{"id":209214,"date":"2020-09-11T06:30:08","date_gmt":"2020-09-10T22:30:08","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=209214"},"modified":"2020-09-10T17:22:05","modified_gmt":"2020-09-10T09:22:05","slug":"%e3%80%90%e6%8a%95%e7%a8%bf%e3%80%91acta-mater%ef%bc%9a%e5%a4%a7%e5%9d%97%e9%87%91%e5%b1%9e%e7%8e%bb%e7%92%83%e5%bd%a2%e5%8f%98%e5%bc%ba%e5%8c%96%e5%a4%9a%e7%ba%a7%e8%b7%a8%e5%b0%ba%e5%ba%a6%e7%bb%93","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=209214","title":{"rendered":"Acta Mater\uff1a\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u5f62\u53d8\u5f3a\u5316\u591a\u7ea7\u8de8\u5c3a\u5ea6\u7ed3\u6784\u975e\u5747\u5300\u6027\u7814\u7a76"},"content":{"rendered":"<p><strong><b>\u3010\u5f15\u8a00\u3011<\/b><\/strong><\/p>\n<p>\u957f\u671f\u4ee5\u6765\uff0c\u91d1\u5c5e\u73bb\u7483\u5851\u6027\u7684\u7ed3\u6784\u8d77\u6e90\u4ee5\u53ca\u7ed3\u6784\u54cd\u5e94\u4e00\u76f4\u60ac\u800c\u672a\u51b3\uff0c\u5176\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u7ed3\u6784-\u6027\u80fd\u5173\u8054\u673a\u5236\u4ecd\u4e0d\u6e05\u695a\uff0c\u56e0\u6b64\u7814\u7a76\u91d1\u5c5e\u73bb\u7483\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u591a\u5c3a\u5ea6\u591a\u7ea7\u7ed3\u6784\u6f14\u53d8\u5bf9\u7406\u89e3\u7ed3\u6784-\u6027\u80fd\u5173\u7cfb\u5177\u6709\u91cd\u8981\u7684\u610f\u4e49\u3002\u975e\u6676\u6001\u6750\u6599\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u591a\u5c3a\u5ea6\u7ed3\u6784\u54cd\u5e94\u7684\u539f\u4f4d\u65e0\u635f\u5316\u8868\u5f81\u662f\u5f53\u524d\u7814\u7a76\u7684\u96be\u70b9\u4e4b\u4e00\u3002\u8be5\u7814\u7a76\u4ee5Pd-Si\u4e8c\u5143\u975e\u6676\u5408\u91d1\u4f53\u7cfb\u4e3a\u7814\u7a76\u5bf9\u8c61\uff0c\u5229\u7528\u5148\u8fdb\u7684\u4e2d\u5b50\u548c\u540c\u6b65\u8f90\u5c04\u7b49\u5927\u79d1\u5b66\u88c5\u7f6e\u4e3a\u4ece\u591a\u5c3a\u5ea6\u7ed3\u6784\u89d2\u5ea6\u7814\u7a76\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u63d0\u4f9b\u4e86\u72ec\u7279\u7684\u624b\u6bb5\u3002\u501f\u52a9\u540c\u6b65\u8f90\u5c04\u9ad8\u80fdX\u5c04\u7ebf\u884d\u5c04\u548c\u5c0f\u89d2\u4e2d\u5b50\/\u540c\u6b65\u8f90\u5c04\u6563\u5c04\uff0c\u8f85\u4ee5\u5e38\u89c4\u7535\u955c\u7b49\u68c0\u6d4b\u624b\u6bb5\uff0c\u5b9e\u73b0\u4e86\u5bf9\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u5f2f\u66f2\u3001\u62c9\u4f38\u548c\u538b\u7f29\u8fc7\u7a0b\u4e2d\u591a\u7ea7\u3001\u8de8\u5c3a\u5ea6\u7ed3\u6784\u7684\u8868\u5f81\uff0c\u901a\u8fc7\u5206\u6790\u4ece\u591a\u5c3a\u5ea6\u7ed3\u6784\u89d2\u5ea6\u7406\u89e3\u4e86\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u3002\u7814\u7a76\u63ed\u793a\u4e86\u56e2\u7c07\u8fde\u901a\u6a21\u5f0f\u5728\u62c9\u4f38\/\u538b\u7f29\u6d41\u53d8\u5e94\u529b\u4e0b\u7684\u4e0d\u540c\u54cd\u5e94\u3002\u7814\u7a76\u53d1\u73b0\u591a\u7ea7\u3001\u8de8\u5c3a\u5ea6\u975e\u5747\u5300\u6027\u7684\u6f14\u53d8\u548c\u6784\u7b51\u5728\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u8d77\u5230\u4e86\u91cd\u8981\u7684\u4f5c\u7528\uff0c\u8868\u660e\u591a\u7ea7\u7684\u8de8\u5c3a\u5ea6\u7ed3\u6784\u8c03\u63a7\u53ef\u80fd\u662f\u672a\u6765\u83b7\u5f97\u4f18\u5f02\u673a\u68b0\u6027\u80fd\u91d1\u5c5e\u73bb\u7483\u7684\u91cd\u8981\u601d\u8def\u4e4b\u4e00\u3002<\/p>\n<p><strong><b>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong><b>\u5357\u4eac\u7406\u5de5\u5927\u5b66\u5170\u53f8\u6559\u6388\uff08\u901a\u8baf\u4f5c\u8005\uff09\u6307\u5bfc\u535a\u58eb\u751f\u5218\u601d\u6960\uff08\