{"id":214598,"date":"2020-12-16T06:29:44","date_gmt":"2020-12-15T22:29:44","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=214598"},"modified":"2020-12-15T20:30:27","modified_gmt":"2020-12-15T12:30:27","slug":"2020%e5%b9%b4ns%e5%8f%91%e6%96%87top3%e9%ab%98%e6%a0%a1%e5%9c%a8%e6%9d%90%e6%96%99%e9%a2%86%e5%9f%9f%e6%94%be%e4%ba%86%e4%bb%80%e4%b9%88%e5%a4%a7%e6%8b%9b%ef%bc%9f","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=214598","title":{"rendered":"2020\u5e74\u5728Nature\u3001Science\u4e0a\u53d1\u6587TOP3\u9ad8\u6821\u5728\u6750\u6599\u9886\u57df\u653e\u4e86\u4ec0\u4e48\u5927\u62db\uff1f"},"content":{"rendered":"<p>\u4f5c\u4e3a\u56fd\u9645\u4e0a\u6700\u4e3a\u77e5\u540d\u7684\u4e24\u5927\u7efc\u5408\u6027\u5b66\u672f\u671f\u520a\uff0cNature\u548cScience\u65e8\u5728\u53d1\u8868\u539f\u521b\u6027\u5f3a\u3001\u89c2\u70b9\u65b0\u9896\u3001\u5f71\u54cd\u5e7f\u6cdb\uff0c\u5e76\u4e14\u5bf9\u6574\u4e2a\u79d1\u5b66\u53d1\u5c55\u5177\u6709\u63a8\u52a8\u4f5c\u7528\u7684\u7a81\u7834\u6027\u53d1\u73b0\u3002\u7531\u4e8e\u7ade\u4e89\u6fc0\u70c8\uff0c\u6240\u6709\u6295\u7a3f\u81f3\u8fd9\u4e24\u5927\u671f\u520a\u7684\u539f\u521b\u6587\u7ae0\u4e2d\u4ec5\u6709\u4e0d\u8db38%\u88ab\u63a5\u53d7\u548c\u53d1\u8868\u3002\u56e0\u6b64N&amp;S\u53d1\u8868\u7684\u8bba\u6587\u4e00\u5b9a\u7a0b\u5ea6\u4e0a\u4ee3\u8868\u7740\u5b66\u79d1\u9886\u57df\u5185\u7684\u6700\u9ad8\u6c34\u5e73\uff0c\u800cN&amp;S\u53d1\u6587\u6570\u4e5f\u662f\u6bd4\u8f83\u56fd\u5bb6\u548c\u673a\u6784\u79d1\u7814\u4ea7\u51fa\u8d28\u91cf\u7684\u91cd\u8981\u6307\u6807\u4e4b\u4e00\u3002<\/p>\n<p>\u672c\u6587\u7edf\u8ba1\u4e86\u6211\u56fd\u56fd\u5185\u9ad8\u68212020\u5e74\u4f5c\u4e3a\u901a\u8baf\u4f5c\u8005\u5355\u4f4d\uff08\u542b\u5171\u540c\u901a\u8baf\u4f5c\u8005\u5355\u4f4d\uff09\u5728\u300a\u81ea\u7136\u300bNature\u3001\u300a\u79d1\u5b66\u300bScience\u671f\u520a\u4e0a\u53d1\u8868\u7684\u60c5\u51b5\u3002\u6570\u636e\u7edf\u8ba1\u622a\u81f32020\u5e7411\u670830\u65e5\u3002\u5e76\u5728\u53d1\u6587\u603b\u6570\u524d\u4e09\u7684\u9ad8\u6821\u4e2d\u5206\u522b\u9009\u53d6\u4e86\u4e00\u4e2a\u5728\u6750\u6599\u5b66\u9886\u57df\u7684\u4ee3\u8868\u6027\u6210\u679c\u8fdb\u884c\u7b80\u4ecb\u3002<\/p>\n<p>\u4eca\u5e74\u6211\u56fd\u5185\u5730\u9ad8\u6821\u5728N&amp;S\u53d1\u8868\u8bba\u6587\u603b\u6570\u524d\u4e09\u7684\u9ad8\u6821\u5206\u522b\u662f\u4e2d\u56fd\u79d1\u5b66\u9662\u3001\u6e05\u534e\u5927\u5b66\u548c\u5317\u4eac\u5927\u5b66\u3002\u6211\u56fd\u53d1\u8868\u603b\u6570\u524d\u5341\u7684\u9ad8\u6821\u5f00\u5c55\u7684\u79d1\u7814\u6d3b\u52a8\u548c\u6d89\u53ca\u9886\u57df\u4e3b\u8981\u96c6\u4e2d\u5728\u751f\u7269\u5b66\u3001\u7269\u7406\u5b66\u3001\u533b\u5b66\u548c\u5316\u5b66\u3002<\/p>\n<p