{"id":216677,"date":"2021-01-30T06:23:00","date_gmt":"2021-01-29T22:23:00","guid":{"rendered":"http:\/\/www.cailiaoniu.com\/?p=216677"},"modified":"2021-01-29T19:23:13","modified_gmt":"2021-01-29T11:23:13","slug":"acs-nano-%e9%80%9a%e8%bf%873d%e6%89%93%e5%8d%b0%e7%9a%84%e5%85%b7%e6%9c%89%e8%b6%85%e5%bc%b9%e6%80%a7%ef%bc%8c%e5%90%b8%e6%b9%bf%e6%80%a7%e5%92%8c%e7%a6%bb%e5%ad%90%e4%bc%a0%e5%af%bc%e6%80%a7","status":"publish","type":"post","link":"http:\/\/www.cailiaoniu.com\/?p=216677","title":{"rendered":"ACS Nano: \u901a\u8fc73D\u6253\u5370\u7684\u5177\u6709\u8d85\u5f39\u6027\uff0c\u5438\u6e7f\u6027\u548c\u79bb\u5b50\u4f20\u5bfc\u6027\u7684\u7ea4\u7ef4\u7d20\u7eb3\u7c73\u7ea4\u7ef4\u6750\u6599"},"content":{"rendered":"<p><strong>\u3010\u5f15\u8a00\u3011<\/strong><\/p>\n<p>\u8fdb\u6765\uff0c\u5177\u6709\u8d85\u5f39\u6027\u548c\u538b\u7f29\u56de\u5f39\u529b\u7684\u4e09\u7ef4(3D)\u8d85\u6750\u6599\u5728\u9694\u70ed\uff0c\u538b\u529b\u4f20\u611f\u5668\u548c\u80fd\u91cf\u5b58\u50a8\u7b49\u65b9\u9762\u5c55\u73b0\u51fa\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u800c\u5907\u53d7\u5173\u6ce8\u3002\u76ee\u524d\u5df2\u6709\u591a\u79cd\u6280\u672f\u7528\u4e8e\u6784\u5efa\u6b64\u7c7b\u8d85\u5f39\u60273D\u6574\u4f53\u7ed3\u6784\uff0c\u5305\u62ec\u7eb3\u7c73\u7ea4\u7ef4\u6a21\u677f\u5408\u6210\uff0c\u6fc0\u5149\u76f4\u5199\u5149\u523b\uff0c\u5149\u805a\u5408\u7269\u539f\u4f4d\u6210\u578b\uff0c\u6eb6\u5242\u70ed\u5408\u6210\u7b49\u3002\u5176\u4e2d\uff0c3D\u6253\u5370\u6216\u589e\u6750\u5236\u9020\u56e0\u5176\u5728\u590d\u6742\u7ed3\u6784\u8bbe\u8ba1\u53ef\u5feb\u901f\u6210\u578b\uff0c\u4ee5\u53ca\u9ad8\u5ea6\u7684\u8bbe\u8ba1\u548c\u751f\u4ea7\u81ea\u7531\u5ea6\u7b49\u4f18\u52bf\u800c\u8131\u9896\u800c\u51fa\u3002\u5df2\u7ecf\u5f00\u53d1\u51fa\u591a\u79cd\u7c7b\u578b\u7684\u80f6\u4f53\u51dd\u80f6\u6cb9\u58a8\uff0c\u4f8b\u5982\u9676\u74f7\uff0c\u7eb3\u7c73\u7ea4\u7ef4\u7d20\uff0c\u77f3\u58a8\u70ef\uff0c\u78b3\u7eb3\u7c73\u7ba1\u548c\u805a\u5408\u7269\uff0c\u4ee5\u4f7f\u7528\u76f4\u63a5\u6cb9\u58a8\u4e66\u5199\uff08DIW\uff093D\u6253\u5370\u6280\u672f\u5236\u9020\u5404\u79cd\u590d\u6742\u7684\u4e09\u7ef4\u7ed3\u6784\u3002\u7531\u4e8e\u8bb8\u591a3D\u6253\u5370\u7ed3\u6784\u4e13\u6ce8\u4e8e\u8f7b\u8d28\u548c\u9ad8\u673a\u68b0\u5f3a\u5ea6\uff0c\u56e0\u6b64\u901a\u5e38\u5728\u4e00\u5b9a\u7a0b\u5ea6\u4e0a\u4f1a\u727a\u7272\u5f39\u6027\u3002