{"id":211430,"date":"2020-10-23T06:30:11","date_gmt":"2020-10-22T22:30:11","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=211430"},"modified":"2020-10-22T21:30:21","modified_gmt":"2020-10-22T13:30:21","slug":"%e8%b7%9f%e7%9d%80%e9%a1%b6%e5%88%8a%e5%ad%a6%e6%b5%8b%e8%af%95%ef%bd%9c%e5%8d%97%e7%a7%91%e5%a4%a7adv-mater%ef%bc%9a%e5%8e%9f%e4%bd%8d%e9%80%8f%e5%b0%84%e7%94%b5%e9%95%9c%e6%8f%ad%e7%a4%ba%e6%b6%b2","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=211430","title":{"rendered":"\u8ddf\u7740\u9876\u520a\u5b66\u6d4b\u8bd5\uff5c\u5357\u79d1\u5927Adv. Mater\uff1a\u539f\u4f4d\u900f\u5c04\u7535\u955c\u63ed\u793a\u6db2\u6001\u9502\u91d1\u5c5e\u8d1f\u6781\u7684\u6210\u6838\u8fc7\u7a0b"},"content":{"rendered":"<p>\u79fb\u52a8\u7535\u5b50\u3001\u7269\u8054\u7f51\u548c\u7535\u52a8\u6c7d\u8f66\u7684\u5feb\u901f\u53d1\u5c55\uff0c\u5bf9\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7684\u53ef\u5145\u7535\u7535\u6c60\u63d0\u51fa\u4e86\u66f4\u9ad8\u7684\u8981\u6c42\uff0c\u800c\u8fd9\u4f9d\u8d56\u4e8e\u66f4\u597d\u7684\u7535\u6781\u3001\u7535\u89e3\u8d28\u548c\u754c\u9762\u3002\u5728\u6240\u6709\u53ef\u80fd\u7684\u9633\u6781\u5019\u9009\u6750\u6599\u4e2d\uff0c\u9502\u91d1\u5c5e\u7531\u4e8e\u5176\u8d85\u9ad8\u7684\u6bd4\u5bb9\u91cf\uff083860 mAh g<sup>\u22121<\/sup>\uff09\u3001\u91cd\u91cf\u8f7b\uff080.53 g cm<sup>\u20133<\/sup>\uff09\u548c\u66f4\u4f4e\u7684\u7535\u5316\u5b66\u7535\u4f4d\uff0c\u662f\u65e0\u4e89\u8bae\u7684\u6700\u7ec8\u9009\u62e9\u3002\u7528\u9502\u91d1\u5c5e\u4ee3\u66ff\u9502\u79bb\u5b50\u7535\u6c60\u4e2d\u7684\u77f3\u58a8\u9633\u6781\u5c06\u4f7f\u80fd\u91cf\u5bc6\u5ea6\u7acb\u5373\u589e\u52a040%\u3002\u5728\u66f4\u5e7f\u6cdb\u7684\u80cc\u666f\u4e0b\uff0c\u9502\u9633\u6781\u4e5f\u662f\u4e0b\u4e00\u4ee3\u6982\u5ff5\u7535\u6c60\u5316\u5b66\u4e2d\u4e0d\u53ef\u6216\u7f3a\u7684\u7ec4\u6210\u90e8\u5206\uff0c\u4f8b\u5982\uff0c\u9502-\u786b\u548c\u9502-\u7a7a\u6c14\u7535\u6c60\uff0c\u5176\u80fd\u91cf\u5bc6\u5ea6\u9884\u8ba1\u5c06\u5206\u522b\u8d85\u8fc7370\u548c1700 Wh kg<sup>\u22121<\/sup>\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-211431 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-1-6.png\" alt=\"\" width=\"600\" height=\"254\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-1-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-1-6-300x127.