style=\"text-align: center;\">\u4e2d\u56fd\u5185\u5730\u9ad8\u6821N&amp;S\u8bba\u6587\u6570<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-214601 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u72471-10.png\" alt=\"\" width=\"294\" height=\"460\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u72471-10.png 294w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u72471-10-192x300.png 192w\" sizes=\"(max-width: 294px) 100vw, 294px\" \/><\/p>\n<p style=\"text-align: left;\"><strong><span style=\"line-height: 1.5;\">\u4e00\u3001\u4e2d\u56fd\u79d1\u5b66\u9662Science\uff1a\u94c1\u57fa\u8d85\u5bfc\u4f53\u4e2d\u6da1\u65cb\u96f6\u6a21\u7684\u8fd1\u91cf\u5b50\u5316\u7535\u5bfc\u5e73\u53f0<\/span><sup>[1]<\/sup><\/strong><\/p>\n<p>\u4e2d\u79d1\u9662\u7269\u7406\u6240\u9ad8\u9e3f\u94a7\u3001\u4e01\u6d2a\u548c\u5f20\u4f59\u6d0b\u7b49\u4eba\u901a\u8fc7\u96a7\u7a7f\u8026\u5408\u5f3a\u5ea6\u53ef\u53d8\u7684\u626b\u63cf\u96a7\u9053\u8c31\uff08STS\uff09\u7814\u7a76\u4e86FeTe<sub>0.55<\/sub>Se<sub>0.45<\/sub>\u8d85\u5bfc\u4f53\u4e2d\u78c1\u901a\u6da1\u65cb\u675f\u7f1a\u6001\u7684\u96a7\u7a7f\u7535\u5bfc\uff0c\u4e3a\u94c1\u57fa\u8d85\u5bfc\u4e2d\u9a6c\u7ea6\u62c9\u7eb3\u96f6\u80fd\u6a21\u7684\u5b58\u5728\u63d0\u4f9b\u4e86\u5b9a\u91cf\u65b0\u8bc1\u636e\u3002\u76f8\u5173\u6210\u679c\u4ee5\u201cNearly quantized conductance plateau of vortex zero mode in an iron-based superconductor\u201d\u4e3a\u9898\u4e8e2020\u5e741\u670810\u65e5\u53d1\u8868\u5728Science\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-214603 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-3-9.png\" alt=\"\" width=\"600\" height=\"342\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-3-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-3-9-300x171.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u5728\u4e00\u79cd\u53ef\u80fd\u5177\u6709\u9a6c\u7ea6\u62c9\u7eb3\u6a21\u578b\u7684\u7279\u6b8a\u8d85\u5bfc\u6750\u6599\u4e2d\uff0c\u91cf\u5b50\u4fe1\u606f\u88ab\u9650\u57df\u4e8e\u5176\u8868\u9762\u6216\u8fb9\u7f18\uff0c\u4ece\u800c\u4e3a\u5b9e\u73b0\u7a33\u5b9a\u7684\u91cf\u5b50\u4f4d\u63d0\u4f9b\u4e86\u53ef\u884c\u7684\u65b9\u6848\u3002\u95ee\u9898\u5728\u4e8e\uff0c\u867d\u7136\u5df2\u7ecf\u5b58\u5728\u8fd9\u6837\u90a3\u6837\u7684\u95f4\u63a5\u8bc1\u636e\uff0c\u4f46\u662f\u59cb\u7ec8\u6ca1\u6