u7b2c\u4e00\u4f5c\u8005\uff09\u548c\u7855\u58eb\u751f\u738b\u5229\u5cf0\uff08\u5171\u540c<\/b><\/strong><strong><b>\u7b2c\u4e00\u4f5c\u8005\uff0c<\/b><\/strong><strong><b>\u73b0\u5728\u5357\u4eac\u534e\u5174\u538b\u529b\u5bb9\u5668\u5236\u9020\u6709\u9650\u516c\u53f8\u4efb\u804c\uff09\uff0c\u8054\u5408\u9999\u6e2f\u57ce\u5e02\u5927\u5b66\u7269\u7406\u7cfb\u738b\u5faa\u7406<\/b><\/strong><strong><b>\u6559\u6388<\/b><\/strong><strong><b>\u3001\u7f8e\u56fd\u963f\u8d21\u5b9e\u9a8c\u5ba4\u5148\u8fdb\u5149\u6e90\u4efb\u6d0b<\/b><\/strong><strong><b>\u535a\u58eb<\/b><\/strong><strong><b>\u3001\u4e2d\u56fd\u6563\u88c2\u4e2d\u5b50\u6e90\u5c0f\u89d2<\/b><\/strong><strong><b>\u6563\u5c04\u7ebf\u7ad9<\/b><\/strong><strong><b>\u67ef\u4e8e<\/b><\/strong><strong><b>\u658c<\/b><\/strong><strong><b>\u526f\u7814\u7a76\u5458\u3001\u4e2d\u79d1\u9662\u7269\u7406\u6240\/\u677e\u5c71\u6e56\u6750\u6599\u5b9e\u9a8c\u5ba4\u5b59\u4fdd\u5b89\u7814\u7a76\u5458\u3001\u65b0\u7586\u5927\u5b66\u7269\u7406\u79d1\u5b66<\/b><\/strong><strong><b>\u4e0e\u6280\u672f<\/b><\/strong><strong><b>\u5b66\u9662\u674e\u5f3a<\/b><\/strong><strong><b>\u6559\u6388<\/b><\/strong><strong><b>\u3001\u5317\u4eac\u79d1\u6280\u5927\u5b66\u65b0\u91d1\u5c5e<\/b><\/strong><strong><b>\u56fd\u5bb6<\/b><\/strong><strong><b>\u91cd\u70b9<\/b><\/strong><strong><b>\u5b9e\u9a8c\u5ba4<\/b><\/strong><strong><b>\u5434<\/b><\/strong><strong><b>\u6e0a\u6559\u6388<\/b><\/strong><strong><b>\u7b49<\/b><\/strong>\u5408\u4f5c\u8005\u5f00\u5c55\u4e86\u76f8\u5173\u7814\u7a76\u5de5\u4f5c\uff0c\u7814\u7a76\u6210\u679c\u4ee5<strong><b>\u201cDeformation-enhancedhierarchicalmultiscale<\/b><\/strong><strong><b>\u00a0structure heterogeneity in a Pd-Si bulk metallic glass<\/b><\/strong><strong><b>\u201d<\/b><\/strong>\u4e3a\u9898\u5728<strong><b>ActaMaterialia<\/b><\/strong>\u53d1\u8868\u3002\u8be5\u5de5\u4f5c\u5229\u7528\u540c\u6b65\u8f90\u5c04\u9ad8\u80fdX\u5c04\u7ebf\u884d\u5c04\u3001\u540c\u6b65\u8f90\u5c04\u5c0f\u89d2X\u5c04\u7ebf\u6563\u5c04\u3001\u5c0f\u89d2\u4e2d\u5b50\u6563\u5c04\uff0c\u7ed3\u5408\u900f\u5c04\u7535\u955c\u7b49\u624b\u6bb5\uff0c\u4ece\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u591a\u7ea7\u3001\u591a\u5c3a\u5ea6\u7ed3\u6784\u54cd\u5e94\u89d2\u5ea6\u51fa\u53d1\uff0c\u7cfb\u7edf\u7684\u7814\u7a76\u4e86Pd<sub>82<\/sub>Si<sub>18<\/sub>\u91d1\u5c5e\u73bb\u7483\u5728\u5f2f\u66f2\u3001\u62c9\u4f38\u548c\u538b\u7f29\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u4ece\u539f\u5b50\u5230\u7eb3\u7c73\u5230\u5fae\u7c73\u5c3a\u5ea6\u4e0a\u7684\u7ed3\u6784\u6f14\u53d8\u3002\u7814\u7a76\u53d1\u73b0\uff0c\u5728\u53d8\u5f62\u8fc7\u7a0b\u4e2d\uff0c\u4e2d\u7a0b\u5e8f\u5c3a\u5ea6\u4e0a\u7684\u56e2\u7c07\u8fde\u901a\u6a21\u5f0f\u4e4b\u95f4\u7684\u8f6c\u6362\u4e3b\u5bfc\u4e86\u5851\u6027\u53d8\u5f62\u7684\u5168\u8fc7\u7a0b\u7ed3\u6784\uff0c\u540c\u65f6\u5728\u62c9\u4f38\u548c\u538b\u7f29\u8fc7\u7a0b\u4e2d\u8868\u73b0\u51fa\u76f8\u53cd\u7684\u56e2\u7c07\u8fde\u901a\u6027\u6f14\u53d8\u6a21\u5f0f\u3002\u5bf9\u5206\u5e03\u51fd\u6570\u5206\u6790\u540c\u65f6\u8868\u660e\uff0c\u4e2d\u7a0b\u5e8f\u5c3a\u5ea6\u4e0a\u56e2\u7c07\u7684\u8fde\u901a\u6027\u8f6c\u53d8\u8fd8\u5f71\u54cd\u4e86\u5f2f\u66f2\u540e\u6837\u54c1\u62c9\u4f38\u4fa7\u548c\u538b\u7f29\u4fa7\u7684\u5806\u79ef\u5bc6\u5ea6\u5dee\u5f02\u3002\u5c0f\u89d2\u6563\u5c04\u548c\u7535\u5b50\u663e\u5fae\u955c\u89c2\u5bdf\u5230\u91d1\u5c5e\u73bb\u7483\u53d8\u5f62\