{"id":212320,"date":"2020-11-05T06:22:58","date_gmt":"2020-11-04T22:22:58","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=212320"},"modified":"2020-11-04T19:23:35","modified_gmt":"2020-11-04T11:23:35","slug":"%e4%bd%99%e6%a1%82%e5%8d%8e%e5%9b%a2%e9%98%9f-adv-mater-%ef%bc%9a%e8%b6%85%e4%bf%9d%e5%bd%a2%e5%92%8c%e5%8f%af%e6%8b%89%e4%bc%b8%e7%9f%b3%e5%a2%a8%e7%83%af%e8%96%84%e8%86%9c%e5%ae%9e%e7%8e%b0","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=212320","title":{"rendered":"\u4f59\u6842\u534e\u56e2\u961f Adv. Mater.\uff1a\u8d85\u4fdd\u5f62\u548c\u53ef\u62c9\u4f38\u77f3\u58a8\u70ef\u8584\u819c\u5b9e\u73b0\u9502\u91d1\u5c5e\u7535\u6c60\u4e2dLi\u9897\u7c92\u7684\u53ef\u9006\u6c89\u79ef"},"content":{"rendered":"<p><strong>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011<\/strong><\/p>\n<p>\u9502\uff08Li\uff09\u91d1\u5c5e\u5177\u6709\u6700\u4f4e\u7684\u7535\u5316\u5b66\u52bf\u548c\u6700\u9ad8\u7684\u7406\u8bba\u6bd4\u5bb9\u91cf\uff0c\u4f46\u662f\u5f53Li\u91d1\u5c5e\u66b4\u9732\u4e8e\u7535\u89e3\u8d28\u4e2d\u65f6\uff0c\u56fa\u6001\u7535\u89e3\u8d28\u4e2d\u95f4\u76f8\uff08SEI\uff09\u4f1a\u5728Li\u91d1\u5c5e\u8868\u9762\u4e0a\u5f62\u6210\u949d\u5316\u5c42\uff0c\u51fa\u73b0\u4e0d\u5747\u5300\u7684Li\u6c89\u79ef\uff0c\u5bfc\u81f4SEI\u975e\u5e73\u9762\u5f62\u6001\u53d8\u5316\u3002\u7531\u4e8eSEI\u4e0d\u53ef\u53d8\u5f62\u4e14\u6613\u788e\uff0c\u88c2\u7eb9\u4f1a\u5728\u539f\u59cbSEI\u4e0a\u6301\u7eed\u51fa\u73b0\uff0c\u5bfc\u81f4\u88c2\u7eb9\u5c40\u90e8Li\u79bb\u5b50\u5feb\u901f\u6269\u6563\uff0c\u5f15\u53d1\u65b0\u7684Li\u679d\u6676\uff0c\u751a\u81f3\u51fa\u73b0\u7206\u70b8\u548c\u706b\u707e\u4e8b\u6545\u3002\u6b64\u5916\uff0cLi\u679d\u6676\u7684\u53cd\u590d\u6c89\u79ef\/\u6eb6\u89e3\u4f1a\u6d88\u8017\u7535\u89e3\u8d28\u548cLi\u91d1\u5c5e\uff0c\u5bfc\u81f4\u5e93\u4f26\u6548\u7387\uff08CE\uff09\u4f4e\u3001\u5faa\u73af\u5bff\u547d\u77ed\u3001\u8fc7\u7535\u4f4d\u9ad8\u548c\u4f53\u79ef\u53d8\u5316\u3002\u56e0\u6b64\uff0c\u5728Li\u91d1\u5c5e\u4e0d\u65ad\u51fa\u73b0\u975e\u5e73\u9762\u7684\u5f62\u8c8c\u53d8\u5316\u8fc7\u7a0b\u4e2d\uff0c\u4e0d\u53ef\u53d8\u5f62\u7684SEI\u4e0d\u80fd\u63d0\u4f9b\u5b9e\u65f6\u4fdd\u62a4\uff0c\u8fd9\u662fLi\u679d\u6676\u548cLi\u7c89\u788e\u7684\u6839\u672c\u539f\u56e0\uff0c\u9650\u5236\u4e86\u9502\u91d1\u5c5e\u7535\u6c60\uff08LMBs\uff09\u7684\u5546\u4e1a\u5e94\u7528\u3002\u7814\u7a76\u53d1\u73b0\uff0c\u5e73\u9762\u7684\u5f62\u8c8c\u53d8\u5316\u9700\u8981Li\u79bb\u5b50\u5728\u6574\u4e2aLi\u8d1f\u6781\u8868\u9762\u5747\u5300\u6c89\u79ef\uff0c\u8981\u6ee1\u8db3\u4ee5\u4e0b\u51e0\u4e2a\u6761