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u8fd1\u65e5\uff0c\u5357\u65b9\u79d1\u6280\u5927\u5b66<strong><b>\u9093\u6c38\u7ea2<\/b><\/strong>\u8bfe\u9898\u7ec4\u548c\u9999\u6e2f\u7406\u5de5\u5927\u5b66<strong><b>\u90d1\u5b50\u5251<\/b><\/strong>\u6559\u6388\u5408\u4f5c\u4ee5\u201c500 Wh kg<sup>\u22121<\/sup>\u00a0Class Li Metal Battery Enabled by a Self-Organized Core\u2013Shell Composite Anode\u201d\u4e3a\u9898\u5728<em><i>Adv. Mater.<\/i><\/em>\u671f\u520a\u4e0a\u53d1\u8868\u91cd\u8981\u7814\u7a76\u6210\u679c\u3002\u8be5\u56e2\u961f\u7814\u5236\u4e86\u4e00\u79cd\u81ea\u7ec4\u7ec7\u6838\u58f3\u7ed3\u6784\u7684\u590d\u5408\u9633\u6781\uff0c\u8be5\u9633\u6781\u7531\u9502\u5316\u6db2\u6001\u91d1\u5c5e\uff08Li<sub>x<\/sub>LM<sub>y<\/sub>\uff09\u5916\u4fdd\u62a4\u5c42\u548c\u9502\u91d1\u5c5e\u5185\u5c42\u7ec4\u6210\uff0c\u5177\u6709\u8f83\u9ad8\u7684\u7535\u5b50\u5bfc\u7535\u6027\u548c\u79bb\u5b50\u5bfc\u7535\u6027\uff0c\u5e76\u5c06\u9502\u4e0e\u7535\u89e3\u6db2\u8fdb\u884c\u7269\u7406\u5206\u79bb\u3002Li<sub>x<\/sub>LM<sub>y<\/sub>\u7684\u5f15\u5165\u4e0d\u4ec5\u9632\u6b62\u4e86\u9502\u679d\u6676\u7684\u5f62\u6210\uff0c\u800c\u4e14\u6d88\u9664\u4e86\u94dc\u4f5c\u4e3a\u60f0\u6027\u886c\u5e95\u7684\u4f7f\u7528\u3002\u8fd9\u79cd\u590d\u5408\u9633\u6781\u548c\u5546\u4e1a\u5316\u7684LiNi<sub>0.6<\/sub>Co<sub>0.2<\/sub>Mn<sub>0.2<\/sub>O<sub>2<\/sub>\uff08NCM622\uff09\u9634\u6781\u7ec4\u88c5\u6210\u7684\u5168\u7535\u6c60\u53ef\u63d0\u4f9b1500 Wh L<sup>\u22121<\/sup>\u548c483 Wh kg<sup>\u22121<\/sup>\u7684\u8d85\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u3002\u9ad8\u5bb9\u91cf\u53ef\u7ef4\u6301500\u4e2a\u5faa\u73af\u4ee5\u4e0a\uff0c\u6bcf\u5faa\u73af\u8870\u51cf\u7387\u5c0f\u4e8e0.05%\u3002\u4e0eLiNi<sub>0.8<\/sub>Co<sub>0.1<\/sub>Mn<sub>0.1<\/sub>O<sub>2<\/sub>\uff08NCM811\uff09\u914d\u5408\u4f7f\u7528\u53ef\u8fdb\u4e00\u6b65\u63d0\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u81f31732 Wh L<sup>\u22121<\/sup>\u548c514 Wh kg<sup>\u22121<\/sup>\u3002<\/p>\n<p>\u8fd9\u79cd\u81ea\u7ec4\u7ec7\u590d\u5408\u7535\u6781(\u79f0\u4e3aLi\/Li<sub>x<\/sub>LM<sub>y<\/sub>)\u662f\u901a\u8fc7LM\u4e00\u6b65\u9502\u5316\u5f62\u6210\u7684\u3002\u7b80\u800c\u8a00\u4e4b\uff0c\u5728\u73af\u5883\u6761\u4ef6\u4e0b\uff0c\u5c06\u539a\u5ea6\u4e3a5 \u03bcm\u7684LM (GaInSn)\u65cb\u6d82\u5230\u5546\u4e1a\u5316\u7684\u805a\u4e19\u70ef(PP)\u9694\u819c\u4e0a(\u56fe1a)\u3002\u7531\u4e8eLM\u5177\u6709\u826f\u597d\u7684\u6d41\u52a8\u6027\uff0c\u6d82\u5c42\u5728PP\u4e0a\u81f4\u5bc6\u4e14\u5747\u5300(\u56fe1b,c)\uff0c\u6613\u4e8e\u5927\u89c4\u6a21\u5236\u5907\u3002\u4f5c\u8005\u7ec4\u88c5\u4e86\u4e00\u4e2a\u7531LM\/PP\u548cLi\u7b94\u7ec4\u6210\u7684\u7535\u6c60\uff0c\u7136\u540e\u653e\u7535\u5bfc\u81f4Li\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u7684\u81ea\u53d1\u5f62\u6210(\u56fe1d)\u3002\u53ef\u4ee5\u770b\u51fa\uff0c\u57280.75 