{"id":203301,"date":"2020-06-08T06:51:28","date_gmt":"2020-06-07T22:51:28","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=203301"},"modified":"2020-06-07T23:07:37","modified_gmt":"2020-06-07T15:07:37","slug":"%e5%a4%a9%e6%b4%a5%e5%a4%a7%e5%ad%a6%e7%ba%b3%e7%b1%b3%e5%8f%8a%e5%a4%8d%e5%90%88%e6%9d%90%e6%96%99%e8%af%be%e9%a2%98%e7%bb%84nature-communications%ef%bc%9a%e7%b2%89%e6%9c%ab%e5%86%b6%e9%87%91","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=203301","title":{"rendered":"\u5929\u6d25\u5927\u5b66\u7eb3\u7c73\u53ca\u590d\u5408\u6750\u6599\u8bfe\u9898\u7ec4Nature Communications\uff1a\u7c89\u672b\u51b6\u91d1\u6cd5\u5236\u5907\u4e09\u7ef4\u7c7b\u77f3\u58a8\u70ef\u7f51\u7edc\u589e\u5f3a\u94dc\u57fa\u590d\u5408\u6750\u6599"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u4e8c\u7ef4\u8702\u7a9d\u7f51\u7edc\u7ed3\u6784\u7684\u77f3\u58a8\u70ef\u6750\u6599\u7531\u4e8e\u5177\u6709\u72ec\u7279\u548c\u8bf1\u4eba\u7684\u529b\u5b66\u6027\u80fd\u5982\u8d85\u9ad8\u5f3a\u5ea6\u548c\u5f39\u6027\u6a21\u91cf\uff0c\u9ad8\u7684\u7535\u5b50\u8fc1\u79fb\u7387\u548c\u70ed\u5bfc\u7387\u4ee5\u53ca\u5927\u7684\u6bd4\u8868\u9762\u79ef\uff0c\u6709\u671b\u88ab\u5e94\u7528\u4e3a\u6811\u8102\u57fa\u3001\u9676\u74f7\u57fa\u548c\u91d1\u5c5e\u57fa\u590d\u5408\u6750\u6599\u7684\u589e\u5f3a\u4f53\uff0c\u4ee5\u671f\u83b7\u5f97\u5177\u6709\u975e\u51e1\u529b\u5b66\u6027\u80fd\u3001\u5bfc\u7535\uff08\u5bfc\u70ed\uff09\u6027\u80fd\u7684\u5168\u65b0\u590d\u5408\u6750\u6599\u3002\u7136\u800c\uff0c\u7531\u4e8e\u4e8c\u7ef4\u77f3\u58a8\u70ef\u6613\u5728\u590d\u5408\u6750\u6599\u4e2d\u5806\u53e0\u5bfc\u81f4\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\uff08GNSs\uff09\u56e2\u805a\u5e76\u5f15\u53d1GNSs\u4e0e\u57fa\u4f53\u4e4b\u95f4\u63a5\u89e6\u7535\u963b\uff08\u70ed\u963b\uff09\u589e\u52a0\u7684\u74f6\u9888\u95ee\u9898\uff0c\u5176\u81ea\u8eab\u7684\u4f18\u5f02\u6027\u80fd\u65e0\u6cd5\u5145\u5206\u53d1\u6325\uff0c\u7531\u6b64\u5bfc\u81f4\u5728\u76ee\u524d\u5236\u5907\u7684\u590d\u5408\u6750\u6599\u4e2d\uff0c\u529b\u5b66\u548c\u5bfc\u7535\uff08\u5bfc\u70ed\uff09\u6027\u80fd\u7684\u589e\u5f3a\u6548\u7387\u4e0e\u7406\u8bba\u503c\u6709\u8f83\u5927\u504f\u5dee\u3002<\/p>\n<p>\u968f\u7740\u76f8\u5173\u7814\u7a76\u7684\u6df1\u5165\u5f00\u5c55\uff0c\u4eba\u4eec\u9010\u6e10\u610f\u8bc6\u5230\u4e3a\u4e86\u5145\u5206\u53d1\u6325\u77f3\u58a8\u70ef\u7684\u6cbf\u9762\u5185\u65b9\u5411\u7684\u4f18\u5f02\u6027\u80fd\u4ee5\u4fc3\u8fdb\u5176\u590d\u5408\u6750\u6599\u7684\u5b9e\u9645\u5e94\u7528\uff0c\u5bf9\u4e8e\u77f3\u58a8\u70ef\u590d\u5408\u6750\u6599\u5728\u4ece\u539f\u5b50\u5230\u5b8f\u89c2\u7684\u591a\u5c3a\u5ea6\u6784\u578b\u8bbe\u8ba1\u81f3\u5173\u91cd\u8981\u3002\u4e0e\u4e8c\u7ef4\u77f3\u58a8\u70ef\u76f8\u6bd4\uff0c\u4ee5\u6c14\u51dd\u80f6\/\u6d77\u7ef5\u6216\u6ce1\u6cab\u72b6\u7684\u4e09\u7ef4\u77f3\u58a8\u70ef\u7a33\u5b9a\u9aa8\u67b6\u7ed3\u6784\u53ef\u4ee5\u6709\u6548\u89e3\u51b3GNSs\u7684\u56e2\u805a\u95ee\u9898\u3002\u6b64\u5916\uff0c \u4e09\u7ef4\u7f51\u7edc\u6784\u578b\u8fd8\u53ef\u4ee5\u6709\u6548\u964d\u4f4e\u4e8c\u7ef4\u77f3\u58a8\u70ef\u7247\u5c42\u95f4\u7684\u63a5\u89e6\u7535\u963b\uff08\u70ed\u963b\uff09\uff0c\u4ece\u800c\u4fc3\u8fdb\u7535\u5b50\u548c\u58f0\u5b50\u7684\u4f20\u8f93\u3002\u76ee\u524d\uff0c\u4e09\u7ef4\u77f3\u58a8\u70ef\u7684\u5236\u5907\u6280\u672f\u53ef\u4ee5\u603b\u7ed3\u4e3a<strong>\u9aa8\u67b6<\/strong><strong>&#8211;<\/strong><strong>\u586b\u5145\u6cd5\uff08\u65b9\u6848<\/strong><strong>\u2160<\/strong><strong>\uff09<\/strong>\u548c<strong>\u77f3\u58a8\u70ef\u5305\u8986<\/strong><strong>&#8211;<\/strong><strong>\u7c89\u672b\u70e7\u7ed3\u6cd5\uff08\u65b9\u6848<\/strong><strong>\u2161<\/strong><strong>\uff09<\/strong>\u4e24\u7c7b\u65b9\u6cd5\uff08\u5177\u4f53\u53ef\u4ee5\u53c2\u7167\u672c\u8bfe\u9898\u7ec4\u6700\u8fd1\u53d1\u8868\u7684\u7efc\u8ff0\u8bba\u6587\uff1aThe superior mechanical and physical properties of nanocarbon reinforced bulk composites achieved by architecture design \u2013 A review, Progress in Materials Science, 2020, 113, 100672\uff09\u3002\u4f46\u5728\u76ee\u524d\uff0c\u5728\u91d1\u5c5e\u57fa\u590d\u5408\u6750\u6599\uff08MMCs\uff09\u4e2d\u5b9e\u73b0\u4e09\u7ef4\u7f51\u7edc\u589e\u5f3a\u4ecd\u7136\u6781\u5177\u6311\u6218\u3002\u4ee5\u91d1\u5c5e\u94dc\u4e3a\u4f8b\uff0c\u65b9\u6848\u2160\u65b9\u6cd5\u9c9c\u6709\u62a5\u9053\uff0c\u4e3b\u8981\u539f\u56e0\u4e3a\u77f3\u58a8\u70ef\u4e0e\u94dc\u4e4b\u95f4\u754c\u9762\u4e0d\u6da6\u6e7f\uff08\u63a5\u89e6\u89d2\u7ea6\u4e3a140\u00b0\uff09\u3001\u8d85\u8fc7\u94dc\u7194\u70b9\u7684\u9ad8\u5236\u5907\u6e29\u5ea6\uff08&gt;1083\u00b0C\uff09\u5f15\u53d1\u4e09\u7ef4\u77f3\u58a8\u70ef\u9884\u5236\u4f53\u8868\u9762\u7f3a\u9677\u589e\u591a\u3001\u4e09\u7ef4\u77f3\u58a8\u70ef\u9884\u5236\u4f53\u7684\u6709\u6548\u5f39\u6027\u6a21\u91cf\u8f83\u4f4e\u5bfc\u81f4\u7ed3\u6784\u574d\u584c\u7b49\u3002\u800c\u65b9\u6848\u2161\u5219\u4e3a\u4e09\u7ef4\u77f3\u58a8\u70ef\u589e\u5f3a\u91d1\u5c5e\u63d0\u4f9b\u4e86\u8f83\u4e3a\u53ef\u884c\u7684\u5236\u5907\u6761\u4ef6\u3002\u4f46\u662f\uff0c\u5bf9\u4e8e\u76ee\u524dMMCs\u4e2d\u4f7f\u7528\u8f83\u591a\u7684\u8fd8\u539f\u6c27\u5316\u77f3\u58a8\u70ef\uff08RGO\uff09\u589e\u5f3a\u4f53\uff0c\u5728\u7c89\u672b\u51b6\u91d1\u5236\u5907\u6e29\u5ea6\u7a97\u53e3\uff08500-1000\u00b0C\uff09\u5185\u7f3a\u4e4f\u6709\u6548\u7684\u7247\u5c42\u8fde\u63a5\u673a\u5236