{"id":205758,"date":"2020-07-21T06:30:35","date_gmt":"2020-07-20T22:30:35","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=205758"},"modified":"2020-07-20T20:40:22","modified_gmt":"2020-07-20T12:40:22","slug":"%e3%80%90%e6%8a%95%e7%a8%bf%e3%80%91%e5%b9%bf%e4%b8%9c%e7%9f%b3%e6%b2%b9%e5%8c%96%e5%b7%a5%e5%ad%a6%e9%99%a2cjce%ef%bc%9a%e7%94%a8%e4%ba%8e%e9%ab%98%e6%95%88%e5%85%89%e5%82%ac%e5%8c%96%e5%88%b6","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=205758","title":{"rendered":"\u5e7f\u4e1c\u77f3\u6cb9\u5316\u5de5\u5b66\u9662CJCE\uff1a\u7528\u4e8e\u9ad8\u6548\u5149\u50ac\u5316\u5236\u6c22\u7684P\u63ba\u6742g-C3N4\u7eb3\u7c73\u7247\u7684\u53ef\u63a7\u5236\u5907"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u901a\u8fc7\u592a\u9633\u5149\u5149\u89e3\u6c34\u5236\u6c22\u662f\u4e00\u79cd\u73af\u4fdd\u7684\u53ef\u518d\u751f\u80fd\u6e90\u7684\u5236\u5907\u6280\u672f\uff0c\u77f3\u58a8\u78b3\u6c2e\u5316\u7269\uff08g-C<sub>3<\/sub>N<sub>4<\/sub>\uff09\u5c3d\u7ba1\u6709\u660e\u663e\u7684\u50ac\u5316\u4f5c\u7528\uff0c\u4ecd\u7136\u4e0d\u80fd\u6ee1\u8db3\u4ea7\u751f\u6c22\u6c14\u7684\u9700\u8981\u3002g-C<sub>3<\/sub>N<sub>4<\/sub>\u7eb3\u7c73\u7ed3\u6784\u4e0d\u4ec5\u53ef\u4ee5\u52a0\u901f\u5149\u751f\u7535\u5b50\u7a7a\u7a74\u5bf9\u7684\u6709\u6548\u5206\u79bb\u548c\u8f6c\u79fb\uff0c\u800c\u4e14\u53ef\u4ee5\u6709\u6548\u5730\u9632\u6b62\u5149\u751f\u8f7d\u6d41\u5b50\u5f7c\u6b64\u590d\u5408\u3002\u8bb8\u591a\u6587\u732e\u8868\u660e\uff0c\u5728\u727a\u7272\u6027\u7684\u8f85\u52a9\u4e0b\u5242\u548c\u52a9\u50ac\u5316\u5242\uff0c\u5149\u50ac\u5316\u5236\u6c22\u6548\u7387\u53ef\u80fd\u66f4\u9ad8\u3002\u539f\u56e0\u662f\u52a9\u50ac\u5316\u5242\u53ef\u4ee5\u4f5c\u4e3a\u4ea7\u6c22\u7684\u6d3b\u6027\u70b9\uff0c\u5149\u751f\u7535\u5b50\u5c06\u6ce8\u5165\u5230\u52a9\u50ac\u5316\u5242\u4e2d\uff0c\u4f7f\u5149\u751f\u8f7d\u6d41\u5b50\u91cd\u65b0\u5206\u5e03\uff0c\u4ece\u800c\u4f7f\u66f4\u591a\u7684\u6d3b\u6027\u8f7d\u6d41\u5b50\u53ef\u4ee5\u53c2\u4e0e\u5149\u50ac\u5316\u53cd\u5e94\uff0c\u63d0\u9ad8\u5149\u50ac\u5316\u6d3b\u6027\u3002\u94c2\u7531\u4e8e\u5177\u6709\u8f83\u9ad8\u7684\u50ac\u5316\u6d3b\u6027\u800c\u6210\u4e3a\u52a9\u50ac\u5316\u5242\u7684\u7814\u7a76\u70ed\u70b9\u3002\u00a0<\/p>\n<p>\u5173\u4e8e\u5f02\u8d28\u7ed3\u7684\u6784\u9020\uff0c\u65e9\u671f\u7684\u62a5\u9053\u79f0\u5176\u5bf9\u5149\u751f\u7535\u5b50\u7684\u5206\u79bb\u751a\u81f3\u7535\u5b50\u7a7a\u7a74\u5bf9\u7684\u590d\u5408\u6709\u5f71\u54cd\uff0c\u4f46\u662f\u5f88\u96be\u5236\u5907\u3002\u63ba\u6742\u91d1\u5c5e\u5143\u7d20\u7684\u673a\u7406\u662f\uff0c\u63ba\u6742