{"id":202788,"date":"2020-06-05T06:56:57","date_gmt":"2020-06-04T22:56:57","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=202788"},"modified":"2020-06-04T19:57:36","modified_gmt":"2020-06-04T11:57:36","slug":"%e5%8d%97%e6%96%b9%e7%a7%91%e5%a4%a7%e6%be%b3%e5%a4%a7-afm-%e7%bb%bc%e8%bf%b0%ef%bc%9a%e7%ae%80%e5%8c%96%e9%ab%98%e6%80%a7%e8%83%bd%e9%92%99%e9%92%9b%e7%9f%bf%e5%a4%aa%e9%98%b3%e8%83%bd%e7%94%b5","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=202788","title":{"rendered":"\u5357\u65b9\u79d1\u5927&#038;\u6fb3\u5927 AFM \u7efc\u8ff0\uff1a\u7b80\u5316\u9ad8\u6027\u80fd\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u7684\u5668\u4ef6\u7ed3\u6784\u7684\u53d1\u5c55\u72b6\u51b5"},"content":{"rendered":"<p><strong>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011<\/strong><\/p>\n<p>\u4f17\u6240\u5468\u77e5\uff0c\u592a\u9633\u80fd\u4f5c\u4e3a\u4e00\u79cd\u6e05\u6d01\u4e14\u53d6\u4e4b\u4e0d\u5c3d\u7684\u80fd\u6e90\uff0c\u662f\u5e94\u5bf9\u5168\u7403\u53d8\u6696\u548c\u80fd\u6e90\u5371\u673a\u7684\u7406\u60f3\u89e3\u51b3\u65b9\u6848\u3002\u56e0\u6b64\uff0c\u79d1\u5b66\u5bb6\u4eec\u53d1\u660e\u4e86\u7845\u3001\u65e0\u673a\u8584\u819c\u3001\u67d3\u6599\u654f\u5316\u3001\u6709\u673a\u8584\u819c\u3001\u91cf\u5b50\u70b9\u3001\u9499\u949b\u77ff\u7b49\u4e00\u7cfb\u5217\u7684\u5149\u4f0f\u6750\u6599\u5c06\u5149\u80fd\u8f6c\u5316\u4e3a\u7535\u80fd\u3002\u5176\u4e2d\uff0c\u6709\u673a-\u65e0\u673a\u5364\u5316\u7269\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\uff08PSCs\uff09\u7531\u4e8e\u5236\u5907\u7b80\u5355\u3001\u6210\u672c\u4f4e\u5ec9\u3001\u6027\u80fd\u4f18\u5f02\u800c\u5f97\u5230\u5e7f\u6cdb\u7684\u5173\u6ce8\u3002\u76ee\u524d\uff0cPSCs\u7684\u80fd\u91cf\u8f6c\u6362\u6548\u7387\uff08PCE\uff09\u6700\u9ad8\u53ef\u8fbe25.2\uff05\uff0c\u8d85\u8fc7\u4e86\u5927\u591a\u6570\u5176\u5b83\u5149\u4f0f\u8bbe\u5907\u3002\u9ad8\u6027\u80fdPSCs\u901a\u5e38\u7531\u7535\u5b50\u4f20\u8f93\u5c42\uff08ETL\uff09\u3001\u9499\u949b\u77ff\u5438\u5149\u5c42\u548c\u7a7a\u7a74\u4f20\u8f93\u5c42\uff08HTL\uff09\u7ec4\u6210\u3002\u5728\u5185\u7f6e\u7535\u573a\u7684\u9a71\u52a8\u4e0b\uff0c\u5149\u751f\u7535\u5b50\u548c\u7a7a\u7a74\u88ab\u5206\u79bb\u5e76\u5206\u522b\u8f6c\u79fb\u5230ETL\u548cHTL\u3002\u5176\u4e2d\uff0cETL\u53ef\u4ee5\u6536\u96c6\u7535\u5b50\u5e76\u963b\u6321\u7a7a\u7a74\uff0c\u800cHTL\u53ef\u4ee5\u6536\u96c6\u7a7a\u7a74\u5e76\u963b\u6321\u7535\u5b50\u3002\u7136\u800c\uff0cETL\/HTL\u4f7fPSCs\u5236\u5907\u8fc7\u7a0b\u590d\u6742\uff0c\u589e\u52a0\u4e86\u751f\u4ea7\u6210\u672c\uff0c\u62b5\u6d88\u4e86\u9499\u949b\u77ff\u6750\u6599\u6210\u672c\u4f4e\u5ec9\u7684\u4f18\u52bf\u3002\u5728PSCs\u6548\u7387\u9010\u6e10\u63a5\u8fd1\u7406\u8bba\u6781\u9650\u7684\u60c5\u51b5\u4e0b\uff0c\u5fae\u5c0f\u7684\u8fdb\u4e00\u6b65\u63d0\u5347\u90fd\u9700\u8981\u4ed8\u51fa\u5de8\u5927\u7684\u4ee3\u4ef7\u3002\u76f8\u53cd\uff0c\u5982\u679c\u4e0d\u727a\u7272\u5149\u4f0f\u6027\u80fd\uff0c\u800c\u80fd\u7b80\u5316\u5668\u4ef6\u7ed3\u6784\uff0c\u5c06\u7ed9\u5546\u4e1a\u5316\u5e26\u6765\u591a\u65b9\u9762\u597d\u5904\u3002\u56e0\u6b64\uff0c\u5404\u79cd\u65e0ETL\u6216\/\u548c\u65e0HTL\u7684PSCs\u88ab\u5f00\u53d1\u4e86\u51fa\u6765\uff0c\u5e76\u4e14\u5438\u5f15\u4e86\u8d8a\u6765\u8d8a\u591a\u7684\u5173\u6ce8\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u57fa\u4e8e\u6b64\uff0c<strong>\u5357\u65b9\u79d1\u6280\u5927\u5b66\u7684\u7a0b\u6625\u526f\u6559\u6388\u548c\u6fb3\u95e8\u5927\u5b66\u7684\u90a2\u8d35\u5ddd\u6559\u6388\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u56e2\u961f<\/strong>\u8054\u5408\u62a5\u9053\u4e86