mAh cm<sup>\u22122<\/sup>\u7684\u653e\u7535\u8fc7\u7a0b\u4e2d\uff0c\u7535\u5316\u5b66\u7535\u4f4d\u8fc5\u901f\u4e0b\u964d\uff0c\u5728\u968f\u540e\u7684\u653e\u7535\u8fc7\u7a0b\u4e2d\uff0c\u653e\u7535\u7535\u4f4d\u8d8b\u4e8e\u7a33\u5b9a\u3002\u7531\u4e8eGa\u5728LM\u4e2d\u5feb\u901f\u6c27\u5316\uff0c\u5728PP\u548cLM\u4e4b\u95f4\u7684\u754c\u9762\u4e0a\u53d1\u73b0\u4e86\u4e00\u5c42\u8584\u8584\u7684Ga<sub>2<\/sub>O<sub>3<\/sub>(\u56fe1e)\u3002\u5728\u9502\u5316\u8fc7\u7a0b\u7684\u65e9\u671f\u9636\u6bb5\uff0cLM\u4e0eLi\u5408\u91d1\u5316\u5f97\u5230Li<sub>x<\/sub>LM<sub>y<\/sub>(\u56fe1f,i)\uff0c\u653e\u7535\u7535\u538b\u4ece1.0 V\u964d\u81f30.01 V\u53ef\u4ee5\u8bc1\u660e\u8fd9\u4e00\u70b9(\u56fe1d)\u3002\u5f53Li\/LM\u6bd4\u22482.5\u65f6\uff0c\u5408\u91d1\u8fbe\u5230\u9971\u548c\u3002<\/p>\n<p><strong><b>\u56fe1. \u590d\u5408\u7535\u6781<\/b><\/strong><strong><b>(Li\/Li<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>LM<\/b><\/strong><strong><sub><b>y<\/b><\/sub><\/strong><strong><b>)\u7684\u5f62\u6210<\/b><\/strong><strong><b>\u3002<\/b><\/strong><\/p>\n<p><strong><b><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-211432 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-5-2.png\" alt=\"\" width=\"457\" height=\"522\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-5-2.png 457w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-5-2-263x300.png 263w\" sizes=\"(max-width: 457px) 100vw, 457px\" \/><\/b><\/strong><\/p>\n<p>\u4f5c\u8005\u91c7\u7528\u539f\u4f4d\u900f\u5c04\u7535\u955c\u76f4\u63a5\u89c2\u5bdfLi\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u7684\u5f62\u6210\u3002\u5b9a\u5236\u7684STM\u652f\u67b6\u7531\u6d82\u6709\u9502\u7684\u94a8\u9488\u7535\u6781\u548c\u78b3\u652f\u6491\u7684\u94dc\u7f51\u683c\u4e0a\u7684LM\u6db2\u6ef4\u7ec4\u6210(\u56fe2a,b)\u3002\u5728\u539f\u4f4d\u900f\u5c04\u7535\u955c\u6280\u672f\u4e2d\uff0cLi\u8868\u9762\u7684\u539f\u751f\u6c34\u4f5c\u4e3a\u56fa\u6001\u7535\u89e3\u8d28\uff0c\u9488\u4e0eLM\u63a5\u89e6\u4ee5\u5f62\u6210\u540e\u8005\u3002\u7ecf\u8fc715 s\u7684\u9502\u5316\u540e\uff0cLM\u7684\u5916\u90e8\u533a\u57df\u53d8\u5f97\u66f4\u4eae\uff0c\u572825 s\u65f6\u6574\u4e2aLM\u7c92\u5b50\u88abLi\u5b8c\u5168\u9971\u548c\uff0c\u5f62\u6210Li<sub>x<\/sub>LM<sub>y<\/sub>(\u56fe2c)\u3002\u4e4b\u540eLi<sup>0<\/sup>\u5f00\u59cb\u5728GaLi\u57fa\u8d28\u4e2d\u6210\u6838(33 