\u3002\u56e0\u6b64\uff0c\u6b64\u65b9\u6848\u4e0b\u7684\u5173\u952e\u79d1\u5b66\u95ee\u9898\u5728\u4e8e\u5982\u4f55\u5b9e\u73b0\u4e8c\u7ef4\u77f3\u58a8\u70ef\u7247\u5c42\u7684\u6709\u6548\u8fde\u63a5\u8fdb\u800c\u5728\u91d1\u5c5e\u57fa\u4f53\u5185\u90e8\u6784\u7b51\u4e3a\u8fde\u7eed\u7684\u7f51\u7edc\u72b6\u62d3\u6251\u7ed3\u6784\u4ee5\u5b9e\u73b0\u4e09\u7ef4\u77f3\u58a8\u70ef\u7684\u4f18\u5f02\u529b\u5b66\u548c\u7269\u7406\u6027\u80fd\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u5929\u6d25\u5927\u5b66\u7eb3\u7c73\u53ca\u590d\u5408\u6750\u6599\u8bfe\u9898\u7ec4<\/strong>\u5f00\u53d1\u4e86\u4e00\u79cd\u5168\u65b0\u7684\u7c89\u672b\u51b6\u91d1\u5236\u5907\u4e09\u7ef4\u7c7b\u77f3\u58a8\u70ef\u7f51\u7edc-\u94dc\uff083D-GLNN\/Cu\uff09\u590d\u5408\u6750\u6599\u3002\u4e3b\u8981\u7ed3\u5408\u4e86\u5728\u7403\u72b6\u94dc\u7c89\u8868\u9762\u91c7\u7528\u5e38\u538b\u5feb\u901f\u52a0\u70ed\u5904\u7406\uff08RTA\uff09\u751f\u957f\u7c7b\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\uff08GLNs\uff09\u5e76\u901a\u8fc7\u5728\u540e\u7eed\u53cd\u5e94\u70ed\u538b\u70e7\u7ed3\u8fc7\u7a0b\u4e2dGLNs\u5728\u70ed\u5e94\u529b\u7684\u4f5c\u7528\u4e0b\u76f8\u4e92\u710a\u63a5\u6210\u4e3a\u8fde\u7eed\u7684\u4e09\u7ef4\u7f51\u7edc\u7ed3\u6784\uff0c\u8fdb\u4e00\u6b65\u91c7\u7528\u70ed\u8f67\u5b9e\u73b0\u66f4\u9ad8\u7a0b\u5ea6\u7684\u5757\u4f53\u81f4\u5bc6\u5316\u3002\u672c\u6587\u4ece\u5b9e\u9a8c\u548c\u5206\u5b50\u52a8\u529b\u5b66\u7406\u8bba\u8ba1\u7b97\u65b9\u9762\uff08\u4e0e\u534e\u4e2d\u79d1\u6280\u5927\u5b66<strong>\u6731\u798f\u9f99\u6559\u6388<\/strong>\u5408\u4f5c\uff09\u90fd\u8bc1\u5b9e\u4e86\u8fde\u7eed\u7f51\u7edc\u7ed3\u6784\u8f83\u4e8c\u7ef4\u5f25\u6563\u5206\u5e03\u77f3\u58a8\u70ef\u5177\u6709\u66f4\u9ad8\u7684\u754c\u9762\u526a\u5207\u5e94\u529b\uff0c\u4ece\u800c\u63d0\u9ad8\u8f7d\u8377\u8f6c\u79fb\u5f3a\u5316\u673a\u5236\u548c\u589e\u5f3a\u6548\u7387\uff1b\u4e0e\u57fa\u4f53\u5f62\u6210\u7684\u53cc\u76f8\u8fde\u7eed\u7f51\u7edc\u7ed3\u6784\u964d\u4f4e\u4e86\u754c\u9762\u5904\u7684\u7535\u5b50\u6563\u5c04\u5e76\u4e8e\u57fa\u4f53\u5185\u90e8\u6210\u529f\u6784\u7b51\u7535\u5b50\u8fde\u7eed\u4f20\u8f93\u901a\u9053\u3002\u7ed3\u679c\u663e\u793a\uff0c3D-GLNN\/Cu \u5c55\u793a\u51fa\u4f18\u5f02\u7684\u529b\u5b66\u3001\u5bfc\u7535\u548c\u5bfc\u70ed\u6027\u80fd\uff0c\u5177\u6709\u5e7f\u6cdb\u7684\u5e94\u7528\u6f5c\u529b\u3002\u6b64\u5916\uff0c\u8fd9\u79cd\u4fbf\u6377\u548c\u6613\u653e\u5927\u7684\u5236\u5907\u65b9\u6cd5\u4e0d\u53d7\u7194\u4f53\u76f8\u5173\u5236\u5907\u65b9\u6cd5\u7684\u6761\u4ef6\u5236\u7ea6\uff0c\u4e3a\u4e8c\u7ef4\u7ed3\u6784\u5355\u5143\u7ec4\u88c5\u6210\u4e09\u7ef4\u7f51\u7edc\u7ed3\u6784\u53ca\u5176\u5728\u91d1\u5c5e\u57fa\u590d\u5408\u6750\u6599\u4e2d\u7684\u5e94\u7528\u63d0\u4f9b\u4e86\u5168\u65b0\u9014\u5f84\u3002<strong>\u8be5\u6210\u679c\u4ee5\u9898\u4e3a<\/strong><strong>\u201cA