\u4e00\u7bc7\u5173\u4e8e\u7b80\u5316\u9ad8\u6027\u80fd\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\uff08PSCs\uff09\u7684\u5668\u4ef6\u7ed3\u6784\u7684\u7efc\u8ff0\u3002\u5728\u672c\u6587\u4e2d\uff0c\u4f5c\u8005\u9996\u5148\u603b\u7ed3\u4e86\u5e38\u89c4PSCs\u4e2d\u5df2\u91c7\u7528\u7684\u5e38\u7528\u4e8e\u964d\u4f4e\u7f3a\u9677\u5bc6\u5ea6\u548c\u4f18\u5316\u80fd\u7ea7\u7684\u7b56\u7565\uff0c\u5e76\u5c06\u8fd9\u4e9b\u7b56\u7565\u5ef6\u4f38\u5230\u7b80\u5316\u65e0ETL\u6216\/\u548cHTL\u7684\u5668\u4ef6\u4e2d\uff0c\u4ee5\u63d0\u9ad8\u5b83\u4eec\u7684\u5149\u4f0f\u6027\u80fd\u3002\u7136\u540e\uff0c\u4f5c\u8005\u603b\u7ed3\u4e86\u5177\u6709\u7b80\u5316\u7ed3\u6784\u7684\u5404\u79cdPSCs\u7684\u53d1\u5c55\u5386\u7a0b\uff0c\u5305\u62ec\u65e0HTL\u7684PSCs\u3001\u65e0ETL\u7684PSCs\u548c\u65e0HTL\/ETL\u7684PSCs\u3002\u8ba8\u8bba\u4e86\u5b83\u4eec\u7684\u5de5\u4f5c\u539f\u7406\u4ee5\u53ca\u5b58\u5728\u7684\u95ee\u9898\uff0c\u5df2\u5b9e\u65bd\u7684\u6280\u672f\u548c\u8fdb\u4e00\u6b65\u7684\u6027\u80fd\u6539\u8fdb\u65b9\u5411\u3002\u603b\u4e4b\uff0c\u4f5c\u8005\u5e0c\u671b\u901a\u8fc7\u672c\u6587\u5173\u4e8e\u7b80\u5f0f PSCs\u7684\u603b\u7ed3\u4ee5\u4fc3\u8fdbPSCs\u7684\u53d1\u5c55\uff0c\u4f7f\u5176\u671d\u7740\u4f4e\u6210\u672c\u548c\u5927\u89c4\u6a21\u5236\u9020\u7684\u6700\u7b80\u5355\u6784\u9020\u53d1\u5c55\u3002\u7814\u7a76\u6210\u679c\u4ee5 <strong>\u201cTowards Simplifying the Device Structure of High-Performance Perovskite Solar Cells\u201d<\/strong>\u4e3a\u9898\u53d1\u8868\u5728\u56fd\u9645\u8457\u540d\u671f\u520a<strong>Advanced Functional Materials<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u672c\u6587\u7b2c\u4e00\u4f5c\u8005\u4e3a\u5357\u65b9\u79d1\u6280\u5927\u5b66\u4e0e\u6fb3\u95e8\u5927\u5b66\u8054\u5408\u57f9\u517b\u7684\u9ec4\u6bd3\u5c9a\u535a\u58eb<\/strong>\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u89e3\u6790\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00\u3001\u672c\u6587\u7684\u6846\u67b6\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202789\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/1-67.jpg\" alt=\"\" width=\"600\" height=\"251\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/1-67.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/1-67-300x126.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe\u4e8c\u3001\u901a\u8fc7\u8868\u9762\u5904\u7406\u4ee5\u964d\u4f4e\u7f3a\u9677\u5bc6\u5ea6<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202790\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/2-68.jpg\" alt=\"\" width=\"600\" height=\"835\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/2-68.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/2-68-216x300.jpg 216w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u7528CH<sub>3<\/sub>NH<sub>2<\/sub>\u6c14\u4f53\u5904\u7406\u7684MAPbI<sub>3<\/sub>\u8584\u819c\u7684\u5408\u6210\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08b-c\uff09\u6709\/\u65e0CH<sub>3<\/sub>NH<sub>2<\/sub>\u6c14\u4f53\u5904\u7406\u7684MAPbI<sub>3<\/sub>\u8584\u819c\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08d-e\uff09\u6709\/\u65e0MABr\u5904\u7406\u7684MAPbI<sub>3<\/sub>\u8584\u819c\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08f-g\uff09\u6709\/\u65e0PMMA\u4fee\u9970\u7684\u9499\u949b\u77ff\u8584\u819c\u7684SEM\u56fe\u50cf\uff08\u65e0HTL\u5668\u4ef6\uff09\u3002<\/p>\n<p><strong>\u56fe\u4e09\u3001\u901a\u8fc7\u9499\u949b\u77ff\u524d\u4f53\u63ba\u6742\u4ee5\u964d\u4f4e\u7f3a\u9677\u5bc6\u5ea6<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202791\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/3-67.jpg\" alt=\"\" width=\"600\" height=\"319\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/3-67.