\u4ef6\uff1a1\uff09Li\u91d1\u5c5e\u8d1f\u6781\u8868\u9762\u5149\u6ed1\uff0c\u7535\u8377\u5206\u5e03\u5747\u5300\uff1b2\uff09SEI\u5177\u6709\u5747\u5300\u7684\u5f62\u6001\u548c\u5747\u5300\u5206\u5e03\u7684\u5316\u5b66\u6210\u5206\uff1b3\uff09\u9700\u8981\u91cd\u65b0\u5206\u5e03\u7535\u89e3\u8d28\u4e2d\u539f\u6765\u4e0d\u5747\u5300\u7684Li\u79bb\u5b50\u901a\u91cf\u3002\u56e0\u800c\u8981\u5b9e\u73b0Li\u7684\u5e73\u9762\u5f62\u6001\u53d8\u5316\u4ecd\u9762\u4e34\u4e0d\u5c11\u6311\u6218\u3002\u867d\u7136\u6784\u5efa\u53ef\u62c9\u4f38SEI\u4ee5\u9002\u5e94Li\u91d1\u5c5e\u7684\u975e\u5e73\u9762\u5f62\u6001\u53d8\u5316\u4e0d\u4ea7\u751f\u88c2\u7eb9\uff0c\u53ef\u4ee5\u4ece\u6839\u672c\u4e0a\u907f\u514dLi\u679d\u6676\u548cLi\u7c89\u788e\uff0c\u4f46\u662f\u5229\u7528\u5e38\u89c4\u65b9\u6cd5\u96be\u4ee5\u4f7f\u8584\u819c\u4e0e\u6574\u4e2aLi\u91d1\u5c5e\u8868\u9762\u7684\u8d85\u4fdd\u5f62\u63a5\u89e6\uff0c\u4e14\u8584\u819c\u7684\u53ef\u62c9\u4f38\u6027\u53d7\u5230\u6ce2\u6d6a\u7ed3\u6784\u9650\u5236\u3002\u56e0\u6b64\uff0c\u6784\u5efa\u7406\u60f3\u7684\u53ef\u62c9\u4f38\u4e14\u8d85\u4fdd\u5f62\u7684SEI\u9762\u4e34\u5de8\u5927\u6311\u6218\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5\uff0c<strong>\u7f8e\u56fd\u5fb7\u514b\u8428\u65af\u5927\u5b66\u5965\u65af\u6c40\u5206\u6821\u4f59\u6842\u534e\u6559\u6388\uff08\u901a\u8baf\u4f5c\u8005\uff09\u7b49\u4eba<\/strong>\u62a5\u9053\u4e86\u4ed6\u4eec\u5229\u7528\u673a\u68b0\u526a\u5207\u8bf1\u5bfc\u77f3\u58a8\u5265\u79bb\uff0c\u540c\u65f6\u5c06\u5e73\u884c\u6392\u5217\u7684\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\u63ba\u5165Li\u7b94\u3002\u5728\u7535\u5316\u5b66\u5265\u79bb\u4e00\u5b9a\u91cf\u7684\u91d1\u5c5eLi\u540e\uff0c\u5728\u91d1\u5c5eLi\u8868\u9762\u4e0a\u5f62\u6210\u4e86\u7531\u65e0\u7f3a\u9677\u7684\u5c11\u5c42\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\u539f\u4f4d\u5806\u53e0\u6784\u6210\u8d85\u5171\u5f62\u8868\u9762\u3002\u5bf9\u6bd4\u5df2\u62a5\u9053\u7684\u5806\u53e0\u5f0f\u77f3\u58a8\u70ef\u8584\u819c\u4f5c\u4e3aLi\u6c89\u79ef\u7684\u4e3b\u4f53\uff0c\u8fd9\u79cd\u65e0\u7f3a\u9677\u7684\u77f3\u58a8\u70ef\u8584\u819c\u662f\u4e00\u79cd\u5f62\u72b6\u81ea\u9002\u5e94\u7684\u4fdd\u62a4\u8868\u5c42\uff0c\u4fdd\u62a4\u5176\u4e0b\u65b9\u7684Li\u6c89\u79ef\u5c42\u3002\u540c\u65f6\uff0c\u77f3\u58a8\u70ef\u5c42\u95f4\u6ed1\u52a8\u80fd\u591f\u63d0\u5347\u8584\u819c\u62c9\u4f38\u6027\u80fd\u4ee5\u9002\u5e94Li\u91d1\u5c5e\u9897\u7c92\u7684\u521d\u59cb\u81a8\u80c0\u800c\u6ca1\u6709\u88c2\u7eb9\u3002\u5728\u53cd\u590d\u7684Li\u5265\u79bb\u548c\u6c89\u79ef\u8fc7\