s)\uff0c\u751f\u957f(40 s)\uff0c\u5f62\u6210Li\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u3002\u9ad8\u89d2\u5ea6\u73af\u5f62\u6697\u573a(HAADF)\u548c\u7535\u5b50\u80fd\u91cf\u635f\u5931\u8c31(EELS)\u5206\u6790\u8fdb\u4e00\u6b65\u8bc1\u5b9e\u4e86\u5728Li\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u5916\u56f4\u533a\u57df\u5b58\u5728\u5bcc\u9553\u76f8\u4ee5\u53caLi\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u4e2d\u95f4\u7684Sn\/In\u76f8\u548cLi(\u56fe2d,e,g)\u3002\u56fe2c \u4e2d33\u548c40 s\u7ea2\u70b9\u533a\u57df\u7684\u9ed1\u70b9\u4ee3\u8868Sn\u548cIn\uff0c\u56fe2c\u4e2d40 s\u84dd\u70b9\u533a\u57df\u7684\u9ed1\u70b9\u5468\u56f4\u7684\u4eae\u70b9\u5e94\u8be5\u662fLi<sup>0<\/sup>\uff0c\u8fd9\u4e5f\u5bf9\u5e94\u4e8e\u56fe2e\u4e2d\u7684EELS\u6620\u5c04\u3002\u975e\u539f\u4f4d\u548c\u539f\u4f4d\u7684\u7814\u7a76\u90fd\u8bc1\u5b9e\u4e86\u81ea\u7ec4\u7ec7\u7684\u590d\u5408\u7ed3\u6784\u3002<\/p>\n<p><strong><b>\u56fe2<\/b><\/strong><strong><b>.<\/b><\/strong><strong><b>\u00a0\u7528\u539f\u4f4d\u900f\u5c04\u7535\u955c\u548c<\/b><\/strong><strong><b>X\u5c04\u7ebf\u7814\u7a76Li\/Li<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>LM<\/b><\/strong><strong><sub><b>y<\/b><\/sub><\/strong><strong><b>\u5f62\u6210\u7684\u81ea\u7ec4\u7ec7\u8fc7\u7a0b<\/b><\/strong><strong><b>\u3002<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-211433 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-6-4.png\" alt=\"\" width=\"583\" height=\"508\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-6-4.png 583w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-6-4-300x261.png 300w\" sizes=\"(max-width: 583px) 100vw, 583px\" \/><\/p>\n<p>\u590d\u5408\u6750\u6599\u7ed3\u6784\u7684\u9ad8\u53ef\u9006\u6027\u786e\u4fdd\u4e86Li\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u5728\u5e38\u89c4\u6db2\u4f53\u7535\u89e3\u8d28\uff081 M LiPF<sub>6<\/sub>\u5728EC:DMC\uff081:1 vol%\uff09\u548c1 wt%VC\uff09\u4e2d\u7684\u957f\u671f\u5faa\u73af\u7a33\u5b9a\u6027\u3002\u590d\u5408\u7535\u6781\uff08Li\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u00a0| Li\/Li<sub>x<\/sub>LM<sub>y<\/sub>\uff09\u7684\u5bf9\u79f0\u7535\u6c60\u57280.5\u62161.0 mA