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/3-67-300x160.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-b\uff09\u6709\/\u65e0\u5c3f\u7d20\u63ba\u6742\u7684\u9499\u949b\u77ff\u8584\u819c\u7684\u7ed3\u6784\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08c-d\uff09\u6709\/\u65e0\u5c3f\u7d20\u63ba\u6742\u7684\u9499\u949b\u77ff\u8584\u819c\u7684AFM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08e\uff09\u63ba\u6742\u4e86K<sup>+<\/sup>\u7684PSCs\u7684\u7ed3\u6784\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08f-g\uff09\u6709\/\u65e0\u63ba\u5165K<sup>+<\/sup>\u7684\u9499\u949b\u77ff\u8584\u819c\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08h-i\uff09MAPbI<sub>3<\/sub>:C<sub>70<\/sub>\u548cMAPbI<sub>3<\/sub>\u8584\u819c\u76f4\u63a5\u6d82\u8986\u5728\u73bb\u7483\/FTO\u4e0a\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08j\uff09\u5177\u6709F4TCNQ\u63ba\u6742\u7684\u9499\u949b\u77ff\u819c\u7684\u522e\u6d82\u5de5\u827a\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08k\uff09\u76f4\u63a5\u6c89\u79ef\u5728\u73bb\u7483\/ITO\u4e0a\u7684\u9499\u949b\u77ff\u8584\u819c\u7684\u6a2a\u622a\u9762SEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u56db\u3001\u8c03\u8282\u80fd\u7ea7\u5339\u914d<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202794\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/4-63.jpg\" alt=\"\" width=\"600\" height=\"333\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/4-63.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/4-63-300x167.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u5177\u6709\u4e0d\u540cBr: I\u6bd4\u7684MAPbBr<sub>3<\/sub>-xIx QD\u3001MAPbI<sub>3<\/sub>\u548cHTL\u7684\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08b-c\uff09\u5728\u4e8c\u6b21\u7535\u5b50\u89d2\u548c\u4ef7\u5e26\u533a\u57df\u4e2d\u6709\/\u65e0MXene\u7684\u9499\u949b\u77ff\u7684UPS\u5149\u8c31\uff1b<\/p>\n<p>\uff08d\uff09\u539f\u59cb\u9499\u949b\u77ff\u548cMXene\u6539\u6027\u9499\u949b\u77ff\u7684\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08e\uff09\u5728HOMO\u533a\u57df\u548c\u7b2c\u4e8ccuto\ufb00\u533a\u57df\u7684UPS\u9891\u8c31\uff1b<\/p>\n<p>\uff08f-g\uff09\u80fd\u7ea7\u5bf9\u51c6\u548c\u754c\u9762\u5076\u6781\u5b50\u7684\u5f62\u6210\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u4e94\u3001\u65e0ETL\u7684PSCs\u7684\u65e9\u671f\u53d1\u5c55<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202795\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/5-53.jpg\" alt=\"\" width=\"600\" height=\"376\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/5-53.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/5-53-300x188.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-b\uff09\u7531Kelly\u7b49\u4eba\u5236\u9020\u7684\u65e0ETL\u7684PSCs\u7684\u7ed3\u6784\u793a\u610f\u56fe\u548cJ-V\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08c\uff09\u4e0d\u540c\u5668\u4ef6\u7684\u5948\u594e\u65af\u7279\u963b\u6297\u56fe\uff1b<\/p>\n<p>\uff08d-e\uff09\u5728\u6709\/\u65e0UVO\u5904\u7406\u7684FTO\u57fa\u677f\u4e0a\u6c89\u79ef\u7684MAPbI<sub>3<\/sub>-xClx\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08f\uff09\u7b2c\u4e00\u4e2a\u65e0ETL\u7684\u53cd\u5f0fPSCs\u7684\u7ed3\u6784\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u516d\u3001\u901a\u8fc7\u6c89\u79ef\u9ad8\u8d28\u91cf\u9499\u949b\u77ff\u8584\u819c\u4ee5\u6539\u5584\u65e0ETL\u7684PSCs\u6027\u80fd<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202796\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/6-26.jpg\" alt=\"\" width=\"600\" height=\"349\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/6-26.