u540e\u7684\u7eb3\u7c73\u5c3a\u5ea6\u975e\u5747\u5300\u6027\u548c\u9ad8\u5bc6\u5ea6\u7684\u591a\u7ea7\u3001\u591a\u91cd\u526a\u5207\u5e26\u3002\u5206\u6790\u8868\u660e\uff0c\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u6837\u54c1\u5728\u5f2f\u66f2\u540e\u5f15\u5165\u4e86\u590d\u6742\u4e14\u5468\u671f\u6027\u5206\u5e03\u7684\u6b8b\u4f59\u5e94\u53d8\uff0c\u5176\u539f\u56e0\u53ef\u80fd\u662f\u7531\u4e8e\u7eb3\u7c73\u5c3a\u5ea6\u7684\u975e\u6676\u76f8\u5206\u79bb\u548c\u5851\u6027\u53d8\u5f62\u589e\u5f3a\u7684\u591a\u7ea7\u526a\u5207\u5e26\u76f8\u4e92\u4f5c\u7528\u7684\u7ed3\u679c\u3002\u8be5\u7814\u7a76\u7ed3\u679c\u8fd8\u8868\u660e\uff0c\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u591a\u7ea7\u8de8\u5c3a\u5ea6\u975e\u5747\u5300\u7ed3\u6784\u7684\u589e\u5f3a\u53ef\u80fd\u662fPd-Si\u73bb\u7483\u5408\u91d1\u5177\u6709\u826f\u597d\u5851\u6027\u7684\u5185\u5728\u539f\u56e0\u3002\u8be5\u7814\u7a76\u7ed3\u679c\u6709\u52a9\u4e8e\u6df1\u5165\u7406\u89e3\u548c\u6784\u7b51\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u7ed3\u6784-\u6027\u80fd\u5173\u8054\u3002<\/p>\n<p><strong><b>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/b><\/strong><\/p>\n<p><strong><b>\u56fe1\uff1a<\/b><\/strong>\u5f2f\u66f2\u53d8\u5f62\u540e\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u7684\u526a\u5207\u5e26\u5f62\u8c8c\u7279\u5f81\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-209215 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72471-9.png\" alt=\"\" width=\"600\" height=\"848\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72471-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72471-9-212x300.png 212w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u53d8\u5f62\u524dPd<sub>82<\/sub>Si<sub>18<\/sub>\u91d1\u5c5e\u73bb\u7483\uff1b<\/p>\n<p>(b)\u5f2f\u66f2\u53d8\u5f62\u540ePd<sub>82<\/sub>Si<sub>18<\/sub>\u91d1\u5c5e\u73bb\u7483\uff1b<\/p>\n<p>(c)\u5f2f\u66f2\u53d8\u5f62\u6837\u54c1\u5c40\u90e8\u653e\u5927\u3002\u53ef\u4ee5\u770b\u5230\u62c9\u4f38\u4fa7(T)\u526a\u5207\u5e26\u5206\u5e03\u8303\u56f4\u8981\u5927\u4e8e\u538b\u7f29\u4fa7(B)\uff1b<\/p>\n<p>(d) (e) (f)\u5f2f\u66f2\u53d8\u5f62\u540e\u4e0d\u540c\u533a\u57df\u526a\u5207\u5e26\u5f62\u8c8c\u7684\u6bd4\u8f83\u3002\u5728\u62c9\u4f38\u4fa7\u4e3b\u526a\u5207\u5e26\u5448\u73b0\u4e24\u79cd\u7c7b\u578b\uff1a\u5f2f\u66f2\u4e14\u5782\u76f4\u8f74\u7ebf\u7684I\u578b\u548c\u5e73\u5766\u4e14\u503e\u659c\u7684II\u578b\uff0cI\u578b\u526a\u5207\u5e26\u4f1a\u8017\u6563\u66f4\u591a\u80fd\u91cf\uff0c\u540c\u65f6\u4f34\u968f\u5927\u91cf\u4e8c\u6b21\u526a\u5207\u5e26\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>2<\/b><\/strong><strong><b>\uff1a<\/b><\/strong>\u5f2f\u66f2\u53d8\u5f62\u524d\u540e\u6837\u54c1\u7684\u540c\u6b65\u8f90\u5c04\u9ad8\u80fdX\u5c04\u7ebf\u884d\u5c04\u7ed3\u679c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-209216 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72472-9.png\" alt=\"\" width=\"600\" height=\"708\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72472-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72472-9-254x300.png 