u7a0b\u4e2d\uff0c\u67d4\u8f6f\u7684\u77f3\u58a8\u70ef\u8584\u819c\u4ea7\u751f\u7684\u8936\u76b1\u4f7fLi\u9897\u7c92\u5728\u6574\u4e2a\u5145\/\u653e\u7535\u8fc7\u7a0b\u4e2d\u88ab\u7d27\u5bc6\u5305\u88f9\u3002\u6b64\u5916\uff0c\u65e0\u7f3a\u9677\u7684\u5c11\u5c42\u77f3\u58a8\u70ef\u6709\u52a9\u4e8eLi\u79bb\u5b50\u7684\u5feb\u901f\u8f6c\u79fb\uff0c\u6709\u6548\u9632\u6b62\u7535\u89e3\u8d28\u4e0eLi\u91d1\u5c5e\u63a5\u89e6\u3002\u5b9e\u9a8c\u7ed3\u679c\u8868\u660e\uff0c\u8fd9\u79cd\u4fdd\u62a4\u6027\u8868\u5c42\u5141\u8bb8\u5fae\u7c73\u5c3a\u5bf8\u7684Li\u9897\u7c92\u53ef\u9006\u6c89\u79ef\uff0c\u4e0d\u51fa\u73b0Li\u679d\u6676\u548cLi\u7c89\u788e\u3002\u66f4\u91cd\u8981\u7684\u662f\uff0c\u8fd9\u79cd\u5bf9\u79f0\u6027\u7535\u6c60\u5728\u7535\u6d41\u5bc6\u5ea6\u4e3a5 mA cm<sup>-2<\/sup>\u4e0b\u53ef\u8fd0\u884c1000 h\uff0c\u8d85\u8fc7\u4e86\u77f3\u58a8\u70ef\u8584\u819c\u7a33\u5b9a\u7684Li\u91d1\u5c5e\u8d1f\u6781\u7684\u4f7f\u7528\u5bff\u547d\u3002\u603b\u4e4b\uff0c\u8be5\u5de5\u4f5c\u4e3a\u77f3\u58a8\u70ef\u5728LMBs\u4e2d\u7684\u5e94\u7528\u63d0\u4f9b\u4e86\u65b0\u7684\u673a\u4f1a\u3002\u8be5\u5de5\u4f5c\u6210\u679c\u4ee5\u9898\u4e3a<strong>\u201cReversible Deposition of Lithium Particles Enabled by Ultraconformal and Stretchable Graphene Film for Lithium Metal Batteries\u201d<\/strong>\u53d1\u8868\u5728\u8457\u540d\u671f\u520a<strong>Adv. Mater.<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u89e3\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00\u3001\u4e0d\u540cSEI\u4e0b\uff0cLi\u6c89\u79ef\u884c\u4e3a\u7684\u793a\u610f\u56fe<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-212321\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/1-1.jpg\" alt=\"\" width=\"600\" height=\"331\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/1-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/1-1-300x166.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u4e0d\u53ef\u53d8\u5f62SEI\u5728Li\u91d1\u5c5e\u4e0a\u5f15\u8d77\u4e0d\u53ef\u9006\u7684Li\u6c89\u79ef\uff1b<\/p>\n<p>\uff08b\uff09\u901a\u8fc7\u53ef\u53d8\u5f62\u548c\u8d85\u5171\u5f62\u7684SEI\uff0c\u5728Li\u91d1\u5c5e\u4e0aLi\u9897\u7c92\u7684\u53ef\u9006\u6c89\u79ef\u3002<\/p>\n<p><strong>\u56fe\u4e8c\u3001\u5728Li\u91d1\u5c5e\u4e0a\u5236\u5907\u77f3\u58a8\u70ef\u8584\u819c<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-212322\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/2-1.jpg\" alt=\"\" width=\"600\" height=\"691\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/2-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/2-1-260x300.jpg 