709\u76f4\u63a5\u7684\u8bc1\u636e\u8bc1\u660e\u9a6c\u7ea6\u62c9\u7eb3\u6a21\u578b\u7684\u5b58\u5728\u3002\u5b9e\u9a8c\u4e2d\uff0c\u4f5c\u8005\u89c2\u6d4b\u4e86\u7535\u5bfc\u5e73\u53f0\u968f\u96a7\u7a7f\u8026\u5408\u5f3a\u5ea6\u7684\u53d8\u5316\uff0c\u53d1\u73b0\u7535\u5bfc\u80fd\u63a5\u8fd1\u751a\u81f3\u8fbe\u5230\u91cf\u5b50\u7535\u5bfc\u503c2e<sup>2<\/sup>\/h\u3002\u76f8\u6bd4\u4e4b\u4e0b\uff0c\u5728\u6709\u9650\u80fd\u91cf\u6da1\u65cb\u675f\u7f1a\u6001\uff0c\u6216\u662f\u8d85\u5bfc\u5e26\u9699\u5916\u7684\u7535\u5b50\u6001\u8fde\u7eed\u533a\uff0c\u5b9e\u9a8c\u5e76\u672a\u89c2\u6d4b\u5230\u7535\u5bfc\u5e73\u53f0\u3002\u4f5c\u8005\u8ba4\u4e3a\uff0c\u6240\u89c2\u6d4b\u5230\u7684\u96f6\u80fd\u6a21\u7535\u5bfc\u5e73\u53f0\u662f\u652f\u6491FeTe<sub>0.55<\/sub>Se<sub>0.45<\/sub>\u4e2d\u5b58\u5728MZMs\u7684\u6709\u529b\u8bc1\u636e\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-214608 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-8-8.png\" alt=\"\" width=\"600\" height=\"312\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-8-8.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-8-8-300x156.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe1. \u5728FeTe<sub>0.55<\/sub>Se<sub>0.45<\/sub>\u4e0a\u89c2\u5bdf\u5230\u96f6\u504f\u7535\u5bfc\u5e73\u53f0<\/p>\n<p><strong>\u4e8c\u3001\u6e05\u534eScience\uff1a\u8d85\u8010\u4e45\u6027\u7684\u8d85\u957f\u78b3\u7eb3\u7c73\u7ba1<sup>[2]<\/sup><\/strong><\/p>\n<p>\u6e05\u534e\u5927\u5b66\u5316\u5de5\u7cfb\u9b4f\u98de\u6559\u6388\u548c\u5f20\u5982\u8303\u526f\u6559\u6388\u56e2\u961f\u5728\u78b3\u7eb3\u7c73\u7ba1\u8010\u75b2\u52b3\u6027\u80fd\u7814\u7a76\u65b9\u9762\u53d6\u5f97\u91cd\u5927\u7a81\u7834\uff0c\u9996\u6b21\u4ee5\u5b9e\u9a8c\u5f62\u5f0f\u6d4b\u8bd5\u4e86\u5398\u7c73\u7ea7\u957f\u5ea6\u5355\u6839\u78b3\u7eb3\u7c73\u7ba1\u7684\u8d85\u8010\u75b2\u52b3\u6027\u80fd\u3002\u76f8\u5173\u6210\u679c\u4ee5\u201c\u8d85\u8010\u4e45\u6027\u7684\u8d85\u957f\u78b3\u7eb3\u7c73\u7ba1\u201d(Super-durable Ultralong Carbon Nanotubes)\u4e3a\u9898\uff0c\u4e8e8\u670828\u65e5\u5728\u7ebf\u53d1\u8868\u4e8eScience\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-214602 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-2-9.png\" alt=\"\" width=\"600\" height=\"247\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-2-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-2-9-300x124.