powder-metallurgy-based strategy toward three-dimensional graphene-like network for reinforcing copper matrix composites\u201d<\/strong><strong>\u6700\u8fd1\u53d1\u8868\u5728<\/strong><strong>Nature Communications<\/strong><strong>\u671f\u520a\u4e0a\u3002<\/strong><\/p>\n<p><strong>\u3010\u56fe\u6587\u89e3\u6790\u3011<\/strong><\/p>\n<p><strong>Figure 1 <\/strong><strong>\u5236\u5907\u5de5\u827a\u793a\u610f\u56fe<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-203303\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/1-13.jpg\" alt=\"\" width=\"827\" height=\"343\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/1-13.jpg 827w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/1-13-300x124.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/1-13-768x319.jpg 768w\" sizes=\"(max-width: 827px) 100vw, 827px\" \/><\/p>\n<p><strong>a<\/strong> \u94dc\u7c89\u8868\u9762\u5305\u8986\u8517\u7cd6\u524d\u9a71\u4f53\uff1b <strong>b<\/strong> \u6df7\u5408\u524d\u9a71\u4f53\u7ecfRTA\u8fc7\u7a0b\u751f\u957fGLNs\uff1b<strong>c<\/strong> \u771f\u7a7a\u70ed\u538b\u70e7\u7ed3\u8fc7\u7a0b\u4e2dGLNs\u76f8\u4e92\u8fde\u63a5\u4e3a\u8fde\u7eed\u7f51\u7edc\u7ed3\u6784\uff1b<strong>d<\/strong> \u70ed\u8f67\u83b7\u5f97\u76843D-GLNN\/Cu\u81f4\u5bc6\u5757\u4f53\u6750\u6599\u3002<\/p>\n<p><strong>Figure 2 <\/strong><strong>\u590d\u5408\u7c89\u672b\u548c\u5757\u4f53\u6750\u6599\u7684\u8868\u5f81\u3002<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-203304\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/2-13.jpg\" alt=\"\" width=\"796\" height=\"599\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/2-13.jpg 796w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/2-13-300x226.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/2-13-768x578.jpg 768w\" sizes=\"(max-width: 796px) 100vw, 796px\" \/><\/p>\n<p><strong>a,b,<\/strong> \u4f4e\u500dSEM\u4e0b\u94dc\u7c89\u8868\u9762\u751f\u957fGLNs\u540e\u7684\u758f\u677e\u5806\u79ef\u7403\u4f53\u7ed3\u6784<strong>(a)<\/strong>\uff0c\u9ad8\u500dSEM\u4e0b\u94dc\u7c89\u8868\u9762\u5747\u5300\u5305\u8986GLNs\u7684\u5178\u578b\u5f62\u8c8c<strong>(b)<\/strong>\uff1b<strong>c,d, <\/strong>\u94dc\u7c89\u523b\u8680\u540eGLNs\u7684TEM\u7167\u7247<strong>(c)<\/strong>, \u53ca\u5176\u8fb9\u7f18\u4f4d\u7f6e\u7684HRTEM\u7167\u7247\uff1b<strong>e,f, <\/strong>\u70ed\u538b\u70e7\u7ed3\u60013D-GLNN\/Cu\u8868\u9762\u8150\u8680\u540e\u66b4\u9732\u51fa\u76843D-GLNN\u7684SEM\u7167\u7247<strong>(e)<\/strong>\u548c\u57fa\u4f53\u523b\u8680\u540e\u7684TEM\u7167\u7247<strong>(f)<\/strong>\uff1b<strong>g<\/strong> 