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/6-26-300x175.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-b\uff09\u5404\u79cd\u5bcc\u52d2\u70ef\u884d\u751f\u7269\u7684\u793a\u610f\u56fe\u4ee5\u53ca\u65e0ETL\u7684PSCs\u7684\u7ed3\u6784\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08c\uff09\u6709\/\u65e0MAC1\u7684\u9499\u949b\u77ff\u819c\u7684\u5236\u5907\u8fc7\u7a0b\u7684\u793a\u610f\u56fe\u53ca\u5176\u76f8\u5e94\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08d\uff09\u6709\/\u65e0Sb\u63ba\u6742\u7684\u65e0ETL\u5668\u4ef6\u7684\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08e\uff09\u4e0d\u540c\u6469\u5c14\u6d53\u5ea6\u7684\u524d\u9a71\u4f53\u5236\u5907\u7684\u9499\u949b\u77ff\u819c\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u4e03\u3001\u901a\u8fc7\u7535\u6781\u4fee\u9970\u4ee5\u6539\u5584\u65e0ETL\u7684PSCs\u6027\u80fd<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202797\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/7-13.jpg\" alt=\"\" width=\"600\" height=\"346\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/7-13.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/7-13-300x173.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u57fa\u4e8e\u8680\u523b\u540e\u7684FTO\u5236\u5907\u7684PSCs\u7684\u622a\u9762SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08b\uff09\u5149\u751f\u7535\u5b50\u4ece\u9499\u949b\u77ff\u5230FTO\u7684\u63d0\u53d6\u884c\u4e3a\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08c-d\uff09\u539f\u59cbFTO\u548c\u8680\u523b\u540e\u7684FTO\u7684SEM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08e\uff09\u57fa\u4e8e\u8680\u523b\u540e\u7684FTO\u7684PSCs\u7684J-V\u66f2\u7ebf\u3002<\/p>\n<p>\uff08f-g\uff09\u9499\u949b\u77ff\u8584\u819c\u5728FTO\u4e0a\u6709\/\u65e0TMAH\u4fee\u9970\u7684AFM\u56fe\u50cf\uff1b<\/p>\n<p>\uff08h\uff09\u57fa\u4e8eTMAH\u4fee\u9970\u7684\u65e0ETL PSCs\u7684J-V\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe\u516b\u3001\u65e0HTL\u7684PSCs<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202798\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/8-9.jpg\" alt=\"\" width=\"600\" height=\"251\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/8-9.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/8-9-300x126.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u65e0HTL\u7684PSC\u7684\u7ed3\u6784\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u65e0HTL\u7684PSC\u7684\u80fd\u7ea7\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u4e5d\u3001\u65e0HTL\u7684\u6b63\u5f0fPSCs<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202799\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/9-5.jpg\" alt=\"\" width=\"600\" height=\"330\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/9-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/9-5-300x165.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-b\uff09\u7b2c\u4e00\u4e2a\u65e0HTL\u7684PSCs\u7684\u7ed3\u6784\u793a\u610f\u56fe\u548cJ-V\u66f2\u7ebf\uff1b<\/p>\n<p>\uff08c\uff09\u68af\u5ea6\u9499\u949b\u77ff\u5f02\u8d28\u7ed3\u7684\u6700\u4f73\u80fd\u7ea7\u56fe\u548c\u8f7d\u6d41\u5b50\u8f6c\u79fb\u673a\u5236\uff1b<\/p>\n<p>\uff08d\uff09\u57fa\u4e8e\u70ed\u538b\u78b3\u7684PSCs\u5408\u6210\u5de5\u827a\uff1b<\/p>\n<p>\uff08e\uff09MAPbI<sub>3<\/sub>\/MAPbIxBr<sub>3<\/sub>-x\u9499\u949b\u77ff\u819c\u7684\u5408\u6210\u8fc7\u7a0b\uff1b<\/p>\n<p>\uff08f\uff09\u6709\/\u65e0PbTiO<sub>3<\/sub>\u4e2d\u95f4\u5c42\u7684\u8017\u5c3d\u533a\u4e2d\u7535\u8377\u4f20\u8f93\u7684\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u5341\u3001\u65e0HTL\u3001\u53ef\u5370\u5237\u7684\u4ecb\u89c2PSCs<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202800\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/10-5.jpg\" alt=\"\" width=\"600\" height=\"339\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/10-5.