260w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a\uff09\u901a\u8fc7\u673a\u68b0\u5265\u79bb\u77f3\u58a8\u548c\u540c\u65f6\u63a7\u5236Li\u91d1\u5c5e\u4e2d\u7684\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\u53d6\u5411\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08b\uff09\u901a\u8fc7\u7535\u5316\u5b66\u5265\u79bb\u90e8\u5206Li\u91d1\u5c5e\u5728\u77f3\u58a8\u70ef-Li\u590d\u5408\u6750\u6599\u7684\u8868\u9762\u4e0a\u5f62\u6210\u5e73\u884c\u5806\u53e0\u7684\u77f3\u58a8\u70ef\u5c42\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08c-d\uff09\u8868\u9762\u5177\u6709\u5e73\u884c\u5806\u53e0\u7684\u77f3\u58a8\u70ef\u5c42\u7684\u77f3\u58a8\u70ef-Li\u590d\u5408\u6750\u6599\u7684\u4fef\u89c6SEM\u56fe\u50cf\u548c\u622a\u9762SEM\u56fe\u50cf\u3002<\/p>\n<p><strong>\u56fe\u4e09\u3001Li\u91d1\u5c5e\u8d1f\u6781\u4e0a\u77f3\u58a8\u70ef\u8584\u819c\u7684\u5f62\u8c8c\u548c\u6027\u80fd<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-212323\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/3-1.jpg\" alt=\"\" width=\"600\" height=\"430\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/3-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/3-1-300x215.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-d\uff09\u5728\u4e0d\u540c\u653e\u5927\u500d\u6570\u7684\u5bf9\u79f0\u7535\u6c60\u4e2d\u7ecf\u8fc7150\u6b21\u5faa\u73af\u540e\uff0c\u7535\u9540\u548c\u5265\u79bb\u540e\u7684\u77f3\u58a8\u70ef\u8584\u819c\u4fdd\u62a4\u7684Li\u91d1\u5c5e\u8d1f\u6781\u7684\u5f62\u8c8c\uff1b<\/p>\n<p>\uff08e\uff09\u4f7f\u7528\u5806\u53e0\u7684\u77f3\u58a8\u70ef\u5c42\u4f5c\u4e3a\u53ef\u62c9\u4f38SEI\u5728Li\u7535\u9540\u548c\u5265\u79bb\u8fc7\u7a0b\u4e2d\u53ef\u9006\u5f62\u8c8c\u53d8\u5316\u7684\u793a\u610f\u56fe\uff1b<\/p>\n<p>\uff08f-g\uff09\u9540\u9502\u540e\uff0cG\/Li\u8d1f\u6781\u8868\u9762\u7684AFM\u56fe\u50cf\u548c\u76f8\u5e94\u7684\u6768\u6c0f\u6a21\u91cf\u56fe\uff1b<\/p>\n<p>\uff08h\uff09\u9540\u9502\u540e\uff0cG\/Li\u8d1f\u6781\u8868\u9762\u7684\u5178\u578b\u529b-\u538b\u75d5\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u56fe\u56db\u3001\u5149\u8c31\u8868\u5f81<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-212324\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/4-1.jpg\" alt=\"\" width=\"600\" height=\"360\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/4-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/4-1-300x180.