3D-GLNN\u7684\u5178\u578bY\u578b\u8fde\u63a5\u4f4d\u7f6eHRTEM\u7167\u7247\uff1b<strong>h,k,<\/strong> FIB\u4e09\u7ef4\u91cd\u6784\u83b7\u5f97\u7684\u70ed\u538b\u6001<strong>(h)<\/strong>\u548c\u70ed\u8f67\u6001<strong>(k)<\/strong>3D-GLNN\u5728\u94dc\u57fa\u4f53\u4e2d\u7684\u5206\u5e03\u6a21\u578b\uff1b<strong>i,j. <\/strong>\u70ed\u8f67\u60013D-GLNN\/Cu\u8868\u9762\u8150\u8680\u540eTD-RD\u9762<strong>(i)<\/strong>\u548cND-RD\u9762<strong>(j)<\/strong>\u7684SEM\u7167\u7247\u3002<\/p>\n<p><strong>Figure 3<\/strong><strong>\u70ed\u538b\u8fc7\u7a0b\u4e2d\u7684\u7ed3\u6784\u6f14\u53d8<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-203305\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/3-13.jpg\" alt=\"\" width=\"833\" height=\"510\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/3-13.jpg 833w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/3-13-300x184.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/3-13-768x470.jpg 768w\" sizes=\"(max-width: 833px) 100vw, 833px\" \/><\/p>\n<p><strong>a-d<\/strong> \u5757\u4f53\u590d\u5408\u6750\u6599\u4e2d\u8868\u9762\u94dc\u57fa\u4f53\u8150\u8680\u540e\u589e\u5f3a\u589e\u5f3a\u76f8\u7684\u5f62\u8c8cSEM\u7167\u7247\uff1a<strong>(a)<\/strong> 800-800-50\uff0c<strong>(b)<\/strong> 800-800-0\uff0c<strong>(c)<\/strong> 800-400-50\u548c<strong>(d)<\/strong> 400-800-50\uff1b<strong>e,f, <\/strong>\u590d\u5408\u7c89\u672b\uff08400-RTA\u548c800-RTA\uff09\u548c\u590d\u5408\u5757\u4f53\uff08800-800-50\uff0c800-800-0\uff0c800-400-50\u548c400-800-50\uff09XPS\u8c31\u56fe\u4e2dC1s\u7684\u7cbe\u7ec6\u8c31<strong>(e)<\/strong>\u548c\u62c9\u66fc\u5149\u8c31<strong>(f)<\/strong>\uff1b<strong>g<\/strong> 800-800-50\u5757\u4f53\u8868\u97623D-GLNN\u7684G\u5cf0\uff081580 cm<sup>-1<\/sup>\uff09\u62c9\u66fc\u9762\u626b\u3002<\/p>\n<p><strong>Figure 4<\/strong><strong>\u7c7b\u77f3\u58a8\u70ef\u710a\u63a5\u673a\u5236\u7684\u5206\u5b50\u52a8\u529b\u5b66\u6a21\u62df<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-203306\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/4-15.jpg\" alt=\"\" width=\"844\" height=\"469\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/4-15.jpg 844w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/4-15-300x167.