f2a\u7b49\u9886\u57df\u5177\u6709\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u3002\u76ee\u524d\u53ef\u4ee5\u901a\u8fc7\u4e00\u4e9b\u6709\u6548\u7684\u7b56\u7565\u6765\u4fc3\u8fdb\u6fc0\u53d1\u5355\u91cd\u6001\u5230\u4e09\u91cd\u6001\u7684\u7cfb\u7edf\u95f4\u7a7f\u8d8a\uff08ISC\uff09\u5e76\u9650\u5236\u975e\u8f90\u5c04\u8dc3\u8fc1\uff0c\u4ece\u800c\u83b7\u5f97\u5bff\u547d\u957f\uff08\u5927\u4e8e1s\uff09\u548c\u9ad8\u91cf\u5b50\u4ea7\u7387\u7684OLPL\u6750\u6599\u3002\u4f46\u662f\uff0c\u5f88\u5c11\u6709\u5173\u4e8e\u5177\u6709\u52a8\u6001\u548c\u6fc0\u53d1\u76f8\u5173\u7279\u6027\u7684OLPL\u6750\u6599\u7684\u62a5\u9053\u3002\u91cd\u5e86\u7406\u5de5\u5927\u5b66\u6768\u671d\u9f99\u6559\u6388\u8bfe\u9898\u7ec4\u6210\u529f\u8bbe\u8ba1\u5e76\u5408\u6210\u4e86\u4e24\u79cd\u65b0\u578b\u7684\u542b\u5494\u5511\u57fa\u5355\u5143\u7684\u65b0\u578b\u805a\u78f7\u8148\u884d\u751f\u7269\uff0c\u5e76\u628a\u5b83\u4eec\u63ba\u5165\u805a\u4e59\u70ef\u9187\uff08PVA\uff09\u8584\u819c\u4e2d\uff0c\u4ee5\u5b9e\u73b0\u805a\u5408\u7269\u957f\u4f59\u8f89\u53d1\u5149\uff08PLPL\uff09\u3002\u51fa\u4e4e\u610f\u6599\u7684\u662f\uff0c\u5728\u73af\u5883\u6761\u4ef6\u4e0b\uff08\u5728\u5ba4\u6e29\u4e0b\u7684\u7a7a\u6c14\u4e2d\uff09\u83b7\u5f97\u4f9d\u8d56\u4e8e\u6fc0\u53d1\u7684PLPL\uff08ED-PLPL\uff09\uff0c\u5e76\u4e14\u968f\u7740\u6fc0\u53d1\u6ce2\u957f\u7684\u53d8\u5316\uff0c\u957f\u4f59\u8f89\u53d1\u5149\u989c\u8272\u53ef\u4ee5\u4ece\u84dd\u8272\u53d8\u4e3a\u7eff\u8272\u3002\u540c\u65f6\uff0c\u57fa\u4e8ePVA\u94fe\u4e0e\u805a\u78f7\u8148\u8367\u5149\u7c89\u4e4b\u95f4\u6c22\u952e\u76f8\u4e92\u4f5c\u7528\u7684\u5f62\u6210\u548c\u7834\u574f\uff0c\u5b9e\u73b0\u4e86ED-PLPL\u7684\u52a8\u6001\u5faa\u73af\u3002\u8fd9\u9879\u5de5\u4f5c\u4e3a\u5728\u73af\u5883\u6761\u4ef6\u4e0b\u8bbe\u8ba1\u989c\u8272\u53ef\u8c03\u7684\u805a\u5408\u7269\u53d1\u5149\u6750\u6599\u63d0\u4f9b\u4e86\u65b0\u7684\u7b56\u7565\u3002<sup>[<\/sup><sup>7]<\/sup>\u76f8\u5173\u7814\u7a76\u4ee5\u201cColor\u2010Tunable Polymeric Long\u2010Persistent Luminescence Based on Polyphosphazenes\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728Anvanced materials\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>7 <\/b><\/strong><strong><b>\u52a8\u6001ED-PLPL\u6750\u6599\u5728\u9632\u4f2a\u52a0\u5bc6\u548c\u4fe1\u606f\u5b58\u50a8\u4e2d\u7684\u5e94\u7528<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-201477 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72477-8.png\" alt=\"\" width=\"522\" height=\"410\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72477-8.png 522w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72477-8-300x236.png 300w\" sizes=\"(max-width: 522px) 100vw, 522px\" \/><\/p>\n<p style=\"text-align: center;\"><strong>\u6f58\u6885\u8bfe\u9898\u7ec4<\/strong><\/p>\n<p><strong>\u5177\u6709\u8870\u51cf\u6548\u7387\u4f4e\u3001\u7eb3\u79d2\u7ea7\u65f6\u5ef6\u8367\u5149\u5206\u5b50\u7684\u6df1\u84dd\u8272OLED\u7684\u7814\u7a76<\/strong><\/p>\n<p>\u5177\u6709\u70ed\u6fc0\u6d3b\u5ef6\u8fdf\u8367\u5149\uff08TADF\uff09\u7684\u82b3\u9999\u6709\u673a\u6df1\u84dd\u8272\u53d1\u5c04\u4f53\u53ef\u4ee5\u6536\u96c6\u7535\u6fc0\u53d1\u8fc7\u7a0b\u4e2d\u5355\u91cd\u6001\u548c\u4e09\u91cd\u6001\u7684\u6240\u6709\u6fc0\u5b50\u8fdb\u884c\u5149\u53d1\u5c04\u3002\u7136\u800c\uff0c\u84dd\u8272TADF\u53d1\u5c04\u4f53\u901a\u5e38\u5177\u6709\u957f\u7684\u6fc0\u5b50\u5bff\u547d\uff0c\u5bfc\u81f4\u5728\u9ad8\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u6548\u7387\u4e25\u91cd\u964d\u4f4e\u540c\u65f6\u5728\u6709\u673a\u53d1\u5149\u4e8c\u6781\u7ba1\u4e2d\u6fc0\u5b50\u6e6e\u6ca1\u3002\u4e2d\u5c71\u5927\u5b66\u6f58\u6885\u6559\u6388\u8bfe\u9898\u7ec4\u62a5\u9053\u4e86\u4e00\u79cd\u91c7\u7528\u7b80\u5355\u5206\u5b50\u8bbe\u8ba1\u7684\u6df1\u84dd\u8272TADF\u53d1\u5c04\u5668\uff0c\u5176\u4e2d\uff0c\u540c\u65f6\u63a7\u5236\u4e86\u6d3b\u5316\u80fd\u4ee5\u53ca\u5177\u6709\u4e0d\u540c\u81ea\u65cb\u591a\u91cd\u6027\u7684\u6fc0\u53d1\u6001\u4e4b\u95f4\u7684\u81ea\u65cb\u8f68\u9053\u8026\u5408\u3002\u5728\u6ca1\u6709\u91cd\u91d1\u5c5e\u5143\u7d20\u7684\u65bd\u4e3b-\u53d7\u4e3b\u578b\u5206\u5b50\u7ed3\u6784\u4e2d\uff0c\u6fc0\u5b50\u7684\u5bff\u547d\u8fbe\u5230\u4e86750 ns\u3002\u4f7f\u7528\u6b64TADF\u53d1\u5c04\u5668\u7684OLED\u663e\u793a\u6df1\u84dd\u8272\u7535\u81f4\u53d1\u5149\uff08EL\uff09\uff0c\u5176CIE\u8272\u5ea6\u5750\u6807\u4e3a\uff080.14\uff0c0.18\uff09\uff0c\u6700\u5927EL\u91cf\u5b50\u6548\u7387\u9ad8\u8fbe20.7\uff05\u3002\u6b64\u5916\uff0c\u5373\u4f7f\u5728\u9ad8\u4eae\u5ea6\u4e0b\uff0c\u9ad8\u7684\u6700\u5927\u6548\u7387\u4e5f\u4fdd\u6301\u4e3a20.2\uff05\u548c17.4\uff05\u3002<sup>[<\/sup><sup>8]<\/sup>\u76f8\u5173\u7814\u7a76\u4ee5\u201cNanosecond-time-scale delayed fluorescence molecule for deep-blue OLEDs with small efficiency rolloff\u201d\u4e3a\u9898\uff0c\u53d1\u8868\u5728Nature Communications\u3002<\/p>\n<p><strong><b>\u56fe8<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>TADF\u673a\u7406\u793a\u610f\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"size-full wp-image-201478 aligncenter\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72478-7.png\" alt=\"\" width=\"511\" height=\"240\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72478-7.png 511w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/\u56fe\u72478-7-300x141.png 300w\" sizes=\"(max-width: 511px) 100vw, 511px\" \/><\/p>\n<p><strong><b>\u53c2\u8003\u6587\u732e<\/b><\/strong><\/p>\n<p>1 Cai, Suzhi, et al. &#8220;Enabling long-lived organic room temperature phosphorescence in polymers by subunit interlocking.&#8221; Nature communications 10.1 (2019): 1-8.<\/p>\n<p>2 Gu, Long, et al. &#8220;Colour-tunable ultra-long organic phosphorescence of a single-component molecular crystal.