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/10-5-300x170.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u4ecb\u89c2\u7684\u65e0HTL PSC\u7684\u7ed3\u6784\u793a\u610f\u56fe\u548c\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u63d2\u5165\u6709\u673a\u7845\u70f7\u5355\u5c42\u7684\u65e0HTL PSC\u7684\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08c\uff09\u542bMAPbI<sub>3<\/sub>\u6216FAPbI<sub>3<\/sub>\u5438\u6536\u5c42\u7684\u65e0HTL PSC\u7684\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08d\uff09\u5236\u5907MAPbI<sub>3<\/sub>\u5355\u6676PSC\u7684\u539f\u4f4d\u6676\u4f53\u8f6c\u79fb\u8fc7\u7a0b\u793a\u610f\u56fe\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e00\u3001\u65e0HTL\u7684\u53cd\u5f0f PSCs<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202801\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/11-4.jpg\" alt=\"\" width=\"600\" height=\"302\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/11-4.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/11-4-300x151.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u65e0HTL\u7684\u53cd\u5f0fPSC\u7684\u7ed3\u6784\u793a\u610f\u56fe\u548c\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u63ba\u6742CuSCN\u7684\u65e0HTL\u7684PSC\u7684\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08c\uff09BDPSO\u63ba\u6742\u5242\u5728\u65e0HTL\u7684PSC\u4e2d\u7684\u4f5c\u7528\u793a\u610f\u56fe\u3002\uff1b<\/p>\n<p>\uff08d\uff09\u5728\u6709\/\u65e0\u63ba\u6742F4-TCNQ\u7684\u60c5\u51b5\u4e0b\uff0cITO\/\u9499\u949b\u77ff\u754c\u9762\u4e0a\u7a7a\u7a74\u4f20\u8f93\u673a\u7406\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08e\uff09\u57fa\u4e8eF4-TCNQ\u7684\u65e0HTL\u7684PSC\u7684J-V\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe\u5341\u4e8c\u3001\u65e0ETL\u548cHTL\u7684PSCs<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-202802\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/12-3.jpg\" alt=\"\" width=\"600\" height=\"231\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/12-3.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/05\/12-3-300x116.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u6700\u7b80\u5f0fPSC\u7684\u793a\u610f\u56fe\u548c\u80fd\u7ea7\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u6700\u7b80\u5f0fPSC\u7684\u793a\u610f\u56fe\u548cJ-V\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u3010\u603b\u7ed3\u4e0e\u5c55\u671b\u3011<\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u76ee\u524d\u5df2\u8bb0\u5f55\u7684PSCs\u7684\u6548\u7387\u5df2\u63a5\u8fd1\u5355\u7ed3\u592a\u9633\u80fd\u7535\u6c60\u7684\u7406\u8bba\u6781\u9650\u3002\u53bb\u9664ETL\u6216HTL\u53ef\u4ee5\u6f5c\u5728\u5730\u7b80\u5316\u5668\u4ef6\u7ed3\u6784\u800c\u4e0d\u4f1a\u727a\u7272\u5149\u4f0f\u6027\u80fd\uff0c\u800c\u7b80\u5316\u7684\u5668\u4ef6\u7ed3\u6784\u53ef\u4ee5\u51cf\u5c11\u5236\u9020\u6b65\u9aa4\u548c\u964d\u4f4e\u6210\u672c\u3002\u7531\u4e8e\u9499\u949b\u77ff\u7684\u53cc\u6781\u6027\u7279\u6027\u548c\u957f\u7684\u8f7d\u6d41\u5b50\u6269\u6563\u957f\u5ea6\uff0cETL\u548cHTL\u5728\u7406\u8bba\u4e0a\u5bf9\