{"id":21554,"date":"2016-06-25T08:10:13","date_gmt":"2016-06-25T00:10:13","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=21554"},"modified":"2016-06-24T21:35:51","modified_gmt":"2016-06-24T13:35:51","slug":"nature-communications-%e6%be%b3%e5%ad%a6%e8%80%85%e5%bc%80%e5%8f%91%e9%87%91%e5%b1%9e%e9%94%82%e8%b4%9f%e6%9e%81%e9%a2%84%e5%a4%84%e7%90%86%e6%96%b9%e6%b3%95-%e6%98%be%e8%91%97%e6%8f%90%e9%ab%98","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=21554","title":{"rendered":"Nature Communications: \u6fb3\u5b66\u8005\u5f00\u53d1\u91d1\u5c5e\u9502\u8d1f\u6781\u9884\u5904\u7406\u65b9\u6cd5 \u663e\u8457\u63d0\u9ad8\u5faa\u73af\u6027\u80fd"},"content":{"rendered":"<p>\u3010<strong>\u7b80\u4ecb<\/strong>\u3011<\/p>\n<p>\u5728\u4ee5\u91d1\u5c5e\u9502\u4e3a\u8d1f\u6781\u7684\u7535\u6c60\u4e2d\uff0c\u63d0\u9ad8\u7535\u6c60\u5faa\u73af\u6027\u80fd\u7684\u4e00\u5927\u5173\u952e\u5c31\u662f\u6291\u5236\u9502\u679d\u6676\u7684\u5f62\u6210\u3002\u6fb3\u5927\u5229\u4e9a\u7684\u79d1\u7814\u4eba\u5458\u5f00\u53d1\u51fa\u4e00\u79cd\u80fd\u6709\u6548\u6291\u5236\u9502\u679d\u6676\u5f62\u6210\u7684\u65b0\u65b9\u6cd5\uff0c\u5373\u5728\u7ec4\u88c5\u7535\u6c60\u524d\uff0c\u8ba9\u9502\u7535\u6781\u5728\u9502\u76d0\u6eb6\u6db2\u4e2d\u6d78\u6ce1\u4e00\u6bb5\u65f6\u95f4\u3002\u901a\u8fc7\u8fd9\u4e00\u7b80\u5355\u7684\u9884\u5904\u7406\uff0c\u53ef\u4ee5\u83b7\u5f97\u4e00\u5c42\u7a33\u5b9a\u5b58\u5728\u7684\u5141\u8bb8\u9502\u79bb\u5b50\u81ea\u7531\u8131\u5d4c\u7684\u56fa\u6001\u7535\u89e3\u8d28\u754c\u9762\u819c\uff08SEI\u819c\uff09\u3002\u7ecf\u8fc7\u9884\u5904\u7406\u5f97\u5230SEI\u819c\u540e\uff0cLi|\u7535\u89e3\u8d28|Li\u5bf9\u79f0\u7535\u6c60\u5728\u5faa\u73af2500\u5c0f\u65f6\u540e\u6ca1\u6709\u660e\u663e\u7684\u9502\u679d\u6676\u751f\u6210\uff1b\u5546\u4e1a\u5316\u7684Li|\u7535\u89e3\u8d28|LiFePO4\u5168\u7535\u6c60\u57281000\u6b21\u5145\u653e\u7535\u5faa\u73af\u540e\uff0c\u5e93\u4f26\u6548\u7387\u4ecd\u53ef\u7ef4\u6301\u572899.5%\u4ee5\u4e0a\uff1b\u9759\u7f6e\u4e86330\u5929\u7684\u7535\u6c60\u4e5f\u53ef\u4ee5\u83b7\u5f9795%\u4ee5\u4e0a\u7684\u5e93\u4f26\u6548\u7387\u3002\u8fd9\u79cdSEI\u819c\u7531\u91d1\u5c5e\u9502\u548c\u6eb6\u89e3\u6709\u9502\u76d0\u7684\u53cc\uff08\u6c1f\u78fa\u9170\uff09\u4e9a\u80fa\u5421\u54af\u70f7\u9393\uff08[C3mPyr+][FSI-]\uff09\u5ba4\u6e29\u79bb\u5b50\u6db2\u6001\u7535\u89e3\u8d28\uff08RTIL\uff09\u5316\u5b66\u53cd\u5e94\u751f\u6210\u3002\u5728\u5faa\u73af\u8fc7\u7a0b\u4e2d\uff0c\u8be5SEI\u819c\u80fd\u591f\u6291\u5236\u9502\u679d\u6676\u7684\u5f62\u6210\uff0c\u5e76\u4e14\u51cf\u5c11\u7535\u89e3\u6db2\u7684\u6d88\u8017\uff0c\u65f6\u95f4\u548c\u9502\u76d0\u662f\u5f71\u54cd\u5176\u52a8\u6001\u5f62\u8c8c\u53d8\u5316\u7684\u4e24\u4e2a\u4e3b\u8981\u56e0\u7d20\u3002\u8fd9\u9879\u7814\u7a76\u63d0\u51fa\u4e86\u4e00\u79cd\u7b80\u5355\u6709\u6548\uff0c\u4e14\u80fd\u591f\u5e94\u7528\u4e8e\u5b9e\u9645\u751f\u4ea7\u4e2d\u7684\u91d1\u5c5e\u9502\u9884\u5904\u7406\u5de5\u827a\uff0c\u4ece\u800c\u4f7f\u9502\u8d1f\u6781\u7535\u6c60\u7684\u5faa\u73af\u5bff\u547d\u53ef\u4ee5\u6ee1\u8db3\u5546\u4e1a\u9700\u6c42\u3002<\/p>\n<p>\u3010<strong>\u56fe\u6ce8<\/strong>\u3011<\/p>\n<p><strong>\u56fe1 \u91d1\u5c5e\u9502\u7ecf\u9884\u5904\u7406\u540e\u7684\u8868\u9762\u5fae\u89c2\u5f62\u8c8c\uff08SEM\uff09<\/strong><\/p>\n<p style=\"text-align: left;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-21916\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/1-43.jpg\" alt=\"1\" width=\"500\" height=\"500\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/1-43.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/1-43-150x150.jpg 150w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/1-43-300x300.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: left;\">(a)\u56fe\u53cd\u6620\u4e86\u91c7\u7528\u91d1\u5c5e\u9502\u548c\u5ba4\u6e29\u79bb\u5b50\u7535\u89e3\u6db2\u5316\u5b66\u53cd\u5e94\u5408\u6210SEI\u819c\u7684\u8fc7\u7a0b\uff1b<br \/>\n(b)\u3001(c)\u3001(d)\u3001(e)\u5206\u522b\u5c55\u793a\u4e86\u91d1\u5c5e\u9502\u4e0e\u542b\u6709LiFSI\u7684[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u53cd\u5e94\uff0c\u7ecf\u8fc74\u5c0f\u65f6\u30017\u5929\u300112\u5929\u53ca18\u5929\u540e\u7684\u8868\u9762\u5f62\u8c8c\u53d8\u5316\uff1b<br \/>\n(f)\u3001(g)\u3001(h)\u3001(i)\u5206\u522b\u5c55\u793a\u4e86\u91d1\u5c5e\u9502\u4e0e\u542b\u6709LiPF6\u7684[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u53cd\u5e94\uff0c\u7ecf\u8fc74\u5c0f\u65f6\u30017\u5929\u300112\u5929\u53ca18\u5929\u540e\u7684\u8868\u9762\u5f62\u8c8c\u53d8\u5316\uff1b<br \/>\n(j)\u3001(k)\u3001(l)\u3001(m)\u5206\u522b\u5c55\u793a\u4e86\u91d1\u5c5e\u9502\u4e0e\u542b\u6709LiAsF6\u7684[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u53cd\u5e94\uff0c\u7ecf\u8fc74\u5c0f\u65f6\u30017\u5929\u300112\u5929\u53ca18\u5929\u540e\u7684\u8868\u9762\u5f62\u8c8c\u53d8\u5316\uff1b<br \/>\nSEM\u56fe\u50cf\u7684\u6bd4\u4f8b\u5c3a\u5747\u4e3a50um\uff0c\u53f3\u4e0a\u89d2\u63d2\u56fe\u7684\u6bd4\u4f8b\u5c3a\u4e3a10um\u3002<\/p>\n<p style=\"text-align: left;\"><strong>\u56fe2 \u9502\u5bf9\u79f0\u7535\u6c60\u57280.1mAcm-1\u7535\u6d41\u5bc6\u5ea6\u4e0b5000\u6b21\u5faa\u73af\u7684\u8868\u5f81<\/strong><\/p>\n<p style=\"text-align: left;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-21917\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/2-39.jpg\" alt=\"2\" width=\"500\" height=\"440\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/2-39.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/2-39-300x264.