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u8d85\u5f3a\u8d85\u97e7\u548c\u8d85\u8010\u75b2\u52b3\u6027\u80fd\u7684\u6750\u6599\u5728\u822a\u7a7a\u822a\u5929\u3001\u519b\u4e8b\u88c5\u5907\u3001\u9632\u5f39\u8863\u3001\u5927\u578b\u6865\u6881\u3001\u8fd0\u52a8\u5668\u6750\u3001\u4eba\u9020\u808c\u8089\u7b49\u4f17\u591a\u9886\u57df\u90fd\u9762\u4e34\u5de8\u5927\u7684\u9700\u6c42\u3002\u78b3\u7eb3\u7c73\u7ba1\u662f\u5178\u578b\u7684\u4e00\u7ef4\u7eb3\u7c73\u6750\u6599\uff0c\u4e5f\u662f\u76ee\u524d\u5df2\u77e5\u7684\u529b\u5b66\u5f3a\u5ea6\u6700\u9ad8\u548c\u97e7\u6027\u6700\u597d\u7684\u6750\u6599\uff0c\u5176\u5b8f\u89c2\u5f3a\u5ea6\u548c\u97e7\u6027\u5747\u6bd4\u76ee\u524d\u5e7f\u6cdb\u4f7f\u7528\u7684\u78b3\u7ea4\u7ef4\u548c\u82b3\u7eb6\u7b49\u6750\u6599\u9ad8\u51fa\u4e00\u4e2a\u6570\u91cf\u7ea7\u4ee5\u4e0a\u3002\u7136\u800c\uff0c\u7531\u4e8e\u5176\u5c0f\u5c3a\u5bf8\u7279\u6027\u4ee5\u53ca\u96be\u4ee5\u88ab\u6d4b\u8bd5\u7684\u7279\u70b9\uff0c\u5355\u6839\u78b3\u7eb3\u7c73\u7ba1\u7684\u75b2\u52b3\u884c\u4e3a\u4ee5\u53ca\u75b2\u52b3\u7834\u574f\u673a\u5236\u7814\u7a76\u662f\u8be5\u9886\u57df\u957f\u671f\u672a\u80fd\u641e\u6e05\u695a\u7684\u91cd\u5927\u96be\u9898\u3002\u7531\u4e8e\u75b2\u52b3\u53ef\u4ee5\u5728\u5e94\u529b\u6c34\u5e73\u8fdc\u4f4e\u4e8e\u9759\u6001\u65ad\u88c2\u5f3a\u5ea6\u7684\u60c5\u51b5\u4e0b\u53d1\u751f\uff0c\u63a2\u7a76\u75b2\u52b3\u884c\u4e3a\u548c\u6f5c\u5728\u7684\u7834\u574f\u673a\u5236\u5bf9\u4e8e\u65b0\u6750\u6599\u7684\u957f\u671f\u53ef\u9760\u6027\u8bc4\u4f30\u53ca\u5e94\u7528\u5177\u6709\u6781\u4e3a\u91cd\u8981\u7684\u610f\u4e49\u3002<\/p>\n<p>\u8be5\u7814\u7a76\u53d1\u73b0\uff0c\u78b3\u7eb3\u7c73\u7ba1\u5728\u5927\u5e94\u53d8\u5faa\u73af\u62c9\u4f38\u6d4b\u8bd5\u6761\u4ef6\u4e0b\uff0c\u5355\u6839\u78b3\u7eb3\u7c73\u7ba1\u53ef\u4ee5\u88ab\u8fde\u7eed\u62c9\u4f38\u4e0a\u4ebf\u6b21\u800c\u4e0d\u53d1\u751f\u65ad\u88c2\uff0c\u5e76\u4e14\u5728\u53bb\u6389\u8f7d\u8377\u540e\uff0c\u5176\u4f9d\u7136\u80fd\u4fdd\u6301\u521d\u59cb\u7684\u8d85\u9ad8\u6297\u62c9\u5f3a\u5ea6\uff0c\u8010\u75b2\u52b3\u6027\u4f18\u4e8e\u76ee\u524d\u6240\u6709\u5de5\u7a0b\u7ea4\u7ef4\u6750\u6599\u3002\u4e0e\u4e00\u822c\u4f20\u7edf\u6750\u6599\u7684\u75b2\u52b3\u635f\u4f24\u7d2f\u79ef\u673a\u5236\u4e0d\u540c\uff0c\u5176\u75b2\u52b3\u7834\u574f\u5448\u73b0\u51fa\u6574\u4f53\u7834\u574f\u6027\uff0c\u4e0d\u5b58\u5728\u635f\u4f24\u7d2f\u79ef\u8fc7\u7a0b\uff0c\u521d\u59cb\u7f3a\u9677\u7684\u751f\u6210\u5bf9\u78b3\u7eb3\u7c73\u7ba1\u7684\u75b2\u52b3\u5bff\u547d\u8d77\u4e3b\u5bfc\u4f5c\u7528\u3002\u6b64\u5916\uff0c\u5176\u8010\u75b2\u52b3\u6027\u53d7\u5230\u6e29\u5ea6\u5f71\u54cd\uff0