&#8221; Nature Photonics 13.6 (2019): 406-411.<\/p>\n<p>3 Xu, Weidong, et al. &#8220;Rational molecular passivation for high-performance perovskite light-emitting diodes.&#8221; Nature Photonics 13.6 (2019): 418-424.<\/p>\n<p>4 Lin, Zesen, et al. &#8220;Influence of energy gap between charge-transfer and locally excited states on organic long persistence luminescence.&#8221; Nature Communications 11.1 (2020): 1-7.<\/p>\n<p>5 Yamanaka, Takahiko, Hajime Nakanotani, and Chihaya Adachi. &#8220;Slow recombination of spontaneously dissociated organic fluorophore excitons.&#8221; Nature Communications 10.1 (2019): 1-6.<\/p>\n<p>6 Su, Yan, et al. &#8220;Excitation\u2010Dependent Long\u2010Life Luminescent Polymeric Systems under Ambient Conditions.&#8221; Angewandte Chemie International Edition (2019).<\/p>\n<p>7 Wang, Zhonghao, et al. &#8220;Color\u2010Tunable Polymeric Long\u2010Persistent Luminescence Based on Polyphosphazenes.&#8221; Advanced Materials (2020): 1907355.<\/p>\n<p>8 Kim, Jong Uk, et al. &#8220;Nanosecond-time-scale delayed fluorescence molecule for deep-blue OLEDs with small efficiency rolloff.&#8221; Nature communications 11.1 (2020): 1-8.<\/p>\n<p>\u672c\u6587\u7531 Leo\u00a0Wu\u4f9b\u7a3f\u3002<\/p>\n<p>\u672c\u5185\u5bb9\u4e3a\u4f5c\u8005\u72ec\u7acb\u89c2\u70b9\uff0c\u4e0d\u4ee3\u8868\u6750\u6599\u4eba\u7f51\u7acb\u573a\u3002<\/p>\n<p>\u672a\u7ecf\u5141\u8bb8\u4e0d\u5f97\u8f6c\u8f7d\uff0c\u6388\u6743\u4e8b\u5b9c\u8bf7\u8054\u7cfbkefu@cailiaoren.com\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u9ec4\u7ef4\u9662\u58eb\u8bfe\u9898\u7ec4 \u4e9a\u5355\u5143\u4e92\u9501\u5b9e\u73b0\u805a\u5408\u7269\u4e2d\u957f\u5bff\u547d\u7684\u6709\u673a\u5ba4\u6e29\u78f7\u5149\u7684\u7814\u7a76 \u957f\u5bff\u547d\u7684\u5ba4\u6e29\u78f7\u5149\uff08LRTP\uff09\u662f\u4e00\u79cd\u5728\u6709\u673a\u7535\u5b50\u548c\u5149\u5b50\u5b66\u4e2d\u5f15\u4eba\u6ce8\u76ee\u7684\u5149\u5b66\u73b0\u8c61\u3002\u5c3d\u7ba1\u8fd1\u4e9b\u5e74\u6765\u53d1\u5c55\u5341\u5206&#8230;<\/p>\n","protected":false},"author":10213,"featured_media":182269,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-201470","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/201470"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/10213"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=201470"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/201470\/revisions"}],"predecessor-version":[{"id":204793,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/201470\/revisions\/204793"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/182269"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=201470"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=201470"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=201470"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}