\u7684\u91d1\u5c5e\u5143\u7d20\u53ef\u4ee5\u5728g-C<sub>3<\/sub>N<sub>4<\/sub>\u7684\u5bfc\u5e26\u4ee5\u4e0b\u6216\u4ef7\u5e26\u4e4b\u4e0a\u751f\u6210\u65b0\u7684\u53d7\u4f53\u80fd\u7ea7\uff0c\u4ece\u800c\u51cf\u5c0fg-C<sub>3<\/sub>N<sub>4<\/sub>\u7684\u5e26\u9699\u5e76\u589e\u5f3a\u53ef\u89c1\u5149\u7684\u5438\u6536\u3002\u5982\u679c\u91c7\u7528\u91d1\u5c5e\u63ba\u6742\uff0c\u5219\u4f1a\u51fa\u73b0\u6676\u4f53\u7f3a\u9677\u3002\u6b64\u5916\uff0c\u63ba\u6742\u7684\u91d1\u5c5e\u5143\u7d20\u53ef\u80fd\u5145\u5f53\u590d\u5408\u4e2d\u5fc3\uff0c\u4ece\u800c\u5bfc\u81f4\u91cf\u5b50\u6548\u7387\u964d\u4f4e\u3002\u975e\u91d1\u5c5e\u5143\u7d20\u63ba\u6742\u901a\u8fc7\u4e0eg-C<sub>3<\/sub>N<sub>4<\/sub>\u7684\u4ef7\u5e26\u6742\u5316\u6765\u51cf\u5c0f\u5e26\u9699\u3002\u4e0e\u91d1\u5c5e\u63ba\u6742\u76f8\u6bd4\uff0c\u975e\u91d1\u5c5e\u63ba\u6742\u4e0d\u4f1a\u5f15\u5165\u8f7d\u6d41\u5b50\u590d\u5408\u4e2d\u5fc3\uff0c\u8fd9\u4e00\u4f18\u52bf\u6709\u5229\u4e8e\u63d0\u9ad8\u5149\u50ac\u5316\u6d3b\u6027\u3002\u6709\u6587\u732e\u5de5\u4f5c\u8868\u660e\uff0c\u56fa\u6001\u6b21\u78f7\u9178\u94a0\u7ecf\u8fc7\u70ed\u5904\u7406\u540e\u53ef\u4ee5\u5206\u89e3\u6210\u6c14\u6001PH<sub>3<\/sub>\uff0c\u800c\u6c14\u6001PH<sub>3<\/sub>\u53ef\u4ee5\u5c06\u78f7\u539f\u5b50\u7ed3\u5408\u5230\u5404\u79cd\u7684\u57fa\u5e95\uff08\u5982\u78b3\u6750\u6599\u3001\u91d1\u5c5e\u6750\u6599\u7b49\uff09\u7ed3\u6784\u4e2d\u3002\u4e0e\u6b21\u78f7\u9178\u94a0\u4e3a\u78f7\u6e90\u5236\u5907\u78f7\u63ba\u6742g-C<sub>3<\/sub>N<sub>4<\/sub>\u5177\u6709\u660e\u6717\u7684\u5e94\u7528\u524d\u666f\u548c\u521b\u65b0\u610f\u4e49\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u56e0\u6b64\uff0c\u5728\u672c\u7814\u7a76\u4e2d\u5e7f\u4e1c\u77f3\u6cb9\u5316\u5de5\u5b66\u9662\u7684\u672c\u79d1\u751f<strong><b>\u6797\u6070\u7eaf<\/b><\/strong>\uff08\u4e00\u4f5c\uff09\u3001<strong><b>\u674e\u6cfd\u80dc<\/b><\/strong>\u526f\u6559\u6388\uff08\u901a\u8baf\uff09\u3001<strong><b>\u4f59\u957f\u6797<\/b><\/strong>\u6559\u6388\uff08\u901a\u8baf\uff09\u7b49\u4eba\u63d0\u51fa\u4e86\u4e00\u79cd\u6709\u6548\u7684\u6c2e\u5316\u78b3\u6539\u6027\u65b9\u6cd5\uff0c\u5373\u5c06\u5df2\u7ecf\u5236\u5907\u597d\u7684\u6c2e\u5316\u78b3\u4e0e\u6b21\u78f7\u9178\u94a0\u6df7\u5408\u5728\u60f0\u6027\u6c14\u6c1b\u4e0b\u8fdb\u884c\u7145\u70e7\uff0c\u4ece\u800c\u5f97\u5230\u5408\u6210\u78f7\u63ba\u6742\u7684\u77f3\u58a8\u6c2e\u5316\u78b3\u3002\u79cd\u56fa-\u6c14\u53cd\u5e94\u5177\u6709\u8bb8\u591a\u4f18\u70b9\uff1a\uff08i\uff09\u5408\u9002\u6279\u91cf\u5316\u7684\u53cd\u5e94\u6e29\u5ea6\uff0c\uff08ii\uff09\u53ef\u63a