254w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u540c\u6b65\u8f90\u5c04\u9ad8\u80fdX\u5c04\u7ebf\u884d\u5c04\u6d4b\u8bd5\u793a\u610f\u56fe\uff1b<\/p>\n<p>(b)\u5f2f\u66f2\u53d8\u5f62\u524d\u540e\u91d1\u5c5e\u73bb\u7483\u7684\u7ed3\u6784\u56e0\u5b50\u6bd4\u8f83\uff0c\u63d2\u56fe\u663e\u793a\u7b2c\u4e00\u884d\u5c04\u5cf0\u5cf0\u4f4d\u7684\u504f\u79fb\uff0c\u4ee3\u8868\u7740\u5f2f\u66f2\u53d8\u5f62\u540e\u538b\u7f29\u4fa7\/\u62c9\u4f38\u4fa7\u4e0e\u521d\u59cb\u6001\u6837\u54c1\u7684\u5806\u79ef\u5bc6\u5ea6\u53d8\u5316\uff1b<\/p>\n<p>(c) \u7b2c\u4e00\u884d\u5c04\u5cf0\u5cf0\u4f4d\u7684\u4e09\u7ef4\u7b49\u9ad8\u7ebf\u56fe\uff0c\u53ef\u4ee5\u770b\u51fa\u5f2f\u66f2\u6837\u54c1\u62c9\u4f38\u4fa7\u5230\u538b\u7f29\u4fa7\uff0c\u5cf0\u4f4d\u53d8\u5316\u5448\u5468\u671f\u6ce2\u6d6a\u72b6\uff1b<\/p>\n<p>(d) \u6839\u636e\u76f8\u5bf9\u5cf0\u503c\u4f4d\u79fb\u8ba1\u7b97\u51fa\u7684\u4ece\u62c9\u4f38\u4fa7\u5230\u538b\u7f29\u4fa7\u5782\u76f4\u6837\u54c1\u4e0d\u540c\u4f4d\u7f6e\u7684\u65b9\u5411\u5e94\u53d8\u03b5<sub>i<\/sub>\uff1b<\/p>\n<p>(e) \u5f2f\u66f2\u6837\u54c1\u6cbf\u4e2d\u8f74\u7ebf\u4ece\u62c9\u4f38\u4fa7\u5230\u538b\u7f29\u4fa7\u7684\u4e09\u4e2a\u5e94\u53d8\u5206\u91cf\uff0c\u9884\u793a\u7740\u539f\u5b50\u5c3a\u5ea6\u4e0a\u7684\u7ed3\u6784\u8d77\u4f0f\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>3<\/b><\/strong><strong><b>\uff1a<\/b><\/strong>\u5f2f\u66f2\u53d8\u5f62\u524d\u540e\u538b\u7f29\u548c\u62c9\u4f38\u4e24\u4fa7\u7684\u7ea6\u5316\u5bf9\u5206\u5e03\u51fd\u6570\u5206\u6790\u7ed3\u679c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-209217 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72473-8.png\" alt=\"\" width=\"600\" height=\"421\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72473-8.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72473-8-300x211.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u7ea6\u5316\u5bf9\u5206\u5e03\u51fd\u6570\u6307\u6570\u62df\u5408\u7ed3\u679c\uff0c\u53d8\u5f62\u533a\u66f4\u5927\u7684\u6307\u6570\u610f\u5473\u7740\u6709\u5e8f\u5ea6\u4f1a\u6269\u5c55\u5230\u66f4\u9ad8\u7684\u914d\u4f4d\u58f3\u5c42\uff1b<\/p>\n<p>(b)(c)(d) \u5bf9\u5206\u5e03\u51fd\u6570\u7684\u6b21\u8fd1\u90bb\u914d\u4f4d\u58f3\u5c42\u7684\u9ad8\u65af\u62df\u5408\u7ed3\u679c\uff0c\u5206\u89e3\u7684\u90e8\u5206\u5206\u522b\u5bf9\u5e94\u77ed\u7a0b\u56e2\u7c071-4\u539f\u5b50\u8fde\u901a\u6a21\u5f0f\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4<\/b><\/strong><strong><b>\uff1a<\/b><\/strong>Pd<sub>82<\/sub>Si<sub>18<\/sub>\u91d1\u5c5e\u73bb\u7483\u6761\u5e26\u539f\u4f4d\u540c\u6b65\u8f90\u5c04\u5355\u8f74\u62c9\u4f38\u7ed3\u679c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-209218 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72474-9.png\" alt=\"\" width=\"600\" height=\"413\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72474-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72474-9-300x207.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u91d1\u5c5e\u73bb\u7483\u6761\u5e26\u62c9\u4f38\u524d\u540e\u7ed3\u6784\u56e0\u5b50\u5bf9\u6bd4\uff0c\u63d2\u56fe\u4e3a\u65b9\u5411\u5e94\u53d8\u4e0e\u5de5\u7a0b\u5e94\u53d8\u5173\u7cfb\u66f2\u7ebf\uff0c\u6a59\u8272\u5b9e\u7ebf\u4e3a\u5f39\u6027\u9636\u6bb5\u62df\u5408\uff0c\u9ed1\u8272\u865a\u7ebf\u7528\u4e8e\u533a\u5206\u5f39\u6027\u548c\u5851\u6027\u9636\u6bb5\uff1b<\/p>\n<p>(b) \u91d1\u5c5e\u73bb\u7483\u6761\u5e26\u62c9\u4f38\u524d\u540e\u7ea6\u5316\u5bf9\u5206\u5e03\u51fd\u6570\u7684\u6307\u6570\u62df\u5408\u7ed3\u679c\uff1b<\/p>\n<p>(c) \u62c9\u4f38\u524d\u540e\u5bf9\u5206\u5e03\u51fd\u6570\u7684\u6b21\u8fd1\u90bb\u914d\u4f4d\u58f3\u5c42\u7684\u9ad8\u65af\u62df\u5408\u7ed3\u679c\uff1b<\/p>\n<p>(d) \u62c9\u4f38\u53d8\u5f62\