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/4-15-768x427.jpg 768w\" sizes=\"(max-width: 844px) 100vw, 844px\" \/><\/p>\n<p><strong>a<\/strong>\u4e24\u7ec4\u9762-\u9762\u76f8\u5bf9\u76843LGs\/Cu\uff086LGs\/Cu\uff09\u7684\u539f\u5b50\u7ed3\u6784\u6a21\u578b\uff1b<strong>b<\/strong> \u4e0d\u540c\u6e29\u5ea6\u4e0b\uff08493K\uff0c693K\uff0c893K\u548c1093K\uff09\u57286LGs\/Cu\u6a21\u578b\u4e2d\u95f4\u4f4d\u7f6eY-Z\u5355\u5c42\u5207\u7247\u5185\u6cbfZ\u65b9\u5411\u5e94\u529b\u4e91\u56fe\uff1b <strong>c,d, <\/strong>6LGs<strong>(c)<\/strong>\u548c6LGs\/Cu<strong>(d)<\/strong>\u6a21\u578b\u4e2d\u4e0d\u540c\u6e29\u5ea6\u4e0b\u7684\u952e\u957f\u7edf\u8ba1\u7ed3\u679c\uff1b<strong>e <\/strong>6LGs\u548c6LGs\/Cu\u6a21\u578b\u4e2d1LG\u4e0d\u540c\u6e29\u5ea6\u4e0b\u7684\u62d4\u51fa\u5e94\u529b\u7ed3\u679c\u3002<\/p>\n<p><strong>\u56fe<\/strong><strong>5 <\/strong><strong>\u5178\u578b\u7ec4\u7ec7\u548c\u6027\u80fd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-203307\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/5-8.jpg\" alt=\"\" width=\"797\" height=\"660\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/5-8.jpg 797w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/5-8-300x248.jpg 300w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/5-8-768x636.jpg 768w\" sizes=\"(max-width: 797px) 100vw, 797px\" \/><\/p>\n<p><strong>a<\/strong> \u70ed\u8f67\u60013D-GLNN\/Cu\u4e09\u4e2a\u4e0d\u540c\u65b9\u5411\u7684EBSD\u6676\u7c92\u5c3a\u5bf8\u53ca\u53d6\u5411\u5206\u5e03\u56fe\uff1b<strong>b<\/strong> 3D-GLNN\/Cu\u7684TEM\u660e\u573a\u50cf\u7167\u7247\uff1b<strong>c,d,<\/strong> 3D-GLNN\/Cu\u7684STEM\u660e\u573a\u50cf<strong>(c)<\/strong>\u548c\u5bf9\u5e94\u7684HRTEM\u7167\u7247\uff1b<strong>e<\/strong> \u7eaf\u94dc\u3001RGO\/Cu\u548c3D-GLNN\/Cu\u7684\u62c9\u4f38\u529b\u5b66\u6027\u80fd\u66f2\u7ebf\uff1b<strong>f<\/strong>\u7eaf\u94dc\u3001RGO\/Cu\u548c3D-GLNN\/Cu\u7684\u62c9\u4f38\u529b\u5b66\u6027\u80fd\u5bf9\u6bd4\u67f1\u72b6\u56fe\uff1b<strong>g<\/strong> \u4e0d\u540c\u6784\u578b\u78b3\u7eb3\u7c73\u76f8\u589e\u5f3a\u94dc\u57fa\u590d\u5408\u7684\u65ad\u88c2\u5ef6\u4f38\u7387\u4fdd\u6301\u7387\u4e0e\u589e\u5f3a\u6548\u7387\u6570\u636e\u5bf9\u6bd4\uff1b<strong>h<\/strong> \u7eaf\u94dc\u3001RGO\/Cu\u548c3D-GLNN\/Cu\u7684\u9762\u5185\u70ed\u5bfc\u7387\u5bf9\u6bd4\uff1b<strong>i<\/strong> \u5ba4\u6e29\u548c300\u00b0C\u6e29\u5ea6\u4e0b\u7eaf\u94dc\u3001RGO\/Cu\u548c3D-GLNN\/Cu\u7684\u70ed\u5bfc\u7387\u6570\u636e\u5bf9\u6bd4\uff1b<strong>j<\/strong> \u70ed\u5bfc\u7387\u589e\u5f3a\u6548\u7387\u548c\u589e\u5f3a\u76f8\u542b\u91cf\u5173\u7cfb\u5bf9\u6bd4\u56fe\u3002<\/p>\n<p><strong>Figure 6 <\/strong><strong>\u4e09\u7ef4\u77f3\u58a8\u70ef<\/strong><strong>\/<\/strong><strong>\u94dc\u548c\u4e8c\u7ef4\u77f3\u58a8\u70ef<\/strong><strong>\/<\/strong><strong>\u540c\u529b\u5b66\u673a\u5236\u5bf9\u6bd4<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-203308\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/6-6.jpg\" alt=\"\" width=\"756\" height=\"526\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/6-6.jpg 