u4e8e\u7535\u8377\u5206\u79bb\u548c\u63d0\u53d6\u5e76\u4e0d\u662f\u5fc5\u4e0d\u53ef\u5c11\u7684\u3002\u4f46\u662f\uff0c\u9664\u53bbETL\u6216HTL\u4ecd\u4f1a\u589e\u52a0\u80fd\u5792\uff0c\u5e76\u5bfc\u81f4\u4e25\u91cd\u7684\u7535\u8377\u590d\u5408\u3002\u901a\u8fc7\u8fdb\u4e00\u6b65\u4f18\u5316\u9499\u949b\u77ff\u8584\u819c\u7684\u8d28\u91cf\uff0c\u53ef\u4ee5\u6291\u5236\u7535\u8377\u590d\u5408\uff0c\u5ef6\u957f\u8f7d\u6d41\u5b50\u5bff\u547d\uff0c\u4ece\u800c\u4e3a\u7535\u6781\u63d0\u53d6\u8f7d\u6d41\u5b50\u7559\u51fa\u4e86\u66f4\u591a\u65f6\u95f4\u3002\u540c\u65f6\uff0c\u5728\u65e0ETL\u7684PSCs\u548c\u65e0HTL\u7684PSCs\u4e2d\uff0cJ-V\u78c1\u6ede\u90fd\u53ef\u4ee5\u5ffd\u7565\u4e0d\u8ba1\uff0c\u610f\u5473\u7740\u65e0ETL\/HTL\u5bf9\u78c1\u6ede\u6ca1\u6709\u8d1f\u9762\u5f71\u54cd\u3002\u901a\u8fc7\u4f7f\u7528\u9488\u5bf9\u5305\u542bETL\u548cHTL\u7684PSCs\u5f00\u53d1\u7684\u8fd9\u4e9b\u65b9\u6cd5\uff0c\u53ef\u4ee5\u8fdb\u4e00\u6b65\u63d0\u9ad8\u65e0HTL\/ETL\u7684PSCs\u7684\u6027\u80fd\u3002<\/p>\n<p>\u6b64\u5916\uff0c\u5927\u591a\u6570\u5df2\u62a5\u9053\u7684\u7b80\u5316\u7684PSCs\u90fd\u662f\u7528\u5c0f\u9762\u79ef\u548c\u521a\u6027\u57fa\u6750\u5236\u6210\u7684\uff0c\u4e0e\u5b9e\u9645\u5e94\u7528\u76f8\u8ddd\u751a\u8fdc\u3002\u5728\u672a\u6765\uff0c\u5982\u4f55\u6309\u6bd4\u4f8b\u653e\u5927\u7b80\u5316\u7684PSCs\u4ee5\u53ca\u5982\u4f55\u5728\u67d4\u6027\u57fa\u677f\u4e0a\u5236\u9020\u9ad8\u6027\u80fd\u7684\u7b80\u5316\u7684PSCs\u5c06\u5438\u5f15\u66f4\u591a\u7684\u7814\u7a76\u5173\u6ce8\u3002\u867d\u7136\u5f88\u591a\u7b56\u7565\u90fd\u53ef\u4ee5\u4f18\u5316\u65e0HTL\/ETL\u7684PSCs\u7684\u6027\u80fd\uff0c\u4f46\u662f\u8fd9\u4e9b\u7b56\u7565\u5927\u591a\u6570\u90fd\u63d0\u9ad8\u4e86\u5236\u9020\u590d\u6742\u6027\u548c\u6210\u672c\uff0c\u635f\u5bb3\u4e86\u7b80\u5316\u7ed3\u6784\u7684\u4f18\u52bf\u3002\u56e0\u6b64\uff0c\u5e94\u91cd\u65b0\u8bc4\u4f30\u8fd9\u4e9b\u7b56\u7565\u7684\u91cd\u8981\u6027\uff0c\u5e76\u5e94\u4ed8\u51fa\u66f4\u591a\u7684\u52aa\u529b\u6765\u8fdb\u4e00\u6b65\u7b80\u5316\u5236\u9020\u8fc7\u7a0b\u3002\u6b64\u5916\uff0c\u7a33\u5b9a\u6027\u662f\u5546\u4e1a\u5316\u7684\u53e6\u4e00\u4e2a\u975e\u5e38\u91cd\u8981\u7684\u95ee\u9898\u3002\u4e0d\u542bETL\u7684PSCs\u7684\u7a33\u5b9a\u6027\u5c1a\u7f3a\u4e4f\u8be6\u7ec6\u7684\u7814\u7a76\uff0c\u503c\u5f97\u5728\u672a\u6765\u5f15\u8d77\u66f4\u591a\u5173\u6ce8\u3002\u540c\u65f6\uff0c\u5f00\u53d1\u5c01\u88c5\u6280\u672f\u5bf9\u4e8e\u8010\u7528\u7684PSCs\u4e5f\u662f\u5fc5\u8981\u7684\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adfm.202000863\" target=\"_blank\" rel=\"noopener\">Towards Simplifying the Device Structure of High-Performance Perovskite Solar Cells<\/a><\/strong>\uff08<em>Adv. Funct. Mater.<\/em> <strong>2020<\/strong>, DOI: 10.1002\/adfm.202000863\uff09<\/p>\n<p style=\"text-align: center;\"><strong>\u901a\u8baf\u4f5c\u8005\u56e2\u961f\u4ecb\u7ecd<\/strong><\/p>\n<p><strong>\u7a0b\u6625\u8bfe\u9898\u7ec4\u56e2\u961f\uff0c\u6210\u7acb\u4e8e2013\u5e746\u6708\uff0c\u4e3b\u8981\u7814\u7a76\u9886\u57df\u4e3a\u5148\u8fdb\u6750\u6599-\u5fae\u7eb3\u7ed3\u6784\u8c03\u63a7\u4e0e\u5e94\u7528\u7b49\uff0c\u5728\u667a\u80fd\u6750\u6599\u3001\u4e8c\u7ef4\u6750\u6599\u53ca\u80fd\u6e90\u6750\u6599\u4e0e\u5668\u4ef6\u7814\u7a76\u4e0a\u53d6\u5f97\u4e86\u9886\u5148\u6210\u679c<\/strong>\u3002\u76ee\u524d\u5df2\u7ecf\u5728Advanced Functional Materials\u3001ACS Nano\u3001Chemistry of Materials\u7b49\u671f\u520a\u4e0a\u53d1\u8868\u8bba\u6587130\u591a\u7bc7\uff0c\u88ab\u5f15\u75282700\u591a\u6b21\uff0cH-index\u4e3a29\uff0c\u7814\u7a76\u6210\u679c\u88abMaterials