u8fc7\u7a0b\u4e2d2\u539f\u5b50\u548c3\u539f\u5b50\u56e2\u7c07\u8fde\u63a5\u65b9\u5f0f\u7684\u53d8\u5316\uff0c\u9ed1\u8272\u865a\u7ebf\u7528\u4e8e\u533a\u5206\u5f39\u6027\u548c\u5851\u6027\u9636\u6bb5\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>5<\/b><\/strong><strong><b>\uff1a<\/b><\/strong>Pd<sub>82<\/sub>Si<sub>18<\/sub>\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u539f\u4f4d\u540c\u6b65\u8f90\u5c04\u5355\u8f74\u538b\u7f29\u7ed3\u679c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-209219 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72475-7.png\" alt=\"\" width=\"600\" height=\"391\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72475-7.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72475-7-300x196.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u5927\u5757\u91d1\u5c5e\u73bb\u7483\u5355\u8f74\u538b\u7f29\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\uff0c\u5927\u5757\u6837\u54c1\u5851\u6027\u5e94\u53d8\u53ef\u8d85\u8fc775%\u800c\u4e0d\u53d1\u751f\u65ad\u88c2\u3002\u63d2\u56fe\u4e3a\u538b\u7f29\u524d\u540e\u6837\u54c1\u626b\u63cf\u7535\u955c\u56fe\u7247\uff0c\u53ef\u4ee5\u770b\u5230\u53d8\u5f62\u540e\u6837\u54c1\u9ad8\u5bc6\u5ea6\u526a\u5207\u5e26\u5206\u5e03\uff0c\u540c\u65f6\u5b58\u5728\u4e30\u5bcc\u7684\u4e8c\u6b21\u526a\u5207\u5e26\uff1b<\/p>\n<p>(b) \u5757\u4f53\u538b\u7f29\u524d\u540e\u7ed3\u6784\u56e0\u5b50\u5bf9\u6bd4\uff0c\u63d2\u56fe\u4e3a\u7b2c\u4e00\u884d\u5c04\u5cf0\u7684\u653e\u5927\uff1b<\/p>\n<p>(c) \u5757\u4f53\u538b\u7f29\u524d\u540e\u7ea6\u5316\u5bf9\u5206\u5e03\u51fd\u6570\u53ca\u6307\u6570\u62df\u5408\u7ed3\u679c\uff1b<\/p>\n<p>(d) \u538b\u7f29\u53d8\u5f62\u8fc7\u7a0b\u4e2d2\u539f\u5b50\u548c3\u539f\u5b50\u56e2\u7c07\u8fde\u63a5\u65b9\u5f0f\u7684\u53d8\u5316\uff0c\u9752\u8272\u865a\u7ebf\u4e3a\u5bf9\u5e94\u7684\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>6<\/b><\/strong><strong><b>\uff1a<\/b><\/strong>Pd<sub>82<\/sub>Si<sub>18<\/sub>\u91d1\u5c5e\u73bb\u7483\u900f\u5c04\u7535\u955c\u56fe\u7247\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-209220 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72476-5.png\" alt=\"\" width=\"600\" height=\"910\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72476-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72476-5-198x300.png 198w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a)\u672a\u53d8\u5f62\u8bd5\u6837\u9ad8\u5206\u8fa8\u900f\u5c04\u7535\u955c\u56fe\u7247\uff0c\u63d2\u56fe\u662f\u56fe\u50cf\u7684\u5feb\u901f\u5085\u7acb\u53f6\u53d8\u6362\uff1b<\/p>\n<p>(b) \u5f2f\u66f2\u53d8\u5f62\u540e\u8bd5\u6837\u9ad8\u5206\u8fa8\u900f\u5c04\u7535\u955c\u56fe\u7247\uff0c\u63d2\u56fe\u662f\u56fe\u50cf\u7684\u5feb\u901f\u5085\u7acb\u53f6\u53d8\u6362\uff1b\u7535\u955c\u7ed3\u679c\u663e\u793a\u6837\u54c1\u53d8\u5f62\u524d\u540e\u5747\u4e3a\u975e\u6676\u6001\uff1b<\/p>\n<p>(c)(e)\u5355\u8f74\u538b\u7f29\uff08\u5de5\u7a0b\u5e94\u53d8~75%\uff09\u540e\u7684TEM\u660e\u573a\u50cf\u3002\uff08e\uff09\u56fe\u9ec4\u8272\u7bad\u5934\u8868\u793a\u9760\u8fd1\u526a\u5207\u5e26\u8fb9\u7f18\u7684\u8f83\u5927\u5c3a\u5ea6\u975e\u5747\u5300\u6790\u51fa\u7269\u3002\u63d2\u56fe\u662f\u6240\u9009\u533a\u57df\u7684\u7535\u5b50\u884d\u5c04\u56fe\uff1b<\/p>\n<p>(d)(f)\u540c\u4e00\u5355\u8f74\u538b\u7f29\u6837\u54c1\u7684\u57fa\u4f53\u548c\u526a\u5207\u5e26\u5c40\u90e8\u533a\u57df\uff08\u5982\u56fe6e\u4e2d\u7684\u7ea2\u65b9\u533a\u57df\u6240\u793a\uff09\u7684\u9ad8\u5206\u8fa8\u7387TEM\u56fe\u50cf\u3002\u63d2\u56fe\u662f\u6bcf\u4e2a\u56fe\u50cf\u7684\u5feb\u901f\u5085\u7acb\u53f6\u53d8\u6362\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>7<\/b><\/strong><strong><b>\uff1a<\/b><\/strong>\u53d8\u5f62\u524d\u540e\u540c\u6b65\u8f90\u5c04\u548c\u4e2d\u5b50\u5c0f\u89d2\u6563\u5c04\u7ed3\u679c\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-209221 