5\u53d7\u7684\u539f\u6599\u4ef7\u683c\uff0c\uff08iii\uff09\u6c14\u6001PH<sub>3<\/sub>\u76f4\u63a5\u53c2\u4e0e\u53cd\u5e94\u800c\u6ca1\u6709\u4e8c\u6b21\u6c61\u67d3\u7b49\u3002\u7136\u540e\u7814\u7a76\u4e86\u50ac\u5316\u5242\u7684\u5149\u50ac\u5316\u6d3b\u6027\u4ee5\u751f\u4ea7\u6c22\u6c14\u3002\u5728\u672c\u6b21\u7814\u7a76\u4e2d\uff0c\u52a0\u5165\u78f7\u5143\u7d20\u662f\u4e3a\u4e86\u8c03\u8282g-C<sub>3<\/sub>N<sub>4<\/sub>\u7684\u6027\u80fd\uff0c\u540c\u65f6\u8fd8\u63d0\u4f9b\u4e86\u727a\u7272\u5242\u548cPt\u52a9\u50ac\u5316\u5242\u4ee5\u5e2e\u52a9\u6709\u6548\u5730\u5149\u50ac\u5316\u5236\u6c22\u3002\u7ed3\u679c\u8868\u660e\uff0c\u4ee5\u4e0d\u540c\u7684\u78b3\u78f7\u6bd4\u5236\u5907\u7684\u50ac\u5316\u6750\u6599\u7684\u50ac\u5316\u6027\u80fd\u662f\u4e0d\u540c\u7684\u3002P\u63ba\u6742\u7684g-C<sub>3<\/sub>N<sub>4<\/sub>\u7684\u6700\u9ad8\u4ea7\u751fH<sub>2<\/sub>\u7684\u901f\u7387\u4e3a318\u03bcmol h<sup>-1<\/sup>g<sup>-1<\/sup>,\uff0c\u662f\u672a\u63ba\u6742\u65f6\u76842.98\u500d\u3002\u672c\u7814\u7a76\u4e3a\u9ad8\u6548\u4fee\u9970g-C<sub>3<\/sub>N<sub>4<\/sub>\u5f00\u8f9f\u4e86\u4e00\u6761\u7b80\u5355\u3001\u73af\u4fdd\u3001\u53ef\u6301\u7eed\u7684\u65b0\u9014\u5f84\u3002\u76f8\u5173\u6210\u679c\u4ee5\u201cControlled preparation of P-doped g-C<sub>3<\/sub>N<sub>4<\/sub>\u00a0nanosheets for efficient photocatalytic hydrogen production\u201d\u4e3a\u9898\u76ee\u53d1\u8868\u4e8e<em><i>Chinese Journal of Chemical Engineering<\/i><\/em>\uff08<strong><b>C<\/b><\/strong><strong><b>JCE<\/b><\/strong>,\u00a0\u56fd\u4ea7<em><i>Chemical Engineering Journal<\/i><\/em>, IF=2.627\uff09\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong><b>\u56fe1\uff1a<\/b><\/strong><strong><b>\u672c\u6b21\u5b9e\u9a8c\u6240\u7528\u5230\u7684<\/b>g-C<sub>3<\/sub>N<sub>4<\/sub>\u00a0<b>\u7efc\u8ff0\u793a\u610f\u56fe<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-205759 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72471-33.png\" alt=\"\" width=\"600\" height=\"328\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72471-33.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72471-33-300x164.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u4e3a\u4e86\u514b\u670d\u4e0a\u8ff0\u95ee\u9898\uff0c\u4eba\u4eec\u63d0\u51fa\u4e86\u5404\u79cd\u4fee\u9970\u65b9\u6cd5\uff0c\u4f8b\u5982\u5236\u5907g-C<sub>3<\/sub>N<sub>4<\/sub>\u7eb3\u7c73\u7ed3\u6784\uff0c\u5171\u50ac\u5316\u5242\u6539\u6027\uff0c\u6784\u5efa\u57fa\u4e8eg-C<sub>3<\/sub>N<sub>4<\/sub>\u7684\u5f02\u8d28\u7ed3\uff0c\u5143\u7d20\u548c\u5206\u5b50\u63ba\u6742\uff0c\u4ee5\u589e\u5