Views\u3001Advanced Science Views\u3001\u6750\u6599\u4eba\u7b49\u62a5\u9053\uff1b\u7533\u8bf7\u53d1\u660e\u4e13\u522912\u4ef6\uff0c\u83b7\u4e13\u5229\u6388\u67432\u4ef6\u3002\u56e2\u961f\u8d1f\u8d23\u4eba\u7a0b\u6625\u62c5\u4efbJournal of Science: Advanced Materials and Devices \u7f16\u59d4\u3002\u8bfe\u9898\u7ec4\u83b7\u6279\u4e3b\u6301\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u9762\u4e0a\u9879\u76ee\u3001\u91cd\u5927\u7814\u53d1\u8ba1\u5212\u57f9\u80b2\u9879\u76ee\u548c\u7ca4\u6e2f\u8054\u5408\u521b\u65b0\u9879\u76ee\u7b49\u3002\u8bfe\u9898\u7ec4\u53d1\u8868\u592a\u9633\u80fd\u7535\u6c60\u65b9\u5411\u6587\u7ae024\u7bc7\uff0c\u5728AFM\uff0cNano Energy\uff0cJMCA\u53caSolar RRL\u4e0a\u53d1\u8868\u901a\u8baf\u4f5c\u8005\u6587\u7ae018\u7bc7, \u5728\u7a7a\u6c14\u4e2d\u7a33\u5b9a\u5236\u5907\u9ad8\u6027\u80fd\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u53ca\u53d1\u5c55\u7b80\u5f0f\u6784\u578b\u9499\u949b\u77ff\u592a\u9633\u80fd\u7535\u6c60\u65b9\u5411\u53d6\u5f97\u4e86\u4f18\u79c0\u7684\u7814\u7a76\u8fdb\u5c55\uff0c<strong>\u8bfe\u9898\u7ec4\u6b22\u8fce\u76f8\u5173\u65b9\u5411\u7684\u4f18\u79c0\u5b66\u751f\u62a5\u8003\u8bfe\u9898\u7ec4\u535a\u58eb\u4ee5\u53ca\u5e94\u8058\u4e3a\u535a\u58eb\u540e\uff0c\u5e38\u5e74\u62db\u8058<\/strong>\u3002<\/p>\n<p><strong>\u9499\u949b\u77ff\u5668\u4ef6\u65b9\u9762\u7684\u4ee3\u8868\u4f5c\u54c1\uff1a<\/strong><\/p>\n<p>1. Hui Liu, Changwen Liu, Wang Li, Weiguang Kong, Hong Chen, Haichao Zhang, Xian Zhang, Weijun Wang, Chun Cheng*, Approaching the Most Economic Preparation of Hole Transport Layer by Organic Monomolecular Strategy for Efficient Inverted Perovskite Solar Cells, <em>Solar RRL<\/em>, <strong>2020<\/strong>, https:\/\/doi.org\/10.1002\/solr.202000011<\/p>\n<p>2. Yulan Huang, Tanghao Liu, Chao Liang, Junmin Xia, Dongyang Li, Haichao Zhang, Abbas Amini, Guichuan Xing*, Chun Cheng*, Towards the Simplest Structure of High-Performance Perovskite Solar Cells, <em>Advanced Functional Materials<\/em> 3\/<strong>2020<\/strong>; DOI:10.1002\/adfm.202000863<\/p>\n<p>3. Dedi Li#; Changwen Liu#; Shi Chen; Weiguang Kong; Haichao Zhang; Deng Wang; Yan Li; Jianhui Chang; Chun Cheng*, Simplified Compact Perovskite Solar Cells with Efficiency of 19.6% via Interface Engineering, <em>Energy Environmental Materials<\/em> <strong>2020<\/strong>,0, 1-7 DOI: 10.1002\/eem2.12063<\/p>\n<p>4. Weiguang Kong, Wang Li, Changwen Liu, Hui Liu, Jun Miao, Weijun Wang, Shi Chen, Manman Hu, Dedi Li, Abbas Amini, Shaopeng Yang, Jianbo Wang, Baomin Xu*, Chun Cheng*: Organic Monomolecular Layers Enable Energy Level Matching for Efficient Hole Transporting Layer Free Inverted Perovskite Solar Cells. <em>ACS Nano<\/em> 01\/<strong>2019<\/strong>; 13(2)., DOI:10.1021\/acsnano.8b07627<\/p>\n<p>5. Wang Li, Changwen Liu, Yunlong Li, Weiguang Kong, Xingzhu Wang, Hong Chen, Baomin Xu*, Chun Cheng*: Polymer Assisted Small Molecule Hole Transport Layers Toward Highly Efficient Inverted Perovskite Solar Cells.<em> Solar RRL<\/em> 08\/<strong>2018<\/strong>; 2(11)., DOI:10.1002\/solr.201800173, <strong>the top 10 most downloaded paper in 2019 on Solar RRL<\/strong>.