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72477-5.png\" alt=\"\" width=\"600\" height=\"1013\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72477-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72477-5-178x300.png 178w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u5f2f\u66f2\u524d\u540e\u6837\u54c1\u7684\u540c\u6b65\u8f90\u5c04\u9ad8\u80fdX\u5c04\u7ebf\u5c0f\u89d2\u6563\u5c04\u8c31\uff08SAXS\uff09\uff1b<\/p>\n<p>(b)\u5355\u8f74\u538b\u7f29\uff08\u5de5\u7a0b\u5e94\u53d8~75%\uff09\u540e\u6837\u54c1\u7684\u5c0f\u89d2\u4e2d\u5b50\u6563\u5c04\u8c31\uff08SANS\uff09\u3002\u63d2\u56fe\u662f\u5f02\u8d28\u7ed3\u6784\u7684\u5c3a\u5bf8\u5206\u5e03\uff0c\u7ed3\u5408SAXS\u62df\u5408\u7ed3\u679c\uff0c\u5c3a\u5bf8\u4e3b\u8981\u5206\u5e03\u57282.5~20nm\uff0c\u6db5\u76d6\u4e86\u526a\u5207\u5e26\u548c\u975e\u5747\u5300\u7ed3\u6784\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>8<\/b><\/strong><strong><b>\uff1a<\/b><\/strong>Pd-Si\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u5728\u5f2f\u66f2\u53d8\u5f62\u524d\u3001\u4e2d\u95f4\u9636\u6bb5\u548c\u53d8\u5f62\u540e(a)\u539f\u5b50(b)\u7eb3\u7c73\u548c(c)\u5fae\u7c73\u5c3a\u5ea6\u975e\u5747\u5300\u6027\u6f14\u5316\u793a\u610f\u56fe\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-209222 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72478-5.png\" alt=\"\" width=\"600\" height=\"319\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72478-5.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/09\/\u56fe\u72478-5-300x160.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>(a) \u5728\u539f\u5b50\u5c3a\u5ea6\u4e0a\uff0c\u62c9\u4f38\u548c\u538b\u7f29\u5f2f\u66f2\u8fc7\u7a0b\u4e2d2\u30013\u539f\u5b50\u7684\u56e2\u7c07\u8fde\u901a\u6a21\u5f0f\u8f6c\u6362\u76f8\u53cd\uff1b<\/p>\n<p>(b) \u5728\u7eb3\u7c73\u5c3a\u5ea6\u4e0a\uff0c\u5f62\u53d8\u8fc7\u7a0b\u4e2d\uff0c\u975e\u5747\u5300\u6027\u7ed3\u6784\uff08\u975e\u6676\u76f8\u5206\u79bb\u3001\u526a\u5207\u5e26\u7ed3\u6784\uff09\u5f97\u5230\u589e\u5f3a\uff0c\u5c24\u5176\u526a\u5207\u5e26\u5728\u6269\u5c55\u8fc7\u7a0b\u4e0e\u7eb3\u7c73\u7ea7\u975e\u5747\u5300\u7ed3\u6784\u7684\u4ea4\u4e92\u4f1a\u8fdb\u4e00\u6b65\u589e\u5f3a\u8fd9\u4e00\u8fc7\u7a0b\u7684\u7d2f\u79ef\u3002\u7528\u9ed1\u8272\u7ec6\u7bad\u5934\u6307\u793a\u526a\u5207\u5e26\u7684\u6269\u5c55\u65b9\u5411\uff1b<\/p>\n<p>(c) \u5728\u5fae\u7c73\u5c3a\u5ea6\u4e0a\uff0c\u5f2f\u66f2\u53d8\u5f62\u8fc7\u7a0b\u4e2d\uff0c\u4e24\u4fa7\u5747\u6709\u5927\u91cf\u526a\u5207\u5e26\u751f\u6210\u3002\u5f2f\u66f2\u540e\u6837\u54c1\u4e2d\u7684\u8272\u5e26\u53cd\u6620\u4e86\u4ece\u62c9\u4f38\u4fa7\u5230\u538b\u7f29\u4fa7\u7684\u4e0d\u5747\u5300\u6b8b\u4f59\u5e94\u53d8\u5206\u5e03\u3002<\/p>\n<p><strong><b>\u3010\u5c0f\u7ed3\u3011<\/b><\/strong><\/p>\n<p>\u7efc\u4e0a\uff0c\u5229\u7528\u540c\u6b65\u8f90\u5c04\u9ad8\u80fdX\u5c04\u7ebf\u884d\u5c04\u548c\u5c0f\u89d2\u4e2d\u5b50\/\u540c\u6b65\u8f90\u5c04\u6563\u5c04\u6280\u672f\uff0c\u7ed3\u5408\u7535\u955