\u76ee\u524d\uff0c\u53ea\u6709\u77f3\u58a8\u70ef\u6750\u6599\u6bd4\u8f83\u5e7f\u6cdb\u7684\u7528\u4e8e3D\u6253\u5370\u8d85\u5f39\u6027\u6750\u6599\uff0c\u5176\u8d85\u5f39\u6027\u4e3b\u8981\u6765\u6e90\u4e8e3D\u6253\u5370\u56fa\u6709\u7684\u5b8f\u89c2\u4e2d\u7a7a\u7ed3\u6784\u548c\u5fae\u89c2\u8702\u7a9d\u7ed3\u6784\u3002\u56e0\u6b64\uff0c\u9700\u8981\u63a2\u7d22\u66f4\u5e7f\u6cdb\u7684\u6750\u6599\u5e93\uff0c\u4ee5\u6ee1\u8db3\u5bf9\u53ef\u6301\u7eed\u548c\u9ad8\u6027\u80fd3D\u6253\u5370\u57fa\u6750\u4e0d\u65ad\u589e\u957f\u7684\u9700\u6c42\u3002<\/p>\n<p><strong>\u3010\u6210\u679c\u7b80\u4ecb\u3011<\/strong><\/p>\n<p>\u8fd1\u65e5<strong>\uff0c\u4e2d\u56fd\u6797\u79d1\u9662\u6728\u6750\u6240\u9648\u5a9b\u52a9\u7406\u7814\u7a76\u5458\u548c\u52a0\u62ff\u5927\u4e0d\u5217\u98a0\u54e5\u4f26\u6bd4\u4e9a\u5927\u5b66\u59dc\u950b\u6559\u6388\u56e2\u961f<\/strong>\u63d0\u51fa\u4e86\u4e00\u79cd\u4f7f\u75283D\u6253\u5370\u548c\u5438\u6e7f\u76d0CaCl<sub>2<\/sub>\u7684\u68af\u5ea6\u5f15\u5165\u6765\u5236\u9020\u8d85\u5f39\u6027\uff0c\u5438\u6e7f\u548c\u79bb\u5b50\u5bfc\u7535\u7ea4\u7ef4\u5c81\u7eb3\u7c73\u7ea4\u7ef4\uff08CNF\uff09\u6574\u4f53\u6750\u6599\u7684\u65b9\u6cd5\u3002\u4e3a\u4e86\u5b9e\u73b0\u8d85\u5f39\u6027\uff0c\u4f7f\u75283D\u6253\u5370\u548c\u51b7\u51bb\u5e72\u71e5\u6765\u5f15\u5165\u5206\u5c42\u7684\u5b8f\u89c2\u548c\u5fae\u89c2\u591a\u5b54\u7ed3\u6784\u3002\u6b64\u5916\uff0c\u5c06CaCl<sub>2<\/sub>\u5f15\u51653D\u6253\u5370\u7684CNF\u6574\u6599\u4e2d\uff0c\u4ee5\u4ea4\u8054\u8868\u9762\u7fa7\u9178\u57fa\u56e2\uff0c\u5f62\u6210\u575a\u56fa\u800c\u521a\u6027\u7684\u7f51\u7edc\u7ed3\u6784\uff0c\u5e76\u7528\u4f5c\u5438\u6e7f\u76d0\uff0c\u5438\u6536\u7a7a\u6c14\u4e2d\u7684\u6c34\u4efd\uff0c\u4ece\u800c\u4ea7\u751f\u5f39\u6027\u548c\u67d4\u97e7\u6027\u3002\u901a\u8fc7\u8c03\u8282CaCl<sub>2<\/sub>\u7684\u542b\u91cf\u53ef\u4ee5\u5bb9\u6613\u5730\u8c03\u8282\u6c34\u7684\u5438\u6536\u91cf\u548c\u901f\u5ea6\u4ee5\u53ca\u673a\u68b0\u54cd\u5e94\u6027\u30023D\u6253\u5370\u7684CNF\u6574\u4f53\u6750\u6599\u5177\u6709\u51fa\u8272\u7684\u5f39\u6027\u548c\u5f62\u72b6\u6062\u590d\u80fd\u529b\uff0c\u80fd\u591f\u4ece70\uff05\u7684\u5e94\u53d8\u4e2d\u5b8c\u5168\u6062\u590d\uff0c\u5e76\u53ef\u4ee5\u627f\u53d7500\u591a\u6b21\u538b\u7f29\u6d4b\u8bd5\u5faa\u73af\u3002\u5177\u6709\u826f\u597d\u79bb\u5b50\u5bfc\u7535\u6027\u80fd\u7684CNF\u6574\u6599\u53ef\u7528\u4f5c\u5e94\u53d8\u548c\u5e94\u529b\u4f20\u611f\u5668\uff0c\u5e94\u529b\u654f\u611f\u5ea6\u4e3a0.337 