cm<sup>\u22122<\/sup>\u7684\u7535\u6d41\u5bc6\u5ea6\u4e0b\u5b8c\u5168\u5145\u7535\u548c\u653e\u7535\uff08\u56fe3a\u2013e\uff09\uff0c\u4ee5\u4e00\u5bf9Li\/Cu\u7535\u6781\u5236\u6210\u7684\u5bf9\u79f0\u7535\u6c60\u4f5c\u4e3a\u53c2\u8003\u3002\u5728\u6240\u6709\u8bd5\u9a8c\u4e2d\uff0cLi\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u663e\u793a\u51fa\u6bd4\u53c2\u8003\u503c\u4f4e\u7684\u8fc7\u7535\u4f4d\u548c\u66f4\u597d\u7684\u5faa\u73af\u7a33\u5b9a\u6027\u3002\u4f8b\u5982\uff0c\u5728\u8d85\u8fc73700\u5c0f\u65f6\u7684\u5145\u653e\u7535\u8bd5\u9a8c\u4e2d\uff0cLi\/Li<sub>x<\/sub>LM<sub>y<\/sub>\uff082.0 mAh cm<sup>\u22122<\/sup>\uff09\u7684\u8fc7\u7535\u4f4d\u5c0f\u4e8e30 mV\uff08\u56fe3b\uff09\u3002\u590d\u5408\u7535\u6781\u7684\u65e0\u679d\u6676\u8868\u9762\u4fdd\u6301\u4e86\u826f\u597d\u7684\u4f4e\u7c97\u7cd9\u5ea6\u6c34\u5e73\uff08\u56fe3f\uff0cg\uff09\u3002\u4e0e\u6b64\u5f62\u6210\u9c9c\u660e\u5bf9\u6bd4\u7684\u662f\uff0c\u5728\u76f8\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0cLi\/Cu\u7684\u8fc7\u7535\u4f4d\u9ad8\u51fa\u4e00\u500d\uff0c\u5e76\u4e14\u5728SEM\u4e0b\u89c2\u5bdf\u5230\u82d4\u85d3\u72b6Li\u7684\u5f62\u6210\uff08\u56fe3h\uff0ci\uff09\u3002Li\/Cu\u7535\u6c60\u5728\u22481200\u5c0f\u65f6\u53d1\u751f\u77ed\u8def\uff08\u56fe3b\uff09\u3002<\/p>\n<p><strong><b>\u56fe3<\/b><\/strong><strong><b>.<\/b><\/strong><strong><b>\u00a0<\/b><\/strong><strong><b>Li\/Li<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>LM<\/b><\/strong><strong><sub><b>y<\/b><\/sub><\/strong><strong><b>\u957f\u5faa\u73af\u5bff\u547d\u7684\u7535\u5316\u5b66\u8868\u5f81\u3002<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-211434 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-7-4.png\" alt=\"\" width=\"435\" height=\"573\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-7-4.png 435w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-7-4-228x300.png 228w\" sizes=\"(max-width: 435px) 100vw, 435px\" \/><\/p>\n<p>Li\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u4e2d\u679d\u6676\u7684\u6d88\u5931\u5f97\u76ca\u4e8e\u4e24\u4e2a\u56e0\u7d20\u7684\u7ed3\u5408\uff1a\u5bfc\u7535\u4fdd\u62a4\u5c42\u548c\u6709\u6548\u7684\u7269\u7406\u963b\u9694\u3002\u9996\u5148\uff0cGaLi\u57fa\u4f53\u63d0\u4f9b\u4e86\u4e00\u4e2a\u9ad8\u79bb\u5b50\u548c\u9ad8\u5bfc\u7535\u6027\u7684\u73af\u5883\uff0c\u8fd9\u662f\u6d88\u9664\u679d\u6676\u548c\u6b7b\u9502\u7684\u6839\u672c\u539f\u56e0\uff0c\u5373\u9502\u8868\u9762SEI\u5316\u5b66\u548c\u5f62\u8c8c\u7684\u4e0d\u5747\u5300\u6027\u3002\u8fd9\u6837\u7684\u5bfc\u7535\u5c42\u4e3a\u9502\u6c89\u79ef\u63d0\u4f9b\u4e86\u673a\u4f1a\uff0c\u56e0\u6b64\u51fa\u73b0\u4e86\u9502\u7684\u5404\u5411\u540c\u6027\u6210\u6838\u548c\u5747\u5300\u751f\u957f\u8fc7\u7a0b\uff08\u56fe4a\uff09\u3002\u6839\u636e\u963b\u6297\u5206\u6790\u5f97\u51fa\u7684GaLi\u9798\u5c42\u7684\u79bb\u5b50\u7535\u5bfc\u7387\u5728\u5faa\u73af\u8fc7\u7a0b\u4e2d\u4fdd\u6301\u5728\u5927\u4e8e1.0\u00d710<sup>\u22123<\/sup>\u00a0S