f3a\u5176\u5149\u50ac\u5316\u6027\u80fd\uff08\u7efc\u8ff0\u793a\u610f\u56fe\u89c1\u56fe1\uff09\u3002\u8f83\u5927\u6bd4\u8868\u9762\u79ef\u7684g-C<sub>3<\/sub>N<sub>4<\/sub>\u7eb3\u7c73\u7ed3\u6784\u7684\u53ef\u4ee5\u63d0\u4f9b\u66f4\u591a\u7684\u6d3b\u6027\u4f4d\u70b9\u3002<\/p>\n<p><strong><b>\u56fe2\uff1a\u5236\u5907\u7684<\/b>g-C<sub>3<\/sub>N<sub>4<\/sub><b>\u6837\u54c1\u7684XRD\u56fe\u8c31<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-205760 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72472-32.png\" alt=\"\" width=\"600\" height=\"427\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72472-32.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72472-32-300x214.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u4f17\u6240\u5468\u77e5\uff0cX\u5c04\u7ebf\u884d\u5c04(XRD)\u53ef\u4ee5\u51c6\u786e\u5730\u8bc4\u4ef7\u6240\u5236\u5907\u7684\u6837\u54c1\u7684\u6676\u4f53\u7ed3\u6784\u6027\u8d28\u3002\u7ed3\u679c\u8868\u660e\uff0cCN\u7684XRD\u56fe\u4e2d\uff0c\u572813.7\u5ea6\u548c27.5\u5ea6\u9644\u8fd1\u6709\u4e24\u4e2a\u660e\u663e\u7684\u884d\u5c04\u5cf0(\u56fe2)\u3002<\/p>\n<p><strong><b>\u56fe3\uff1a\u6837\u54c1\u7684<\/b><\/strong><strong><b>XPS\u5149\u8c31<\/b><\/strong><strong><b>\uff1a<\/b><\/strong><strong><b>C1<\/b><\/strong><strong><b>s<\/b><\/strong><strong><b>(B)<\/b><\/strong><strong><b>\u3001N<\/b><\/strong><strong><b>1<\/b><\/strong><strong><b>s<\/b><\/strong><strong><b>(C)<\/b><\/strong><strong><b>\u3001P<\/b><\/strong><strong><b>2p(D)<\/b><\/strong><strong><b>\u7684<\/b><\/strong><strong><b>\u6d4b\u91cf\u548c\u9ad8\u5206\u8fa8\u7387<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-205761 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72473-30.png\" alt=\"\" width=\"600\" height=\"454\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72473-30.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72473-30-300x227.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u4e3a\u4e86\u9a8c\u8bc1\u78f7\u63ba\u6742\u65b9\u6cd5\u7684\u6709\u6548\u6027\uff0c\u8fdb\u4e00\u6b65\u786e\u5b9a\u6240\u5f97\u5230\u6750\u6599\u7684\u5316\u5b66\u6210\u5206\uff0c\u901a\u8fc7X\u5c04\u7ebf\u5149\u7535\u5b50\u80fd\u8c31(XPS)\u5bf9\u6837\u54c1\u8fdb\u884c\u4e86\u8bc4\u4f30\u3002\u6700\u7ec8\u7ed3\u679c\u5982\u56fe3\u6240\u793a\u3002PCN-S\u6837\u54c1,\u53ea\u6709C\u3001N\u3001O\u548cP\u5143\u7d20\u88ab\u68c0\u6d4b\u5230,\u8fd9\u8868\u660e\u6709\u9ad8\u7eaf\u5ea6\u7684\u6750\u6599\u3002\u901a\u8fc7\u89c2\u5bdf\u56fe3A\u548c3B\u540e,\u53ef\u4ee5\u53d1\u73b0CN\u548cPCN-S\u51e0\u4e4e\u76f8\u540c\u7684C1s\u548cN1s\u5149\u8c31,\u8868\u660eP\u63ba\u6742\u540e\u7684\u5316\u5b66\u7ed3\u6784\u4ecd\u7136\u4fdd\u7559\u3002<\/p>\n<p>\u5bf9\u4e8eC1s\u8c31\uff0c\u53ef\u4ee5\u770b\u5230\u4e24\u4e2a\u4e3b\u5cf0\u5206\u522b\u4f4d\u4e8e284.66eV\u548c288.14eV\u3002C=C-C\u952e\u53ef\u80fd\u5bfc\u81f4\u5728284.66 