kP<sup>-1<\/sup>\u3002\u76f8\u5173\u7814\u7a76\u6210\u679c\u201c<strong>Superelastic, Hygroscopic, and Ionic Conducting Cellulose Nanofibril Monoliths by 3D Printing<\/strong>\u201d\u4e3a\u9898\u53d1\u8868\u5728<strong>ACS Nano<\/strong>\u4e0a\u3002<\/p>\n<p><strong>\u3010\u56fe\u6587\u5bfc\u8bfb\u3011<\/strong><\/p>\n<p><strong>\u56fe\u4e00<\/strong><strong>3D<\/strong><strong>\u6253\u5370\u7684<\/strong><strong>CNF<\/strong><strong>\u6574\u4f53\u6750\u6599\u793a\u610f\u56fe\u53ca\u4f5c\u7528\u673a\u7406<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-216682\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/s.jpg\" alt=\"\" width=\"600\" height=\"505\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/s.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/s-300x253.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p><strong>\u56fe\u4e8c<\/strong><strong>3D<\/strong><strong>\u6253\u5370\u58a8\u6c34\u7684\u6d41\u53d8\u6027\u80fd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-216678\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/1-12.jpg\" alt=\"\" width=\"600\" height=\"311\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/1-12.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/1-12-300x156.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff0cb\uff092.0\uff05\u548c2.5\uff05CNF\u6cb9\u58a8\u7684\u6d41\u53d8\u7279\u6027\uff1a<\/p>\n<p>\uff08c\uff09\u7ea610\u6beb\u7c73\u9ad8\u7684\u6c34\u51dd\u80f6\u72b6\u548c\u51bb\u5e723D\u6253\u5370\u6574\u4f53\u6750\u6599\u7684\u7167\u7247\u3002<\/p>\n<p>\uff08d\uff093D\u6253\u5370\u6574\u6599\u5728\u51b7\u51bb\u5e72\u71e5\u4e4b\u524d\u548c\u4e4b\u540e\u7684\u4f53\u79ef\u4fdd\u7559\u503c\u3002<\/p>\n<p>\uff08e\uff09\u572843\uff05RH\u548c\u5e72\u71e5\u72b6\u6001\u4e0b3D\u6253\u5370\u6574\u4f53\u6750\u6599\u7684\u5bc6\u5ea6\u3002<\/p>\n<p>\uff08f\uff09\u572843\uff05\u76f8\u5bf9\u6e7f\u5ea6\u4e0b3D\u6253\u5370\u6574\u4f53\u6750\u6599\u7684\u5438\u6c34\u7387\u548c\u76f8\u5e94\u7684\u7070\u5206\u4ea7\u7387\u3002<\/p>\n<p><strong>\u56fe\u4e09<\/strong><strong>3D<\/strong><strong>\u6253\u5370\u6574\u6599\u7684\u529b\u5b66\u6027\u80fd<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-216679\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/2-11.jpg\" alt=\"\" width=\"600\" height=\"371\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/2-11.