cm<sup>\u22121<\/sup>\u7684\u503c\uff08\u56fe4b\uff09\uff0c\u8fd9\u8868\u660eGaLi\u4e2d\u7684Li<sup>+<\/sup>\u5feb\u901f\u4f20\u8f93\u52a8\u529b\u5b66\u3002\u7528\u6807\u51c6\u8303\u5fb7\u5821\u6cd5\u6d4b\u91cf\u7684GaLi\u7684\u7535\u5bfc\u7387\u4e5f\u663e\u793a\u4e863.63\u00d710<sup>3<\/sup>\u00a0S cm<sup>\u22121<\/sup>\u7684\u9ad8\u503c\uff08\u56fe4c\uff09\u3002\u5229\u7528\u7535\u5bfc\u7387\u53c2\u6570\uff0c\u4f5c\u8005\u8fd8\u6a21\u62df\u4e86\u9502\u79bb\u5b50\u5728Li<sub>x<\/sub>LM<sub>y<\/sub>\u548c\u4f20\u7edf\u94dc\u7b94\u4e0a\u7684\u6c89\u79ef\u8fc7\u7a0b\u3002\u5bf9\u4e8e\u524d\u8005\uff0c\u5c0f\u7684\u9502\u539f\u5b50\u6838\u51fa\u73b0\u5728Li<sub>x<\/sub>LM<sub>y<\/sub>\u7684\u57fa\u4f53\u4e2d\uff0c\u7136\u540e\u6210\u957f\u4e3a\u66f4\u5927\u7684\u7c92\u5b50\uff0c\u7136\u540e\u5408\u5e76\u6210\u4e00\u4e2a\u8fde\u7eed\u7684Li<sup>0<\/sup>\u8584\u819c\uff08\u56fe4d\uff09\u3002<\/p>\n<p><strong><b>\u56fe<\/b><\/strong><strong><b>4.<\/b><\/strong>\u00a0<strong><b>Li\/Li<\/b><\/strong><strong><sub><b>x<\/b><\/sub><\/strong><strong><b>LM<\/b><\/strong><strong><sub><b>y<\/b><\/sub><\/strong><strong><b>\u65e0\u679d\u6676\u7279\u6027\u7684\u7814\u7a76<\/b><\/strong><strong><b>\u3002<\/b><\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-211435 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-8-4.png\" alt=\"\" width=\"600\" height=\"461\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-8-4.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/10\/\u56fe\u7247-8-4-300x231.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u4f5c\u8005\u62a5\u9053\u4e86\u4e00\u79cd\u81ea\u7ec4\u7ec7\u590d\u5408\u7535\u6781Li\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u3002Li\u9996\u5148\u4e0eLM\u5408\u91d1\u5f62\u6210\u79bb\u5b50\u5bfc\u7535Li<sub>x<\/sub>LM<sub>y<\/sub>\u9798\u5c42\uff0c\u7136\u540e\u5728\u9798\u5c42\u4e0b\u6210\u6838\u751f\u957f\u4e3a\u8fde\u7eed\u7684Li<sup>0<\/sup>\u91d1\u5c5e\u819cLi<sub>x<\/sub>LM<sub>y<\/sub>\uff0c\u5728\u53cd\u590d\u7684\u7535\u5316\u5b66\u5faa\u73af\u8fc7\u7a0b\u4e2d\u8d77\u5230\u4fdd\u62a4Li\u7684\u4f5c\u7528\u3002\u8fd9\u79cd\u5bfc\u7535\u4fdd\u62a4\u5c42\u4e0d\u4ec5\u4e3a\u5747\u5300\u65e0\u679d\u6676Li\u6c89\u79ef\u63d0\u4f9b\u4e86\u4e00\u4e2a\u5404\u5411\u540c\u6027\u7684\u73af\u5883\uff0c\u800c\u4e14\u901a\u8fc7\u5c06Li<sup>0<\/sup>\u4e0e\u7