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: left;\"><span style=\"line-height: 1.5;\">(a)(b)\u56fe\u5c55\u793a\u4e86\u672a\u9884\u5904\u7406\u7684Li|\u7535\u89e3\u8d28|Li\u5bf9\u79f0\u7535\u6c60\u5145\u653e\u7535\u5faa\u73af\u6d4b\u8bd5\u7684\u7535\u538b-\u65f6\u95f4\u56fe\u7ebf\uff0c\u5176\u4e2d(a)\u91c7\u7528\u542bLiPF6\u7684[C3mPyr+][FSI-]\u7535\u89e3\u6db2\uff0c\u7ecf\u8fc71300\u6b21\u5faa\u73af\uff08\u7ea6250h\uff09\u540e\u5931\u6548\uff0c\u4f46\u5728\u4f11\u7720\u4e8622\u5929\u540e\uff0c\u53c8\u5faa\u73af\u4e86100\u591a\u6b21\u624d\u5f7b\u5e95\u5931\u6548\u3002<\/span><span style=\"line-height: 1.5;\">(b)\u91c7\u7528\u542bLiAsF6\u7684[C3mPyr+][FSI-]\u7535\u89e3\u6db2\uff0c\u53ef\u4ee5\u5faa\u73af5000\u6b21\u3002<\/span><span style=\"line-height: 1.5;\">(c)-(h)\u7684SEM\u56fe\u50cf\u5c55\u793a\u4e86\u9502\u679d\u6676\u88ab\u6291\u5236\u7684\u60c5\u51b5\uff0c\u5176\u4e2d\u91c7\u7528LiFSI\/[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u7684\u7535\u6c60\u8d1f\u6781\u89c1(c)\u56fe\uff0c\u9694\u819c\u89c1(d)\u56fe\uff1b\u91c7\u7528LiAsF6\/[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u7684\u7535\u6c60\u8d1f\u6781\u89c1(e)\u56fe\uff0c\u9694\u819c\u89c1(f)\u56fe\uff1b\u91c7\u7528LiPF6\/[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u7684\u7535\u6c60\u8d1f\u6781\u89c1(g)\u56fe\uff0c\u9694\u819c\u89c1(h)\u56fe,<\/span><span style=\"line-height: 1.5;\">SEM\u56fe\u50cf\u7684\u6bd4\u4f8b\u5c3a\u5747\u4e3a50um\uff0c\u53f3\u4e0a\u89d2\u63d2\u56fe\u7684\u6bd4\u4f8b\u5c3a\u4e3a10um\u3002<\/span>\u636e\u62a5\u9053\u91c7\u7528LiFSI\/[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u7684\u7535\u6c60\u4e5f\u80fd\u5faa\u73af5000\u591a\u6b21\uff0c\u53ef\u89c1SEI\u819c\u7684\u7535\u5316\u5b66\u6027\u80fd\u4e0e\u9502\u76d0\u79cd\u7c7b\u6709\u5173\u3002<\/p>\n<p style=\"text-align: left;\">(a)\u56fe\u53ef\u4ee5\u8bf4\u660e\u7535\u6c60\u6700\u7ec8\u5931\u6548\u4e0d\u662f\u9502\u679d\u6676\u5f15\u8d77\u7684\u77ed\u8def\u95ee\u9898\uff0c(c)(e)(g)\u56fe\u4e2d\u9502\u8d1f\u6781\u8868\u9762\u4e5f\u6ca1\u6709\u660e\u663e\u7684\u679d\u6676\u751f\u6210\u3002\u5728(d)(f)(h)\u56fe\u4e2d\uff0c\u6211\u4eec\u53ef\u4ee5\u53d1\u73b0\u7535\u89e3\u6db2\u5206\u89e3\u4ea7\u7269\u5835\u585e\u4e86\u9694\u819c\u7684\u5b54\u9699\u7ed3\u6784\uff0c\u8fdb\u800c\u5f97\u51fa\u7535\u6c60\u5931\u6548\u7684\u5b9e\u9645\u539f\u56e0\uff0c\u5176\u5b9e\u662f\u9502\u8d1f\u6781\u8868\u9762\u79ef\u589e\u52a0\u7684\u901f\u5ea6\u8d76\u4e0d\u4e0a\u9694\u819c\u5b54\u9699\u88ab\u5835\u585e\u7684\u901f\u5ea6\uff0c\u963b\u788d\u4e86Li+\u7684\u4f20\u8f93\u3002<\/p>\n<p style=\"text-align: left;\"><strong>\u56fe3 \u672a\u5904\u7406\u548c\u9884\u5904\u740612\u5929\u540e\u7684\u9502\u5bf9\u79f0\u7535\u6c60\u7684\u7535\u5316\u5b66\u963b\u6297\u8c31<\/strong><\/p>\n<p style=\"text-align: left;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-21918\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/3-36.jpg\" alt=\"3\" width=\"429\" height=\"650\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/3-36.jpg 429w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/3-36-198x300.jpg 198w\" sizes=\"(max-width: 429px) 100vw, 429px\" \/><\/p>\n<p style=\"text-align: left;\">\u00a0(a)\u56fe\u4e3a\u672a\u5904\u7406\u7684\u4ee5LiAsF6\/[C3mPyr+][FSI-]\u4e3a\u7535\u89e3\u6db2\u7684\u9502\u5bf9\u79f0\u7535\u6c60\u7684\u5948\u594e\u65af\u7279\u56fe\u8c31\uff0c\u5176\u4e2d\u9ed1\u7ebf\u8868\u793a\u521d\u59cb\u72b6\u6001\uff0c\u754c\u9762\u7535\u963b\u4e3a251.5\u2126cm-2;\u7ea2\u7ebf\u8868\u793a\u7535\u6d41\u5bc6\u5ea60.1mAcm-1\uff0c\u7ecf\u8fc75000\u6b21\u5faa\u73af\u540e\u7684\u72b6\u6001\uff0c\u7535\u6c60\u7684\u754c\u9762\u7535\u963b\u964d\u4e3a51.3\u2126cm-2 (b)\u56fe\u662f\u9502\u7535\u6781\u7ecf\u8fc712\u5929\u9884\u5904\u7406\u7684\u4ee5LiFSI\/[C3mPyr+][FSI-]\u4e3a\u7535\u89e3\u6db2\u7684\u7535\u6c60\u7684\u963b\u6297\u8c31\uff0c\u5176\u4e2d\u9ed1\u7ebf\u8868\u793a\u521d\u59cb\u72b6\u6001\uff1b\u7ea2\u7ebf\u8868\u793a\u7535\u6d41\u5bc6\u5ea61.0mAcm-1\uff0c\u9996\u6b21\u5145\u7535\u540e\u7684\u60c5\u51b5\uff1b\u84dd\u7ebf\u8868\u793a\u5728\u540c\u6837\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u7ecf\u8fc7333\u6b21\u5faa\u73af\u540e\u7684\u60c5\u51b5\uff0c\u7535\u6c60\u7684\u754c\u9762\u7535\u963b\u540c\u6837\u660e\u663e\u4e0b\u964d\u3002<\/p>\n<p style=\"text-align: left;\"><strong>\u56fe4 \u57281.0mAcm-1\u7684\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u4e0d\u540c\u9884\u5904\u7406\u65f6\u95f4\u7684\u9502\u5bf9\u79f0\u7535\u6c60\u7684\u5faa\u73af\u6027\u80fd\u6bd4\u8f83<\/strong><\/p>\n<p style=\"text-align: left;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-21919\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/4-24.jpg\" alt=\"4\" width=\"500\" height=\"458\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/4-24.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/4-24-300x275.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p>\u56fe(a)(b)(c)\u4e3a\u9502\u5bf9\u79f0\u7535\u6c60\u5145\u653e\u7535\u5faa\u73af\u6d4b\u8bd5\u7684\u7535\u538b-\u65f6\u95f4\u66f2\u7ebf\uff0c\u4e09\u7ec4[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u4e2d\u5206\u522b\u6dfb\u52a0\u4e86LiFSI\u3001LiPF6\u3001LiAsF6,\u5176\u4e2d\u5f69\u8272\u66f2\u7ebf\u53cd\u6620\u4e86\u9884\u5904\u740612\u5929\u540e\u7684\u60c5\u51b5\uff0c\u9ed1\u7ebf\u4e3a\u9884\u5904\u740618\u5929\u7684\u60c5\u51b5\uff1b\u5229\u7528SEM\u6280\u672f\u89c2\u5bdfLi|LiFSI\/[C3mPyr+][FSI-]|Li\u7535\u6c60333\u6b21\u5faa\u73af\u540e\u7684\u5fae\u89c2\u5f62\u8c8c\uff0c\u7814\u7a76\u8005\u7740\u91cd\u89c2\u5bdf\u4e86(d)\u9502\u7247(e)\u9502\u7247\u6a2a\u622a\u9762(f)\u9694\u819c\u6750\u6599\u7684\u5f62\u8c8c\u53d8\u5316\u3002\u56fe(d)(f)\u7684\u6bd4\u4f8b\u5c3a\u4e3a20um,\u56fe(e)\u4e3a100um\u3002<\/p>\n<p