c\u89c2\u6d4b\uff0c\u8be5\u5de5\u4f5c\u7cfb\u7edf\u7814\u7a76\u4e86Pd<sub>82<\/sub>Si<sub>18<\/sub>\u4e8c\u5143\u91d1\u5c5e\u73bb\u7483\u53d8\u5f62\u524d\u540e\u4ece\u539f\u5b50\u5230\u7eb3\u7c73\u5230\u5fae\u7c73\u5c3a\u5ea6\u7ed3\u6784\u54cd\u5e94\u3002\u5b9e\u9a8c\u7ed3\u679c\u8868\u660e\uff0c\u53d8\u5f62\u540e\u7684\u591a\u5c3a\u5ea6\u591a\u7ea7\u7ed3\u6784\u7684\u975e\u5747\u8d28\u6027\u663e\u8457\u589e\u5f3a\u3002\u5f2f\u66f2\u53d8\u5f62\u540e\u89c2\u5bdf\u5230\u9ad8\u5bc6\u5ea6\u7684\u591a\u7ea7\u526a\u5207\u5e26\uff0c\u5e76\u5bfc\u81f4\u590d\u6742\u4e14\u5468\u671f\u6027\u5206\u5e03\u7684\u6b8b\u4f59\u5e94\u53d8\u3002\u5bf9\u5206\u5e03\u51fd\u6570\u5206\u6790\u8868\u660e\uff0c\u4e2d\u7a0b\u5e8f\u5c3a\u5ea6\u4e0a\u539f\u5b50\u56e2\u7c07\u7684\u8fde\u901a\u6027\u53d8\u6362\u51b3\u5b9a\u4e86\u5f2f\u66f2\u540e\u6837\u54c1\u62c9\u4f38\u4fa7\u548c\u538b\u7f29\u4fa7\u7684\u5806\u79ef\u5bc6\u5ea6\u5dee\u5f02\u3002\u539f\u4f4d\u540c\u6b65\u8f90\u5c04X\u5c04\u7ebf\u884d\u5c04\u7814\u7a76\u8fd8\u63ed\u793a\u4e86\u77ed\u7a0b\u56e2\u7c07\u5728\u5355\u8f74\u62c9\u4f38\u548c\u538b\u7f29\u4f5c\u7528\u4e0b\u7684\u8fde\u63a5\u6a21\u5f0f\u7684\u5bf9\u5e94\u53d8\u5316\uff0c\u8fd9\u4e0e\u5f2f\u66f2\u524d\u540e\u7684Pd<sub>82<\/sub>Si<sub>18<\/sub>\u73bb\u7483\u5408\u91d1\u4e2d\u62c9\u4f38\/\u538b\u7f29\u90e8\u4f4d\u7684\u8fde\u63a5\u6a21\u5f0f\u8f6c\u53d8\u4e00\u81f4\u3002\u5c0f\u89d2\u6563\u5c04\u548c\u900f\u5c04\u7535\u955c\u89c2\u5bdf\u5230\u91d1\u5c5e\u73bb\u7483\u53d8\u5f62\u540e\u660e\u663e\u589e\u5f3a\u7684\u7eb3\u7c73\u975e\u5747\u5300\u6027\uff0c\u5176\u539f\u56e0\u53ef\u80fd\u662f\u7531\u4e8e\u7eb3\u7c73\u5c3a\u5ea6\u7684\u975e\u6676\u76f8\u5206\u79bb\u548c\u5851\u6027\u53d8\u5f62\u589e\u5f3a\u7684\u591a\u7ea7\u526a\u5207\u5e26\u76f8\u4e92\u4f5c\u7528\u7684\u7ed3\u679c\u3002\u7814\u7a76\u7ed3\u679c\u8868\u660e\uff0c\u5728\u591a\u5c3a\u5ea6\u4e0a\u591a\u7ea7\u975e\u5747\u5300\u7ed3\u6784\u7684\u5f3a\u5316\u53ef\u4ee5\u89e3\u91caPd-Si\u73bb\u7483\u5408\u91d1\u5177\u6709\u826f\u597d\u7684\u5851\u6027\u53ca\u52a0\u5de5\u786c\u5316\u73b0\u8c61\uff0c\u6709\u52a9\u4e8e\u52a0\u6df1\u4eba\u4eec\u5bf9\u91d1\u5c5e\u73bb\u7483\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u7ed3\u6784-\u6027\u80fd\u5173\u7cfb\u7684\u7406\u89e3\u3002<\/p>\n<p><strong><b>\u3010\u6587\u732e\u8fde\u63a5\u3011<\/b><\/strong><\/p>\n<p>S.N. Liu<sup>#<\/sup>, L.F. Wang<sup>#<\/sup>, J.C. Ge, Z.D. Wu, Y.B. Ke, Q. Li, B.A. Sun, T. Feng, Y. Wu, J.T. Wang, H. Hahn, J.D. Almer, X.-L. Wang, S. Lan*. Deformation-enhanced hierarchical multiscale structure heterogeneity in a Pd-Si bulk metallic glass[J]. Acta Materialia 200, 2020, pp. 42-55. https:\/\/doi.org\/10.1016\/j.actamat.2020.08.077<\/p>\n<p><strong><b>\u3010\u81f4\u8c22\u3011<\/b><\/strong><\/p>\n<p>\u672c\u8bba\u6587\u7814\u7a76\u5de5\u4f5c\u83b7\u5f97\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u652f\u6301<\/p>\n<p><strong><b>\u3010\u5170\u53f8\u6559\u6388\u7b80\u4ecb\u3011<\/b><\/strong><\/p>\n<p>\u73b0\u4efb\u5357\u4eac\u7406\u5de5\u5927\u5b66\u6750\u6599\u79d1\u5b66\u4e0e\u5de5\u7a0b\u5b66\u9662\/\u683c\u83b1\u7279\u7814\u7a76\u9662\u9662\u957f\u52a9\u7406\u3001\u526f\u6240\u957f\u3001\u6559\u6388\uff0c\u83b7\u5f97\u6c5f\u82cf\u7701\u6770\u51fa\u9752\u5e74\u57fa\u91d1\u548c\u56fd\u5bb6\u81ea\u7136\u79d1\u5b66\u57fa\u91d1\u9762\u4e0a\u9879\u76ee\u8d44\u52a9\uff0c\u4e00\u76f4\u4ece\u4e8b\u5927\u5757\u91d1\u