c\u8868\u73b0\u51fa\u968f\u7740\u6e29\u5ea6\u5347\u9ad8\u800c\u4e0b\u964d\u7684\u7279\u70b9\u3002\u8fd9\u9879\u5de5\u4f5c\u63ed\u793a\u4e86\u8d85\u957f\u78b3\u7eb3\u7c73\u7ba1\u7528\u4e8e\u5236\u9020\u8d85\u5f3a\u8d85\u8010\u75b2\u52b3\u7ea4\u7ef4\u7684\u5149\u660e\u524d\u666f\uff0c\u540c\u65f6\u4e3a\u78b3\u7eb3\u7c73\u7ba1\u5728\u8bb8\u591a\u9886\u57df\u5e94\u7528\u7684\u5bff\u547d\u8bbe\u8ba1\u63d0\u4f9b\u4e86\u91cd\u8981\u7684\u53c2\u8003\u4f9d\u636e\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-214611 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u5fae\u4fe1\u56fe\u7247_20201215150848.jpg\" alt=\"\" width=\"600\" height=\"602\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u5fae\u4fe1\u56fe\u7247_20201215150848.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u5fae\u4fe1\u56fe\u7247_20201215150848-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u5fae\u4fe1\u56fe\u7247_20201215150848-300x300.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe2. \u8d85\u957f\u78b3\u7eb3\u7c73\u7ba1\u7684\u8010\u75b2\u52b3\u6027\u80fd.\uff08A-E\uff09\u5398\u7c73\u7ea7\u8d85\u957f\u78b3\u7eb3\u7c73\u7ba1\u6837\u54c1\uff1b\uff08F-G\uff09\u975e\u63a5\u89e6\u5f0f\u58f0\u5b66\u5171\u632f\u6d4b\u8bd5\u7cfb\u7edf\u673a\u7406\u793a\u610f\u56fe;\uff08H-I\uff09\u8d85\u957f\u78b3\u7eb3\u7c73\u7ba1\u7684\u8010\u75b2\u52b3\u6027\u80fd\u3002<\/p>\n<p><strong>\u4e09\u3001\u5317\u5927Nature:\u539f\u5b50\u7ea7\u6210\u50cf\u63ed\u793a\u4e8c\u7ef4\u51b0\u5c42\u7684\u751f\u957f\u53ca\u5176\u8fb9\u7f18\u7ed3\u6784<sup>[3]<\/sup><\/strong><\/p>\n<p>\u5317\u4eac\u5927\u5b66\u7684\u6c5f\u9896\u3001\u738b\u6069\u54e5\u3001\u5f90\u8389\u6885\u4ee5\u53ca\u7f8e\u56fd\u5185\u5e03\u62c9\u65af\u52a0\u5927\u5b66\u6797\u80af\u5206\u6821\u7684\u66fe\u6653\u6210\uff08\u5171\u540c\u901a\u8baf\u4f5c\u8005\uff09\u7b49\u4eba\u62a5\u9053\u5c55\u793a\u4e86\u5229\u7528\u975e\u63a5\u89e6\u539f\u5b50\u529b\u663e\u5fae\u5b66\u5bf9\u5728\u91d1(111)\u8868\u9762\u8fdb\u884c\u751f\u957f\u7684\u4e8c\u7ef4\u53cc\u5c42\u51b0\u7684\u8fb9\u7f18\u7ed3\u6784\u5b9e\u73b0\u4e86\u6210\u50cf\u89c2\u5bdf\u3002\u76f8\u5173\u6210\u679c\u4ee5\u9898\u4e3a\u201cAtomic imaging of the edge structure and growth of a two-dimensional hexagonal ice\u201d \u4e8e2020\u5e7401\u670801\u65e5\u5728\u7ebf\u53d1\u8868\u5728Nature\u4e0a\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-214604 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-4-8.png\" alt=\"\" width=\"600\" height=\"138\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-4-8.