eV\u51fa\u73b0\u5cf0\u503c\u3002\u800c\u4e3b\u5cf0\u5728288.14eV\uff0c\u76f8\u5173\u6587\u732e\u8868\u660e\u5176\u53ef\u5f52\u56e0\u4e8eN-C=N\u3002<\/p>\n<p>N1s\u8c31(\u56fe3B)\u6e05\u695a\u5730\u8bc1\u660e\u4e86\u6c2e\u539f\u5b50\u5b58\u5728\u4e8e\u4e09\u79cd\u5316\u5b66\u73af\u5883\u3002\u7b2c\u4e00\u4e2a\u4e3b\u8981\u5cf0\u51fa\u73b0\u5728398.46 eV\uff0c\u8fd9\u662fC-N=C\u4e2dSP2 N\u539f\u5b50\u7684\u7279\u5f81\u3002\u7b2c\u4e8c\u4e2a\u5f3a\u5ea6\u8f83\u4f4e\uff0c\u5904\u4e8e\u8f83\u9ad8\u7684\u7ed3\u5408\u80fd\uff0c\u53ef\u80fd\u662fN-(C)3,\uff0c\u800c\u5728400.70eV\u65f6\uff0c\u5e94\u8be5\u662fH\u2013N-C\u4e2dSP2 N\u6742\u5316N\u539f\u5b50\u7684\u7279\u5f81\u3002C\u548cN\u7684\u952e\u4ef7\u5f62\u5f0f\u662f\u77f3\u58a8\u76f8\u6c2e\u5316\u78b3\u7684\u7279\u5f81\u7ed3\u6784\uff0c\u8fd9\u4e0e\u4e4b\u524d\u7684\u62a5\u9053\u4e00\u81f4\u3002<\/p>\n<p>\u6b63\u5982\u6240\u9884\u6599\uff0c\u5728CN\u8c31\u4e2d\u7684P 2p\uff0c\u6ca1\u6709\u51fa\u73b0P 2p\u5cf0\uff0c\u56e0\u4e3a\u8fd9\u4e2a\u6837\u54c1\u6ca1\u6709\u63ba\u6742\u78f7\u3002\u7136\u800c\uff0cP-N\u8d21\u732e\u4e86PCN\u8c31\u4e2d\u51fa\u73b0\u7684133.56\u5cf0\u3002\u56e0\u6b64\uff0c\u53ef\u4ee5\u63d0\u51fa\u5728P\u63ba\u6742\u8fc7\u7a0b\u4e2d\uff0c\u7528\u78f7\u5143\u7d20\u53d6\u4ee3C-N\u952e\u4e2d\u7684C\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4<\/b><\/strong><strong><b>\uff1a\u6837\u54c1\u7684<\/b><\/strong><strong><b>TEM<\/b><\/strong><strong><b>\u548cE<\/b><\/strong><strong><b>DS<\/b><\/strong><strong><b>\u5143\u7d20\u626b\u63cf\u56fe\u7247<\/b><\/strong><\/p>\n<p><strong><b>\u00a0<img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-205762 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72474-31.png\" alt=\"\" width=\"600\" height=\"342\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72474-31.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72474-31-300x171.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/b><\/strong><\/p>\n<p>\u7528\u900f\u5c04\u7535\u955cTEM\u8fdb\u4e00\u6b65\u89c2\u5bdf\u4e86\u6837\u54c1\u7684\u5f62\u8c8c\u7ec6\u8282\u3002\u56fe\u50cf\u5982\u56fe4\uff08A-C\uff09\u6240\u793a\u3002\u4ece\u56fe4\u56fe\u50cf\uff08A-B\uff09\u53ef\u4ee5\u770b\u51fa\uff0c\u5df2\u7ecf\u6210\u529f\u5408\u6210\u4e86\u4e0d\u89c4\u5219\u7684\u4e8c\u7ef4\u