style=\"text-align: left;\"><strong>\u56fe5 \u7ecf12\u5929\u9884\u5904\u7406\u7684Li|LiFSI\/[C3mPyr+][FSI-]|Li\u7535\u6c60\u7684\u7cfb\u5217\u8868\u5f81<\/strong><\/p>\n<p style=\"text-align: left;\"><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-21920\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/5-21.jpg\" alt=\"5\" width=\"500\" height=\"300\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/5-21.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/5-21-300x180.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p style=\"text-align: left;\">(a)\u56fe\u662f2.0mAcm-1\u4e0b500\u6b21\u5145\u653e\u7535\u5faa\u73af\u7684\u7535\u538b-\u5faa\u73af\u6b21\u6570\u66f2\u7ebf\uff1b<br \/>\n(b)\u56fe\u7535\u6d41\u5bc6\u5ea6\u4f9d\u6b21\u8bbe\u7f6e\u4e3a0.1mAcm-1\uff0c1mAcm-1\uff0c5mAcm-1\u548c10mAcm-1\uff0c\u5728\u6bcf\u79cd\u7535\u6d41\u5bc6\u5ea6\u4e0b\uff0c\u5747\u5145\u653e\u7535\u5faa\u73af50\u6b21\uff1b<br \/>\n(c)(d)\u56fe\u5206\u522b\u4e3a\u7535\u6d41\u5bc6\u5ea6\u4ece0.1mAcm-1\u7a81\u53d8\u52301mAcm-1\uff0c\u4ece5mAcm-1\u7a81\u53d8\u523010mAcm-1\u65f6\u7684\u653e\u5927\u663e\u793a\uff1b<br \/>\n(e)\u56fe\u53cd\u6620\u4e86\u8be5\u5bf9\u79f0\u7535\u6c60\u9996\u6b21\u5145\u653e\u7535\u8bd5\u9a8c\u7684\u7535\u538b\u53d8\u5316\u60c5\u51b5\uff1b<br \/>\n(f)\u56fe\u662f\u5bf9\u5e94\u7684\u9502\u8d1f\u6781\u4e0a\u9996\u6b21\u9502\u6c89\u79ef\u7684SEM\u56fe\uff08\u6bd4\u4f8b\u5c3a10um\uff09\uff1b<br \/>\n(g)\u56fe\u662f\u9996\u6b21\u9502\u5265\u843d\u7684SEM\u56fe\uff08\u6bd4\u4f8b\u5c3a50um\uff09\u3002<\/p>\n<p><strong>\u56fe6 \u6b63\u6781\u6750\u6599\u4e3aLiFeO4\uff0c\u8d1f\u6781\u6750\u6599\u9009\u7528\u672a\u5904\u7406\u7684\u91d1\u5c5e\u9502\u6216\u8005\u7ecf\u6db2\u6001\u79bb\u5b50\u7535\u89e3\u8d28\u6d78\u6ce112\u5929\u9884\u5904\u7406\u540e\u7684\u91d1\u5c5e\u9502\uff0c\u6bd4\u8f83\u4e24\u79cd\u7535\u6c60\u7684\u7535\u5316\u5b66\u6027\u80fd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-21921\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/6-23.jpg\" alt=\"6\" width=\"500\" height=\"379\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/6-23.jpg 500w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2016\/06\/6-23-300x227.jpg 300w\" sizes=\"(max-width: 500px) 100vw, 500px\" \/><\/p>\n<p>\u56fe(a)-(d)\u5c55\u793a\u4e86Li|LiFSI\/[C3mPyr+][FSI-]|LiFeO4\u5168\u7535\u6c60\u57281C\u500d\u7387\u4e0b\uff0c\u653e\u7535\u5bb9\u91cf\u548c\u5e93\u4f26\u6548\u7387\u968f\u5faa\u73af\u6b21\u6570\u7684\u53d8\u5316\uff0c\u5176\u4e2d(a)\u56fe\u4e2d\u7535\u6c60\u88c5\u914d\u7684\u662f\u672a\u7ecf\u9884\u5904\u7406\u7684\u9502\u7247\uff1b(b)\u662f\u7528LiFSI\/[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u9884\u5904\u7406\u540e\u7684\u9502\u7247\uff1b(c)\u662f\u7528LiPF6\/[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u9884\u5904\u7406\u540e\u7684\u9502\u7247\uff1b(d)\u662f\u7528LiAsF6\/[C3mPyr+][FSI-]\u7535\u89e3\u6db2\u9884\u5904\u7406\u540e\u7684\u9502\u7247\u3002<br \/>\n(e)\u56fe\u663e\u793a\u7684\u662f(b)\u56fe\u4e2d\u7684\u7535\u6c60\u9759\u7f6e330\u5929\u540e\uff0c\u57280.6C\u30011.2C\u30013C\u500d\u7387\u4e0b\u7684\u653e\u7535\u5bb9\u91cf\u548c\u5e93\u4f26\u6548\u7387\u3002<br \/>\n\u7814\u7a76\u8005\u8fd8\u5229\u7528SEM\u6280\u672f\u89c2\u5bdf\u4e86\u8be5\u4f53\u7cfb\u7535\u6c60\u7684\u5fae\u89c2\u5f62\u8c8c\uff0c\u7ed3\u679c\u5982\u56fe(f)-(i)\u6240\u793a\uff0c\u5176\u4e2d(f)\u662f\u9502\u8d1f\u6781\uff1b(g)\u662f\u9502\u8d1f\u6781\u7684\u9ad8\u500d\u653e\u5927\u6548\u679c\uff1b(h)\u662f\u9502\u8d1f\u6781\u7684\u6a2a\u622a\u9762\uff1b(i)\u662f\u9694\u819c\u6750\u6599\uff0c\u56fe(g)\u4e2d\u7684\u6807\u5c3a\u4ee3\u886810um\uff0c\u5176\u4f59\u56fe\u7247\u4e2d\u5747\u4e3a100um.<\/p>\n<p>\u6587\u732e\u5730\u5740\uff1a<a href=\"http:\/\/www.nature.com\/ncomms\/2016\/160613\/ncomms11794\/full\/ncomms11794.html\" target=\"_blank\">Stabilizing lithium metal using ionic liquids for long-lived batteries<\/a><\/p>\n<p>\u611f\u8c22\u7f16\u8f91\u90e8\u7cef\u7c73\u63d0\u4f9b\u7d20\u6750<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u7b80\u4ecb\u3011 \u5728\u4ee5\u91d1\u5c5e\u9502\u4e3a\u8d1f\u6781\u7684\u7535\u6c60\u4e2d\uff0c\u63d0\u9ad8\u7535\u6c60\u5faa\u73af\u6027\u80fd\u7684\u4e00\u5927\u5173\u952e\u5c31\u662f\u6291\u5236\u9502\u679d\u6676\u7684\u5f62\u6210\u3002\u6fb3\u5927\u5229\u4e9a\u7684\u79d1\u7814\u4eba\u5458\u5f00\u53d1\u51fa\u4e00\u79cd\u80fd\u6709\u6548\u6291\u5236\u9502\u679d\u6676\u5f62\u6210\u7684\u65b0\u65b9\u6cd5\uff0c\u5373\u5728\u7ec4\u88c5\u7535\u6c60\u524d\uff0c\u8ba9&#8230;<\/p>\n","protected":false},"author":169,"featured_media":21568,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[2],"tags":[129],"class_list":["post-21554","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-keji","tag-battery"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/21554"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/169"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=21554"}],"version-history":[{"count":13,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/21554\/revisions"}],"predecessor-version":[{"id":21923,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/21554\/revisions\/21923"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/21568"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=21554"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=21554"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=21554"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}