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-d\uff09\u5728\u4e0d\u540c\u6e85\u5c04\u65f6\u95f4\u4e0b\uff0cC 1s\u3001O 1s\u3001F 1s\u548cLi 1s\u5728Li||NMC\u7535\u6c60\u4e2d\uff0c\u7ecf\u8fc750\u6b21\u5faa\u73af\u7684\u88f8Li\u8d1f\u6781\u548cG\/Li\u590d\u5408\u8d1f\u6781\u4e0aSEI\u7684XPS\u5149\u8c31\uff1b<\/p>\n<p>\uff08e\uff09\u77f3\u58a8\u3001GLi\u548cG\/Li\u6837\u54c1\u7684\u62c9\u66fc\u5149\u8c31\uff1b<\/p>\n<p>\uff08f\uff09\u9759\u6b6210 h\u524d\u540e\uff0c\u672a\u5faa\u73af\u7684\u629b\u5149Li||\u629b\u5149Li\u548cGLi||GLi\u5bf9\u79f0\u7535\u6c60\u7684\u5948\u594e\u65af\u7279\u56fe\u3002<\/p>\n<p><strong>\u56fe\u4e94\u3001\u7535\u5316\u5b66\u6027\u80fd<\/strong><br \/>\n <img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-212325\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/5-1.jpg\" alt=\"\" width=\"600\" height=\"603\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/5-1.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/11\/5-1-150x150.jpg 150w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/>\uff08a-b\uff09\u5728\u4e0d\u540c\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u4ee5\u88f8\u9732Li\u6216\u77f3\u58a8\u70ef-Li\u7eb3\u7c73\u590d\u5408\u6750\u6599\u4e3a\u8d1f\u6781\u7684\u5bf9\u79f0\u7535\u6c60\uff1b<\/p>\n<p>\uff08c\uff09\u6bd4\u8f83\u4f7f\u7528\u77f3\u58a8\u70ef\u8584\u819c\u4fdd\u62a4\u7684Li\u3001\u5806\u53e0\u7684rGO\u7a33\u5b9a\u7684Li\u548c\u5178\u578b\u8bbe\u8ba1\u7684SEI\u4fdd\u62a4\u7684Li\u6784\u6210\u5bf9\u79f0\u7535\u6c60\u7684\u5faa\u73af\u6027\u80fd\uff1b<\/p>\n<p>\uff08d\uff09\u88f8\u9732Li\u6216\u77f3\u58a8\u70ef-Li\u7eb3\u7c73\u590d\u5408\u6750\u6599\u4e3a\u8d1f\u6781\u3001NCM\u4e3a\u6b63\u6781\u6784\u6210\u5b8c\u6574\u7535\u6c60\u7684\u6027\u80fd\uff1b<\/p>\n<p>\uff08e-f\uff09\u539f\u59cbLi||NCM\u7535\u6c60\u548c\u77f3\u58a8\u70ef-Li||NCM\u7535\u6c60\u7684\u7b2c1-200\u6b21\u5faa\u73af\u7684\u76f8\u5e94\u7535\u538b\u66f2\u7ebf\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u7efc\u4e0a\u6240\u8ff0\uff0c\u4f5c\u8005\u62a5\u9053\u4e86\u4e00\u79cd\u7b80\u4fbf\u4e14\u4f4e\u6210\u672c\u7684\u7b56\u7565\u6765\u6784\u5efa\u5177\u6709\u5806\u53e0\u77f3\u58a8\u70ef\u5c42\u7684Li\u91d1\u5c5e\u8d1f\u6781\u4fdd\u62a4\u5c42\u3002Li\u91d1\u5c5e\u8f85\u52a9\u5265\u79bb\u6280\u672f\u5236\u5907\u51fa\u65e0\u7f3a\u9677\u7684\u591a\u5c42\u77f3\u58a8\u70ef\uff0c\u540c\u65f6\u4f7fLi\u91d1\u5c5e\u4e2d\u7684\u77f3\u58a8\u70ef\u7eb3\u7c73\u7247\u5e73\u884c\u6392\u5217\u3002\u4ece\u590d\u5408\u8d1f\u6781\u5265\u79bb\u4e00\u5b9a\u91cf\u7684Li\u540e\uff0c\u5bc6\u96c6\u5806\u79ef\u7684\u77f3\u58a8\u70ef\u5c42\u5728Li\u8d1f\u6781\u8868\u9762\u4e0a\u539f\u4f4d\u5f62\u6210\u8d85\u5171\u5f62SEI\u3002\u5176\u4e2d\uff0c\u77f3\u58a8\u70ef\