5927\u5c3a\u5ea6\u7ed3\u6784\uff0cPCN-S-3\u8868\u9762\u7f3a\u4e4f\u5149\u6ed1\u5ea6\u3002\u56fe4C\u663e\u793aPCN-S-3\u5448\u5411\u5185\u5377\u66f2\u7684\u8d8b\u52bf\u3002\u6b64\u5916\uff0c\u6211\u4eec\u4f7f\u7528HAADF-STEM\u89c2\u5bdf\u5355\u4e2a\u7eb3\u7c73\u9897\u7c92\uff08\u89c1\u56fe4D\uff09\u3002\u6b64\u5916\uff0c\u8fd8\u6dfb\u52a0\u4e86\u5143\u7d20\u6620\u5c04\u56fe\uff08\u89c1\u56fe4E-G\uff09\uff0c\u7ed3\u679c\u8868\u660e\uff0cC\u3001N\u548cP\u5747\u5206\u5e03\u5728PCN-S-3\u7684\u6574\u4e2a\u7ed3\u6784\u4e2d\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>5<\/b><\/strong><strong><b>\uff1a\u5149\u89e3\u5236\u6c22\u56fe\u8868:<\/b><\/strong><strong><b>(<\/b><\/strong><strong><b>A<\/b><\/strong><strong><b>)CN (B) PCN-S-1 (C) PCN-S-2 (D) PCN-S-3 (E)\u6807\u51c6\u66f2\u7ebf<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>(F)\u5cf0\u9762\u79ef\u4e0e\u6c22\u542b\u91cf\u7684\u5173\u7cfb\u66f2\u7ebf<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-205763 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72475-26.png\" alt=\"\" width=\"600\" height=\"662\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72475-26.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/07\/\u56fe\u72475-26-272x300.png 272w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u5149\u50ac\u5316\u5236\u6c22\u6837\u54c1\u7684\u6c14\u76f8\u8272\u8c31\u56fe\u5982\u56fe4A\uff0c4B\uff0c4C\uff0c4D\u6240\u793a\u3002\u901a\u8fc7\u5c06\u4e00\u5b9a\u91cf\u4f53\u79ef\u7684\u6807\u51c6\u6c22\u6ce8\u5165\u6c14\u76f8\u8272\u8c31\u4eea\u83b7\u5f97\u56fe4E\u3002\u56fe4F\u662f\u901a\u8fc7\u7406\u60f3\u7684\u6c14\u4f53\u72b6\u6001\u65b9\u7a0b\u5c06\u4f53\u79ef\uff08ML\uff09\u8f6c\u6362\u4e3a\u6469\u5c14\u4f53\u79ef\uff08\u03bcmol\uff09\uff0c\u7136\u540e\u5efa\u7acb\u5cf0\u9762\u79ef\u4e0e\u6c22\u6469\u5c14\u4f53\u79ef\u4e4b\u95f4\u7684\u5173\u7cfb\uff0c\u7ed9\u51fa\u6807\u51c6\u504f\u5dee\uff0c\u5c06\u5728\u4e0d\u540c\u65f6\u95f4\u83b7\u5f97\u7684\u4e00\u7cfb\u5217\u5236\u6c22\u6570\u636e\u4ee3\u5165\u5f97\u5230\u3002\u53ef\u4ee5\u7ed8\u5236\u51fa\u5236\u6c22\u6469\u5c14\u91cf\uff08\u03bcmol\uff09\u4e0e\u65f6\u95f4\uff08h\uff09\u4e4b\u95f4\u7684\u5173\u7cfb\u66f2\u7ebf\uff0c\u7136\u540e\u901a\u8fc7\u7ebf\u6027\u62df\u5408\u5f97\u51fa\u76f4\u7ebf\u5f62\u7684\u659c\u7387\uff0c\u62df\u5408\u540e\u7684\u7ebf\u662f\u6837\u54c1\u7684\u50ac\u5316\u4ea7\u6c22\u7387\u503c\u3002\u53ef\u4ee5\u5f97\u51fa\uff0c\u901f\u7387\u503c\u8d8a\u9ad8\uff0c\u50ac\u5316\u5242\u7684\u5149\u50ac\u5316\u6d3b\u6027\u8d8a\u597d\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