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-4-8-300x69.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\u7814\u7a76\u53d1\u73b0\uff0c\u4e8c\u7ef4\u516d\u65b9\u6676\u7cfb\u7684\u51b0\u5728\u751f\u957f\u8fc7\u7a0b\u4e2d\uff0c\u4e0d\u4ec5\u5b58\u5728Z\u578b\u8fb9\u7f18\u7ed3\u6784\uff08\u5e38\u89c1\u4e8e\u4e8c\u7ef4\u516d\u65b9\u6676\u4f53\uff09\uff0c\u8fd8\u6709\u6276\u624b\u6905\u578b\u8fb9\u7f18\u7ed3\u6784\u4e0e\u5176\u5171\u5b58\u3002\u51b7\u51bb\u89c2\u5bdf\u548c\u8fdb\u4e00\u6b65\u7684\u6a21\u62df\u5b9e\u9a8c\u8fd8\u63ed\u793a\u4e86\u4e8c\u7ef4\u51b0\u7684\u751f\u957f\u673a\u5236\uff0c\u5176\u4e2dZ\u578b\u8fb9\u7f18\u7ed3\u6784\u53c2\u4e0e\u6d89\u53ca\u4e86\u4ece\u6c34\u5206\u5b50\u6f14\u53d8\u5230\u8fb9\u7f18\u7ed3\u6784\u7684\u8fc7\u7a0b\uff08\u96c6\u4f53\u6027\u6865\u63a5\u673a\u5236\uff09\uff0c\u800c\u6276\u624b\u6905\u7ed3\u6784\u7684\u4e2d\u95f4\u4ea7\u7269\u5219\u53c2\u4e0e\u4e86\u5c40\u90e8\u7684\u6676\u79cd\u751f\u6210\u548c\u8fb9\u7f18\u91cd\u6784\u8fc7\u7a0b\u3002\u8fd9\u4e9b\u73b0\u8c61\u548c\u673a\u5236\u7814\u7a76\u4e3a\u7814\u7a76\u4e8c\u7ef4\u6750\u6599\u7684\u751f\u957f\u673a\u5236\u63d0\u4f9b\u4e86\u65b0\u9896\u7684\u89c2\u5bdf\u89d2\u5ea6\u3002<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-214606 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-6-9.png\" alt=\"\" width=\"600\" height=\"521\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-6-9.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-6-9-300x261.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe3.\u00a0\u4e8c\u7ef4\u51b0\u5c42\u7684\u5b9e\u9a8c\u89c2\u6d4b\u53ca\u5176STM\u3001AFM\u56fe\u50cf<\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter wp-image-214607 size-full\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-7-6.png\" alt=\"\" width=\"600\" height=\"290\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-7-6.png 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2020\/12\/\u56fe\u7247-7-6-300x145.png 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p style=\"text-align: center;\">\u56fe4.\u00a0Z\u578b\u548c\u6276\u624b\u6905\u578b\u8fb9\u7f18\u7ed3\u6784\u7684\u751f\u957f\u8fc7\u7a0b<\/p>\n<p>\u53c2\u8003\u6587\u732e\uff1a<\/p>\n<p>[1]Shiyu Zhu, Lingyuan Kong, Lu Cao, Hui Chen, Micha\u0142 Papaj, Shixuan Du, Yuqing Xing, Wenyao Liu, Dongfei Wang, Chengmin Shen, Fazhi Yang, John Schneeloch, Ruidan Zhong, Genda Gu, Liang Fu, Yu-Yang Zhang, Hong Ding, Hong-Jun Gao, Nearly quantized conductance plateau of vortex zero mode in an iron-based superconductor, Science, 2020 (367) 189-192.