u8584\u819c\u5177\u6709\u67d4\u6027\u548c\u53ef\u62c9\u4f38\u6027\uff0c\u53ef\u4ee5\u6709\u6548\u5730\u4fdd\u62a4Li\u514d\u4e8e\u76f4\u63a5\u4e0e\u7535\u89e3\u8d28\u63a5\u89e6\u3002\u968f\u7740\u91cd\u590d\u7684\u6c89\u79ef\/\u6eb6\u89e3\u8fc7\u7a0b\uff0cSEI\u4fdd\u6301\u4e0e\u4e0b\u9762\u7684Li\u91d1\u5c5e\u7684\u5171\u540c\u53d8\u5f62\uff0c\u4ee5\u4fdd\u6301Li\u9897\u7c92\u7d27\u5bc6\u5305\u88f9\u3002\u5b9e\u9a8c\u7ed3\u679c\u8868\u660e\uff0c\u5177\u6709\u5f62\u72b6\u9002\u5e94\u6027\u7684SEI\u901a\u8fc7\u6291\u5236Li\u679d\u6676\u7684\u751f\u957f\u548c\u6700\u5927\u7a0b\u5ea6\u5730\u51cf\u5c11\u6b7bLi\uff0c\u5b9e\u73b0\u4e86\u53ef\u9006\u7684\u5fae\u7c73\u7ea7Li\u9897\u7c92\u7684\u6c89\u79ef\/\u6eb6\u89e3\u3002\u603b\u4e4b\uff0c\u8be5\u5de5\u4f5c\u4e3a\u5728\u5b9e\u7528\u7684\u9ad8\u80fd\u7535\u6c60\u4e0a\u5728Li\u91d1\u5c5e\u8d1f\u6781\u4e0a\u6784\u5efa\u77f3\u58a8\u70ef\u8584\u819c\u4f5c\u4e3a\u7406\u60f3\u7684SEI\u63d0\u4f9b\u4e86\u4e00\u79cd\u7b80\u5355\u800c\u5ec9\u4ef7\u7684\u65b9\u6cd5\uff0c\u540c\u65f6\u5bf9\u4e8e\u89e3\u51b3\u5176\u4ed6\u91d1\u5c5e\u548c\u91d1\u5c5e\u5408\u91d1\u8d1f\u6781\u6750\u6599\u7684\u679d\u6676\u548c\u7c89\u788e\u95ee\u9898\u63d0\u4f9b\u65b0\u601d\u8def\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<a href=\"https:\/\/onlinelibrary.wiley.com\/doi\/10.1002\/adma.202005763\" target=\"_blank\" rel=\"noopener\">Reversible Deposition of Lithium Particles Enabled by Ultraconformal and Stretchable Graphene Film for Lithium Metal Batteries<\/a><\/strong>.\uff08<em>Adv. Mater.<\/em>, <strong>2020<\/strong>, DOI: 10.1002\/adma.202005763\uff09<\/p>\n<p style=\"text-align: center;\"><strong>\u901a\u8baf\u4f5c\u8005\u7b80\u4ecb<\/strong><\/p>\n<p><strong>\u3010\u56e2\u961f\u4ecb\u7ecd\u3011<\/strong><\/p>\n<p><strong>\u4f59\u6842\u534e\uff0c\u535a\u58eb\u5bfc\u5e08\uff0c\u7f8e\u56fd\u5fb7\u514b\u8428\u65af\u5927\u5b66\u5965\u65af\u6c40\u5206\u6821\u6750\u6599\u79d1\u5b66\u4e0e\u5de5\u7a0b\u7cfb\uff0c\u673a\u68b0\u7cfb\u7ec8\u8eab\u6559\u6388<\/strong>\uff0c\u82f1\u56fd\u7687\u5bb6\u5316\u5b66\u5b66\u4f1a\u4f1a\u58eb\uff08FRSC\uff09\uff0c\u82f1\u56fd\u7687\u5bb6\u7269\u7406\u5b66\u4f1a\u4f1a\u58eb\uff08FInstP\uff09\uff0cACS Materials Letters \u526f\u4e3b\u7f16\u3002\u4f59\u6559\u6388\u56e2\u961f\u7684\u7814\u7a76\u91cd\u70b9\u5305\u62ec\u6709\u673a\u548c\u590d\u5408\u529f\u80fd\u6027\u6750\u6599\u7684\u7eb3\u7c73\u7ed3\u6784\u8bbe\u8ba1\uff0c\u5408\u6210\u548c\u81ea\u7ec4\u88c5\uff0c\u4ee5\u53ca\u5bf9\u5176\u5316\u5b66\u548c\u7269\u7406\u6027\u8d28\u7684\u6df1\u5165\u89e3\u6790\uff0c\u4ece\u800c\u5e94\u7528\u4e8e\u80fd\u6e90\uff0c\u73af\u5883\u548c\u751f\u547d\u79d1\u5b66\u7b49\u9886\u57df\u3002\u76ee\u524d\u5df2\u5728Science, Nature, Nature