535\u89e3\u6db2\u9694\u79bb\u6765\u7a33\u5b9aLi<sup>0<\/sup>\u3002\u56e0\u6b64\uff0c\u4f7f\u7528\u78b3\u9178\u76d0\u57fa\u7535\u89e3\u8d28\u65f6\uff0cLi\/Li<sub>x<\/sub>LM<sub>y<\/sub>\u7684\u5e93\u4ed1\u6548\u7387\u8fbe\u523099%\u4ee5\u4e0a\u3002\u66f4\u91cd\u8981\u7684\u662f\uff0c\u7531\u4e8eLi<sub>x<\/sub>LM<sub>y<\/sub>\u7684\u9ad8\u5bfc\u7535\u6027\uff0c\u7535\u6c60\u7ec4\u4ef6\u4e2d\u4e0d\u518d\u9700\u8981\u94dc\u7b94\uff0c\u8fd9\u5e26\u6765\u4e86\u989d\u5916\u7684\u597d\u5904\uff0c\u51cf\u5c11\u60f0\u6027\u8d28\u91cf\u548c\u4f53\u79ef\u5728\u7535\u6c60\u6c34\u5e73\u3002<\/p>\n<p>\u6587\u732e\u94fe\u63a5\uff1a500 Wh kg<sup>\u22121<\/sup>\u00a0Class Li Metal Battery Enabled by a Self-Organized Core\u2013Shell Composite Anode,\u00a0<strong><em><b><i>Adv. Mater.<\/i><\/b><\/em><\/strong>\u00a02020, 2004793.\u00a0DOI:\u00a010.1002\/adma.202004793.<\/p>\n<p>\u539f\u6587\u94fe\u63a5\uff1ahttps:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.202004793.<\/p>\n<p>\u672c\u6587\u7531\u79d1\u7814\u767e\u6653\u751f\u4f9b\u7a3f\u3002<\/p>\n<p>\u672c\u5185\u5bb9\u4e3a\u4f5c\u8005\u72ec\u7acb\u89c2\u70b9\uff0c\u4e0d\u4ee3\u8868\u6750\u6599\u4eba\u7f51\u7acb\u573a\u3002<\/p>\n<p>\u672a\u7ecf\u5141\u8bb8\u4e0d\u5f97\u8f6c\u8f7d\uff0c\u6388\u6743\u4e8b\u5b9c\u8bf7\u8054\u7cfbkefu@cailiaoren.com\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u79fb\u52a8\u7535\u5b50\u3001\u7269\u8054\u7f51\u548c\u7535\u52a8\u6c7d\u8f66\u7684\u5feb\u901f\u53d1\u5c55\uff0c\u5bf9\u9ad8\u80fd\u91cf\u5bc6\u5ea6\u7684\u53ef\u5145\u7535\u7535\u6c60\u63d0\u51fa\u4e86\u66f4\u9ad8\u7684\u8981\u6c42\uff0c\u800c\u8fd9\u4f9d\u8d56\u4e8e\u66f4\u597d\u7684\u7535\u6781\u3001\u7535\u89e3\u8d28\u548c\u754c\u9762\u3002\u5728\u6240\u6709\u53ef\u80fd\u7684\u9633\u6781\u5019\u9009\u6750\u6599\u4e2d\uff0c\u9502\u91d1\u5c5e\u7531\u4e8e\u5176\u8d85\u9ad8&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-211430","post","type-post","status-publish","format-standard","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/211430"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=211430"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/211430\/revisions"}],"predecessor-version":[{"id":211437,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/211430\/revisions\/211437"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=211430"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=211430"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=211430"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}