<\/p>\n<p>[2]Yunxiang Bai, Hongjie Yue, Jin Wang, Boyuan Shen, Silei Sun, Shijun Wang, Haidong Wang, Xide Li, Zhiping Xu, Rufan Zhang, Fei Wei, Super-durable ultralong carbon nanotubes, Science, 2020 (369) 1104-1106.<\/p>\n<p>[3]Runze Ma, Duanyun Cao, Chongqin Zhu, Ye Tian, Jinbo Peng, Jing Guo, Ji Chen, Xin-Zheng Li, Joseph S. Francisco, Xiao Cheng Zeng, Li-Mei Xu, En-Ge Wang, Ying Jiang, Atomic imaging of the edge structure and growth of a two-dimensional hexagonal ice, Nature, 2020 (577) 60-63.<\/p>\n<p>\u672c\u6587\u7531\u6625\u6625\u4f9b\u7a3f\u3002<\/p>\n<p>\u672c\u5185\u5bb9\u4e3a\u4f5c\u8005\u72ec\u7acb\u89c2\u70b9\uff0c\u4e0d\u4ee3\u8868\u6750\u6599\u4eba\u7f51\u7acb\u573a\u3002<\/p>\n<p>\u672a\u7ecf\u5141\u8bb8\u4e0d\u5f97\u8f6c\u8f7d\uff0c\u6388\u6743\u4e8b\u5b9c\u8bf7\u8054\u7cfbkefu@cailiaoren.com\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1: tougao@cailiaoren.com.<\/p>\n<p>\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaorenVIP\u3002<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u4f5c\u4e3a\u56fd\u9645\u4e0a\u6700\u4e3a\u77e5\u540d\u7684\u4e24\u5927\u7efc\u5408\u6027\u5b66\u672f\u671f\u520a\uff0cNature\u548cScience\u65e8\u5728\u53d1\u8868\u539f\u521b\u6027\u5f3a\u3001\u89c2\u70b9\u65b0\u9896\u3001\u5f71\u54cd\u5e7f\u6cdb\uff0c\u5e76\u4e14\u5bf9\u6574\u4e2a\u79d1\u5b66\u53d1\u5c55\u5177\u6709\u63a8\u52a8\u4f5c\u7528\u7684\u7a81\u7834\u6027\u53d1\u73b0\u3002\u7531\u4e8e\u7ade\u4e89\u6fc0&#8230;<\/p>\n","protected":false},"author":11454,"featured_media":214609,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[1187],"tags":[],"class_list":["post-214598","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-zhuanlan"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/214598"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/11454"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=214598"}],"version-history":[{"count":5,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/214598\/revisions"}],"predecessor-version":[{"id":214622,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/214598\/revisions\/214622"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/214609"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=214598"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=214598"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=214598"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}