756w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/06\/6-6-300x209.jpg 300w\" sizes=\"(max-width: 756px) 100vw, 756px\" \/><\/p>\n<p><strong>a<\/strong> RGO\/Cu\u4e0e3D-GLNN\/Cu\u7684\u539f\u4f4d\u62c9\u4f38\u66f2\u7ebf\u675c\u6bd4\uff1b<strong>b,c,<\/strong> RGO\/Cu<strong>(b)<\/strong>\u548c3D-GLNN\/Cu<strong>(c)<\/strong>\u7684\u539f\u4f4d\u62c9\u4f38\u6837\u54c1\u65ad\u88c2\u88c2\u7eb9\u5b8f\u89c2\u5f62\u8c8cSEM\u7167\u7247\uff1b<strong>d <\/strong>RGO\/Cu \u62c9\u4f38\u8fc7\u7a0b<strong>(C)<\/strong>\u9636\u6bb5\u4ece\u57fa\u4f53\u4e2d\u5265\u79bb\u5f62\u8c8c\uff1b<strong>e,f, <\/strong>\u5178\u578b\u7684\u7531\u77f3\u58a8\u70ef\/\u94dc\u4e92\u9501\u7ed3\u6784<strong>(e)<\/strong>\u548c3D-GLNN<strong>(f)<\/strong>\u5bfc\u81f4\u7684\u88c2\u7eb9\u6865\u63a5SEM\u7167\u7247\uff1b<strong>g,h, <\/strong>2D-G\/Cu<strong>(g)<\/strong>\u548c3D-G\/Cu<strong>(h)<\/strong>\u7684\u5206\u5b50\u52a8\u529b\u5b66\u6a21\u62df\u539f\u5b50\u6a21\u578b\uff1b<strong>i,j, <\/strong>2D-G\/Cu<strong>(i)<\/strong>\u548c3D-G\/Cu<strong>(j)<\/strong>\u7684\u62d4\u51fa\u529b-\u4f4d\u79fb\u66f2\u7ebf\uff1b<strong>k<\/strong> 3D-G\/Cu\u6a21\u578b\u4e2d3D-G\u62d4\u51fa\u8fc7\u7a0b\u622a\u56fe\u3002<\/p>\n<p><strong>\u3010\u603b\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u5de5\u4f5c\u5229\u7528\u57fa\u4f53\u548c\u589e\u5f3a\u4f53\u4e4b\u95f4\u7531\u4e8e\u70ed\u81a8\u80c0\u7cfb\u6570\u5dee\u5f02\u5bfc\u81f4\u7684\u5185\u5e94\u529b\u6548\u5e94\uff0c\u5e76\u91c7\u7528\u4fbf\u6377\u3001\u53ef\u6269\u5927\u5316\u7684\u70ed\u538b\u548c\u70ed\u8f67\u5de5\u827a\u5b9e\u73b0\u7c7b\u77f3\u58a8\u70ef\u7ed3\u6784\u7247\u5c42\u7684\u7d27\u5bc6\u710a\u63a5\u5e76\u6784\u7b51\u8fde\u7eed\u7684\u4e09\u7ef4\u7c7b\u77f3\u58a8\u70ef\u7f51\u7edc\/\u94dc\u590d\u5408\u6750\u6599\u3002\u5b9e\u9a8c\u4e0e\u5206\u5b50\u52a8\u529b\u5b66\u8ba1\u7b97\u90fd\u8868\u660e\u70ed\u5e94\u529b\u5bf9\u77f3\u58a8\u70ef\u7247\u5c42\u710a\u63a5\u53ca\u7f51\u7edc\u6784\u578b\u7684\u5f62\u6210\u5177\u6709\u81f3\u5173\u91cd\u8981\u7684\u4f5c\u7528\u3002\u66f4\u4e3a\u91cd\u8981\u7684\u662f\uff0c\u672c\u6587\u9996\u6b21\u8bc1\u5b9e\u4e86\u7f51\u7edc\u6784\u578b\u53ef\u4ee5\u6709\u6548\u63d0\u9ad8\u77f3\u58a8\u70ef\/\u94dc\u4e4b\u95f4\u7684\u754c\u9762\u526a\u5207\u5e94\u529b\uff08\u8f83\u4e8c\u7ef4\u77f3\u58a8\u70ef\/\u94dc\u63d0\u5347\u4e24\u500d\u4ee5\u4e0a\uff09\u4ece\u800c\u4fc3\u8fdb\u4e86\u8f7d\u8377\u8f6c\u79fb\u5f3a\u5316\u673a\u5236\uff1b\u540c\u65f6\uff0c\u7ed3\u679c\u8868\u660e\u5728\u94dc\u57fa\u4f53\u5185\u6784\u7b51\u8fde\u7eed\u7684\u77f3\u58a8\u70ef\u7f51\u7edc\u8f83\u4e8c\u7ef4\u77f3\u58a8