<\/p>\n<p><strong>\u6fb3\u95e8\u5927\u5b66\u90a2\u8d35\u5ddd\u6559\u6388\u56e2\u961f\u4e3b\u8981\u4ece\u4e8b\u4f4e\u7ef4\u7eb3\u7c73\u6750\u6599\u4e0e\u65b0\u578b\u5149\u7535\u529f\u80fd\u6750\u6599\u7684\u975e\u7ebf\u6027\u5149\u5b66\u4e0e\u8d85\u5feb\u5149\u8c31\u5b66\u7814\u7a76<\/strong>\u3002\u65e8\u5728\u63a2\u7d22\u6750\u6599\u672c\u8eab\u53ca\u5176\u5728\u5668\u4ef6\u4e2d\u7684\u5149\u7535\u5b50\u5e94\u7528\u5de5\u4f5c\u673a\u7406\u3001\u5e76\u53cd\u9988\u6307\u5bfc\u6750\u6599\u7684\u8bbe\u8ba1\u4e0e\u5668\u4ef6\u7684\u7ed3\u6784\u4f18\u5316\uff0c\u4ece\u800c\u5b9e\u73b0\u9ad8\u6027\u80fd\u5149\u7535\u5b50\u5668\u4ef6\u3002\u8fd110\u5e74\u6765\uff0c\u59cb\u7ec8\u56f4\u7ed5\u201c\u91d1\u5c5e\u5364\u5316\u7269\u9499\u949b\u77ff\u5149\u8c31\u7269\u7406\u53ca\u5668\u4ef6\u7814\u7a76\u201d\u8fd9\u4e00\u4e3b\u9898\uff0c\u4ee5\u63a2\u7a76\u91d1\u5c5e\u5364\u5316\u7269\u9499\u949b\u77ff\u5149\u7535\u673a\u5236\u4e3a\u6838\u5fc3\uff0c\u4ee5\u63d0\u9ad8\u5668\u4ef6\u6027\u80fd\u53ca\u5f00\u62d3\u5176\u65b0\u7684\u5149\u7535\u5b50\u5e94\u7528\u4e3a\u76ee\u6807\u5c55\u5f00\u5de5\u4f5c\u3002\u9488\u5bf9\u9499\u949b\u77ff\u578b\u6750\u6599\u4e0e\u5668\u4ef6\u9886\u57df\u5b58\u5728\u7684\u4e00\u4e9b\u5173\u952e\u79d1\u5b66\u95ee\u9898\uff0c\u8fd0\u7528\u98de\u79d2\u8d85\u5feb\u5149\u8c31\u624b\u6bb5\u63a2\u6d4b\u5206\u6790\u5176\u80cc\u540e\u57fa\u672c\u7684\u5149\u7269\u7406\u53ca\u5149\u5316\u5b66\u8bf1\u56e0\uff0c\u5728\u7406\u89e3\u8fd9\u4e9b\u8bf1\u56e0\u8fc7\u7a0b\u7684\u57fa\u7840\u4e0a\uff0c\u5bf9\u9499\u949b\u77ff\u6750\u6599\u7684\u7ef4\u5ea6\u3001\u7ed3\u6676\u8fc7\u7a0b\u3001\u5fae\u7eb3\u7ed3\u6784\u5f62\u8c8c\u3001\u8584\u819c\u5f62\u8c8c\u53ca\u5668\u4ef6\u80fd\u5e26\u5de5\u7a0b\u7b49\u8fdb\u884c\u8c03\u63a7\u4ee5\u514b\u670d\u8fd9\u4e9b\u95ee\u9898\u3002\u5171\u53d1\u8868SCI\u8bba\u6587140\u4f59\u7bc7\uff0c\u5305\u62ec\u4e00\u4f5c\u6216\u901a\u8baf\u7684Science\uff0cNature Materials\uff0cNature Communications\uff0cAdvanced Materials\uff0cNano Energy\uff0cACS Nano\u7b49\uff0c\u8bba\u6587\u88ab\u5f1512500\u4f59\u6b21\u3002<strong>\u6b22\u8fce\u76f8\u5173\u65b9\u5411\u7684\u4f18\u79c0\u5b66\u751f\u7533\u8bf7\u8bfe\u9898\u7ec4\u535a\u58eb\u4ee5\u53ca\u5e94\u8058\u4e3a\u535a\u58eb\u540e\uff0c\u4f18\u79c0\u535a\u58eb\u751f\u53ef\u83b7\u5f97\u56db\u5e74\u5956\u5b66\u91d1100\u4e07\u6fb3\u95e8\u5e01\uff0c\u4f18\u79c0\u535a\u58eb\u540e\u53ef\u83b7\u5f97\u4e24\u5e74\u85aa\u91d1100\u4e07\u6fb3\u95e8\u5e01\uff0c\u5e38\u5e74\u62db\u8058<\/strong>\u3002<\/p>\n<p>\u672c\u6587\u7531CQR\u7f16\u8bd1\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1\uff1atougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenvip.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011 \u4f17\u6240\u5468\u77e5\uff0c\u592a\u9633\u80fd\u4f5c\u4e3a\u4e00\u79cd\u6e05\u6d01\u4e14\u53d6\u4e4b\u4e0d\u5c3d\u7684\u80fd\u6e90\uff0c\u662f\u5e94\u5bf9\u5168\u7403\u53d8\u6696\u548c\u80fd\u6e90\u5371\u673a\u7684\u7406\u60f3\u89e3\u51b3\u65b9\u6848\u3002\u56e0\u6b64\uff0c\u79d1\u5b66\u5bb6\u4eec\u53d1\u660e\u4e86\u7845\u3001\u65e0\u673a\u8584\u819c\u3001\u67d3\u6599\u654f\u5316\u3001\u6709\u673a\u8584\u819c\u3001\u91cf\u5b50\u70b9&#8230;<\/p>\n","protected":false},"author":7770,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[533],"tags":[3888],"class_list":["post-202788","post","type-post","status-publish","format-standard","hentry","category-zongshu","tag-pscs"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/202788"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7770"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=202788"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/202788\/revisions"}],"predecessor-version":[{"id":203152,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/202788\/revisions\/203152"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=202788"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=202788"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=202788"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}