u672c\u6b21\u5b9e\u9a8c\u63d0\u51fa\u4e86\u4e00\u79cd\u6539\u6027\u6c2e\u5316\u78b3\u7684\u65b0\u7b56\u7565\uff1a\u9009\u62e9\u6b21\u78f7\u9178\u94a0\u4f5c\u4e3a\u78f7\u6e90\uff0c\u901a\u8fc7\u70ed\u5904\u7406\u6210\u529f\u5236\u5907\u4e86\u542b\u78f7g-C<sub>3<\/sub>N<sub>4<\/sub>\u7eb3\u7c73\u7247\u3002\u5728\u8fd9\u9879\u5b9e\u9a8c\u4e2d\uff0c\u8bc1\u660e\u4e86P\u539f\u5b50\u4ee3\u66ffC\u539f\u5b50\u5e76\u7eb3\u5165C\u539f\u5b50\uff0cPCN-S-2\u7684C=N-C\u4e2d\u7684N-C\u952e\u53ef\u80fd\u5728\u63ba\u78f7\u8fc7\u7a0b\u4e2d\u65ad\u88c2\u3002\u727a\u7272\u5242\u548c\u52a9\u50ac\u5316\u5242\u4e5f\u88ab\u63d0\u4f9b\u4ee5\u5e2e\u52a9\u6709\u6548\u7684\u5149\u50ac\u5316\u5236\u6c22\u3002PCN-S-3\u91ca\u653eH2\u7684\u901f\u7387\u662fCN\u76842.98\u500d\u3002\u7279\u522b\u6709\u8da3\u7684\u662f\uff0cPCN-S-2\u4e0d\u4ec5\u6210\u529f\u63ba\u6742\u4e86\u78f7\uff0c\u800c\u4e14\u8fd8\u5b58\u5728\u78b3\u7f3a\u9677\u3002\u5f53\u78f7\u63ba\u6742\u548c\u78b3\u7f3a\u9677\u540c\u65f6\u5b58\u5728\u65f6\u4f1a\u4ea7\u751f\u79ef\u6781\u5f71\u54cd\uff0c\u5927\u5927\u63d0\u9ad8\u4e86\u6c34\u751f\u6c22\u7684\u5149\u89e3\u901f\u7387\u3002<\/p>\n<p><strong><b>\u6587\u732e\u94fe\u63a5\uff1a<\/b><\/strong><strong><b>Controlled preparation of P-doped g-C3N4 nanosheets for efficient photocatalytic hydrogen production \uff08https:\/\/doi.org\/10.1016\/j.cjche.2020.06.037\uff09<\/b><\/strong><\/p>\n<p>\u672c\u6587\u7531\u5e7f\u4e1c\u77f3\u6cb9\u5316\u5de5\u5b66\u9662\u674e\u6cfd\u80dc\u526f\u6559\u6388\u8bfe\u9898\u7ec4\u6295\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u901a\u8fc7\u592a\u9633\u5149\u5149\u89e3\u6c34\u5236\u6c22\u662f\u4e00\u79cd\u73af\u4fdd\u7684\u53ef\u518d\u751f\u80fd\u6e90\u7684\u5236\u5907\u6280\u672f\uff0c\u77f3\u58a8\u78b3\u6c2e\u5316\u7269\uff08g-C3N4\uff09\u5c3d\u7ba1\u6709\u660e\u663e\u7684\u50ac\u5316\u4f5c\u7528\uff0c\u4ecd\u7136\u4e0d\u80fd\u6ee1\u8db3\u4ea7\u751f\u6c22\u6c14\u7684\u9700\u8981\u3002g-C3N4\u7eb3\u7c73\u7ed3&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-205758","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/205758"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=205758"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/205758\/revisions"}],"predecessor-version":[{"id":205838,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/205758\/revisions\/205838"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=205758"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=205758"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=205758"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}