\u70ef\u4e0d\u4ec5\u53ef\u4ee5\u6709\u6548\u63d0\u9ad8\u590d\u5408\u6750\u6599\u7684\u529b\u5b66\u6027\u80fd\uff08\u5f3a\u5ea6\u548c\u5851\u97e7\u6027\uff09\uff0c\u4e5f\u80fd\u63d0\u9ad8\u5bfc\u7535\u548c\u5bfc\u70ed\u7269\u7406\u6027\u80fd\u3002\u6b64\u5916\uff0c\u672c\u6587\u7684\u5236\u5907\u7b56\u7565\u53ef\u4ee5\u62d3\u5c55\u5230\u5236\u5907\u5176\u4ed6\u4e8c\u7ef4\u7ed3\u6784\u57fa\u5143\uff08\u5982\u516d\u65b9\u6c2e\u5316\u787c\u3001\u8fc7\u6e21\u91d1\u5c5e\u4e8c\u7ef4\u786b\u5316\u7269\u548c\u6c27\u5316\u7269\u7b49\uff09\u7ec4\u6210\u7684\u4e09\u7ef4\u7f51\u7edc\u5e76\u4e14\u5236\u5907\u5176\u589e\u5f3a\u7684\u91d1\u5c5e\u57fa\u590d\u5408\u6750\u6599\uff08\u94dc\u3001\u9541\u3001\u94dd\u3001\u949b\u7b49\uff09\uff0c\u8fdb\u800c\u6709\u671b\u4fc3\u8fdb\u8fd9\u7c7b\u6750\u6599\u7684\u7ed3\u6784\u4e0e\u529f\u80fd\u5316\u5e94\u7528\u3002<\/p>\n<p>\u8bba\u6587\u7b2c\u4e00\u4f5c\u8005\u4e3a\u5f20\u7fd4 \u535a\u58eb\uff0c\u534e\u4e2d\u79d1\u6280\u5927\u5b66<strong>\u6731\u798f\u9f99\u6559\u6388<\/strong>\u548c\u5929\u6d25\u5927\u5b66<strong>\u4f55\u6625\u5e74\u6559\u6388<\/strong>\u4e3a\u5171\u540c\u901a\u8baf\u4f5c\u8005\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1aA powder-metallurgy-based strategy toward three-dimensional graphene-like network for reinforcing copper matrix composites, Nature Communications,<strong>2020<\/strong>, 11: 2775\u3002<\/p>\n<p>DOI\uff1ahttps:\/\/doi.org\/10.1038\/s41467-020-16490-4<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u4e8c\u7ef4\u8702\u7a9d\u7f51\u7edc\u7ed3\u6784\u7684\u77f3\u58a8\u70ef\u6750\u6599\u7531\u4e8e\u5177\u6709\u72ec\u7279\u548c\u8bf1\u4eba\u7684\u529b\u5b66\u6027\u80fd\u5982\u8d85\u9ad8\u5f3a\u5ea6\u548c\u5f39\u6027\u6a21\u91cf\uff0c\u9ad8\u7684\u7535\u5b50\u8fc1\u79fb\u7387\u548c\u70ed\u5bfc\u7387\u4ee5\u53ca\u5927\u7684\u6bd4\u8868\u9762\u79ef\uff0c\u6709\u671b\u88ab\u5e94\u7528\u4e3a\u6811\u8102\u57fa\u3001\u9676\u74f7\u57fa\u548c\u91d1\u5c5e&#8230;<\/p>\n","protected":false},"author":2,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-203301","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/203301"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/2"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=203301"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/203301\/revisions"}],"predecessor-version":[{"id":203309,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/203301\/revisions\/203309"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=203301"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=203301"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=203301"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}