Reviews Materials, Nature Materials, Nature Nanotechnology, Nature Communications, PNAS, Chemical Reviews, Chemical Society Reviews, Accounts of Chemical Research, JACS, Angewandte Chemie, Advanced Materials, Chem, Joule, Nano Letters, Energy &amp; Environmental Sciences,\u7b49\u56fd\u9645\u8457\u540d\u520a\u7269\u4e0a\u53d1\u8868\u8bba\u6587200\u4f59\u7bc7\uff0c\u8bba\u6587\u5f15\u7528\u903e33\uff0c000\u6b21\uff0cH\u56e0\u5b5093\u3002\u5176\u4e2d40\u591a\u7bc7\u8bba\u6587\u88ab\u671f\u520a\u9009\u4e3a\u975e\u5e38\u91cd\u8981\u8bba\u6587\u548c\u70ed\u70b9\u8bba\u6587\u3002\u5176\u53d1\u8868\u5de5\u4f5c\u66fe\u88ab\u591a\u4e2a\u56fd\u9645\u5a92\u4f53\u4eae\u70b9\u62a5\u9053\uff0c\u5176\u4e2d\u5305\u62ecNature News, Science News, ABC News, Fox News, Forbes, Discover, National Geographic, Science Daily, R&amp;D Magazine, MIT Technology Review, Popular Science, Ars Technica, C&amp;EN, Gizmag, IEEE Spectrum, MRS Bulletin\u7b49\u3002<\/p>\n<p><strong>\u3010\u56e2\u961f\u5728\u8be5\u9886\u57df\u5de5\u4f5c\u6c47\u603b\u3011<\/strong><\/p>\n<p>\u4f5c\u4e3a\u7814\u7a76\u91cd\u70b9\u4e4b\u4e00\uff0c\u4f59\u6842\u534e\u6559\u6388\u56e2\u961f\u81f4\u529b\u4e8e\u7814\u53d1\u529f\u80fd\u6027\u4e8c\u7ef4\u7eb3\u7c73\u6750\u6599\uff0c\u901a\u8fc7\u5bf9\u5176\u5316\u5b66\u7ec4\u5206\u7684\u8c03\u63a7\u4ee5\u53ca\u7eb3\u7c73\u7ed3\u6784\u7684\u8bbe\u8ba1\uff0c\u53d1\u5c55\u4e86\u4e00\u7cfb\u5217\u9ad8\u6027\u80fd\u78b1\u91d1\u5c5e\u79bb\u5b50\u7535\u6c60\u6750\u6599\u548c\u9ad8\u6d3b\u6027\u7535\u50ac\u5316\u5242\u3002\u7ed3\u5408\u591a\u79cd\u7535\u5316\u5b66\u6d4b\u8bd5\u6280\u672f\uff0c\u539f\u4f4d\u8868\u5f81\uff0c\u4ee5\u53ca\u7406\u8bba\u8ba1\u7b97\u6a21\u62df\uff0c\u4ece\u5fae\u89c2\u81f3\u4ecb\u89c2\u5bf9\u6750\u6599\u4f53\u7cfb\u5185\u7684\u7535\u5316\u5b66\u8fc7\u7a0b\u8fdb\u884c\u591a\u5c3a\u5ea6\u7684\u5206\u6790\u548c\u63a2\u8ba8\uff0c\u5e76\u6df1\u5165\u7814\u7a76\u4e86\u79bb\u5b50\u548c\u5c0f\u5206\u5b50\u5d4c\u5165\u4e8c\u7ef4\u7eb3\u7c73\u6750\u6599\u7684\u673a\u7406\u548c\u52a8\u529b\u5b66\u8fc7\u7a0b\u3002<\/p>\n<p><strong>\u3010\u76f8\u5173\u4f18\u8d28\u6587\u732e\u63a8\u8350\u3011<\/strong><\/p>\n<p>1. Y. Zhou, X. Zhang, Y. Ding, J. Bae, X. Guo, Y. Zhao, G. Yu, &#8216;Redistributing Li-Ion Flux by Parallelly Aligned Holey Nanosheets for Dendrite-Free Li Metal Anode&#8217;, <em>Adv. Mater.<\/em> <em>32<\/em>, 2003920 (<strong>2020<\/strong>).