5c5e\u73bb\u7483\u53ca\u5f62\u6210\u6db2\u4f53\u4e2d\u6db2\u6001\u76f8\u53d8\u76f8\u5173\u9886\u57df\u7684\u7814\u7a76\u5de5\u4f5c\uff0c\u81ea\u535a\u58eb\u3001\u535a\u58eb\u540e\u3001\u4ee5\u53ca\u5de5\u4f5c\u4ee5\u6765\uff0c\u4ee5\u540c\u6b65\u8f90\u5c04\u548c\u4e2d\u5b50\u6563\u5c04\u53ca\u900f\u5c04\u7535\u955c\u7b49\u5148\u8fdb\u7814\u7a76\u624b\u6bb5\uff0c\u5728\u4e00\u7cfb\u5217\u91d1\u5c5e\u73bb\u7483\u5408\u91d1\u4f53\u7cfb\u6db2-\u6db2\u76f8\u53d8\u7684\u5fae\u89c2\u673a\u5236\u539f\u4f4d\u6563\u5c04\u7814\u7a76\u7b49\u8bfe\u9898\u4e0a\u505a\u51fa\u4e86\u91cd\u8981\u7684\u7814\u7a76\u6210\u679c\uff0c\u5728Nature Communications, Communications Physics, Acta Materialia\uff0cPhysicalReviewLetters\u3001ScriptaMaterialia\u7b49\u53d1\u8868\u91cd\u8981\u8bba\u658760\u4f59\u7bc7\uff0c\u5177\u6709\u4e30\u5bcc\u7684\u76f8\u5173\u7814\u7a76\u7ecf\u9a8c\u3002\u5173\u4e8e\u94af-\u954d-\u78f7\u975e\u6676\u5408\u91d1\u7684\u9690\u85cf\u6db2\u6001\u76f8\u53d8\u7684\u7814\u7a76\u5de5\u4f5c\u4e8e2017\u5e74\u53d1\u8868\u5728\u56fd\u9645\u6743\u5a01\u6742\u5fd7\u81ea\u7136\u901a\u8baf\u4e0a\uff0c\u88ab\u57fa\u91d1\u59d4\u9996\u9875\u4ee5\u8981\u95fb\u62a5\u9053\uff0c\u540c\u65f6\u88ab\u81ea\u7136\u901a\u8baf\u6742\u5fd7\u51b6\u91d1\u4e13\u680f\u6536\u85cf\u3002\u7531\u4e8e\u53d6\u5f97\u7684\u4e00\u7cfb\u5217\u7814\u7a76\u6210\u679c\uff0c\u8fd8\u83b7\u5f97\u6c5f\u82cf\u7701333\u9ad8\u5c42\u6b21\u4eba\u624d\u8ba1\u5212\u3001\u516d\u5927\u4eba\u624d\u9ad8\u5cf0\u4eba\u624d\u8ba1\u5212\u3001\u53cc\u521b\u535a\u58eb\u8ba1\u5212\u652f\u6301\u3002\u56e0\u4e3a\u91d1\u5c5e\u73bb\u7483\u7ed3\u6784\u548c\u5408\u91d1\u6db2\u4f53\u65b9\u9762\u7684\u7a81\u51fa\u5de5\u4f5c\uff0c2017\u5e747\u6708\u83b7\u5f97\u4e2d\u56fd\u6750\u6599\u5927\u4f1a\u975e\u6676\u5408\u91d1\u201c\u6770\u51fa\u9752\u5e74\u79d1\u5b66\u5bb6\u5956\u201d\u30022017\u5e748\u6708\u7ec4\u7ec7\u56fd\u9645\u77e5\u540d\u7684\u6208\u767b\u7814\u8ba8\u4f1a\uff08GRS\uff09\u4e2d\u5b50\u6563\u5c04\u7814\u8ba8\u4f1a\u5e76\u4f5c\u9080\u8bf7\u62a5\u544a\u3002<\/p>\n<p>\u672c\u6587\u7531\u5357\u4eac\u7406\u5de5\u5927\u5b66\u5170\u53f8\u6559\u6388\u8bfe\u9898\u7ec4\u4f9b\u7a3f\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u957f\u671f\u4ee5\u6765\uff0c\u91d1\u5c5e\u73bb\u7483\u5851\u6027\u7684\u7ed3\u6784\u8d77\u6e90\u4ee5\u53ca\u7ed3\u6784\u54cd\u5e94\u4e00\u76f4\u60ac\u800c\u672a\u51b3\uff0c\u5176\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u7ed3\u6784-\u6027\u80fd\u5173\u8054\u673a\u5236\u4ecd\u4e0d\u6e05\u695a\uff0c\u56e0\u6b64\u7814\u7a76\u91d1\u5c5e\u73bb\u7483\u5851\u6027\u53d8\u5f62\u8fc7\u7a0b\u4e2d\u591a\u5c3a\u5ea6\u591a\u7ea7\u7ed3\u6784\u6f14\u53d8&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[],"class_list":["post-209214","post","type-post","status-publish","format-standard","hentry","category-jiedu"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/209214"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=209214"}],"version-history":[{"count":4,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/209214\/revisions"}],"predecessor-version":[{"id":209256,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/209214\/revisions\/209256"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=209214"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=209214"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=209214"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}