<\/p>\n<p>2. Y. Zhou, X. Zhang, Y. Ding, L. Zhang, G. Yu, &#8216;Reversible Deposition of Lithium Particles Enabled by Ultraconformal and Stretchable Graphene Film for Lithium Metal Batteries&#8217;, <em>Adv. Mater.<\/em> <em>32<\/em>, 2005763 (<strong>2020<\/strong>).<\/p>\n<p>3. Y. Zhu, Y. Qian, Z. Ju, Y. Ji, Y. Yan, Y. Liu, G. Yu, &#8216;Understanding Charge Storage in Hydrated Layered Solids MOPO4 (M = V, Nb) with Tunable Interlayer Chemistry&#8217;, <em>ACS Nano<\/em> <em>14<\/em>, 13824 (<strong>2020<\/strong>).<\/p>\n<p>4. Y. Zhu, Z. Ju, X. Zhang, D. Lutz, L. Housel, Y. Zhou, K. Takeuchi, E. Takeuchi, A. Marschilok, G. Yu, &#8216;Evaporation Induced Vertical Alignment Enabling Directional Ion Transport in 2D Nanosheet-Based Battery Electrode&#8217;, <em>Adv. Mater.<\/em> <em>32<\/em>, 1907941 (<strong>2020<\/strong>).<\/p>\n<p>5. Y. Zhu, L. Peng, Z. Fang, C. Yan, X. Zhang, G. Yu, &#8220;Structural Engineering of 2D Materials for Energy Storage and Catalysis&#8221;, <em>Adv. Mater.<\/em> <em>30<\/em>, 1706347 (<strong>2018<\/strong>).<\/p>\n<p>\u672c\u6587\u7531CQR\u7f16\u8bd1\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1\uff1atougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenvip.<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u80cc\u666f\u4ecb\u7ecd\u3011 \u9502\uff08Li\uff09\u91d1\u5c5e\u5177\u6709\u6700\u4f4e\u7684\u7535\u5316\u5b66\u52bf\u548c\u6700\u9ad8\u7684\u7406\u8bba\u6bd4\u5bb9\u91cf\uff0c\u4f46\u662f\u5f53Li\u91d1\u5c5e\u66b4\u9732\u4e8e\u7535\u89e3\u8d28\u4e2d\u65f6\uff0c\u56fa\u6001\u7535\u89e3\u8d28\u4e2d\u95f4\u76f8\uff08SEI\uff09\u4f1a\u5728Li\u91d1\u5c5e\u8868\u9762\u4e0a\u5f62\u6210\u949d\u5316\u5c42\uff0c\u51fa\u73b0\u4e0d&#8230;<\/p>\n","protected":false},"author":7770,"featured_media":0,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[4366],"class_list":["post-212320","post","type-post","status-publish","format-standard","hentry","category-jiedu","tag-lmbs"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/212320"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7770"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=212320"}],"version-history":[{"count":3,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/212320\/revisions"}],"predecessor-version":[{"id":212569,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/212320\/revisions\/212569"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=212320"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=212320"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=212320"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}