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/2-11-300x186.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u5177\u6709\u4e0d\u540cCNF\u6d53\u5ea6\u7684\u5370\u5237\u6574\u6599\u7684\u538b\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\u3002<\/p>\n<p>\uff08b\uff09\u5728\u5e73\u9762\uff08\u9876\u90e8\uff09\u548c\u5e73\u9762\u5916\uff08\u5e95\u90e8\uff09\u538b\u7f29\u540e\uff0c3D\u6253\u5370\u76842.0\uff05-20\uff05CNF\u6574\u6599\u7684\u5f62\u72b6\u6062\u590d\u7167\u7247\u3002<\/p>\n<p>\uff08c-e\uff09\u5728\u03b5\u301c70\uff05\u548c50 mm\/min\u52a0\u8f7d\/\u5378\u8f7d\u901f\u7387\u4e0b3D\u6253\u5370\u6574\u6599\u7684\u5faa\u73af\u538b\u7f29\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\uff0820\u4e2a\u5faa\u73af\uff09\u3002<\/p>\n<p><strong>\u56fe\u56db<\/strong><strong>CNF<\/strong><strong>\u6574\u6599\u7684\u7269\u5316\u548c\u5438\u6c34\u6027\u80fd\u8868\u5f81<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-216680\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/3-13.jpg\" alt=\"\" width=\"600\" height=\"457\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/3-13.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/3-13-300x229.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u75280.5 M CaCl2\u6eb6\u6db2\u4ea4\u8054\u76843D\u6253\u5370\u76842.0\uff05-25\uff05CNF\u6574\u6599\u7684SEM\u56fe\u50cf\u3002<\/p>\n<p>\uff08b\uff09\u572843\uff05RH\u4e0b\u5177\u6709\u4e0d\u540c\u76d0\u6d53\u5ea6\u76843D\u6253\u5370\u5e72\u71e5\u76842.0\uff05-25\uff05CNF\u6574\u6599\u7684\u5438\u6c34\u80fd\u529b\u7684\u65f6\u95f4\u66f2\u7ebf\u3002<\/p>\n<p>\uff08c\uff09\u653e\u5927\u540e\u7684\u5256\u9762\u56fe\u663e\u793a\u4e86\u521d\u59cb\u5438\u6c34\u7387\uff08k\uff09\u3002<\/p>\n<p>\uff08d\uff09\u5728\u76f8\u5bf9\u6e7f\u5ea6\u5206\u522b\u4e3a43\uff05\uff0c65\uff05\u548c95\uff05\u7684\u6761\u4ef6\u4e0b\uff0c\u5438\u6c34\u80fd\u529b\u4e3a2.0\uff05-2.5\uff050.5 M\u6574\u6599\u7684\u65f6\u95f4\u66f2\u7ebf\u3002<\/p>\n<p>\uff08e\uff09TGA\uff0c\uff08f\uff09DTG\u66f2\u7ebf\u548c\uff08g\uff092.0\uff05-25\uff05\u6574\u6599\u4e0e0-2 M CaCl2\u4ea4\u8054\u7684FTIR\u5149\u8c31\u3002<\/p>\n<p><strong>\u56fe\u4e94\u901a\u8fc7\u6539\u53d8<\/strong><strong>CaCl<sub>2<\/sub><\/strong><strong>\u542b\u91cf\u53ef\u4ee5\u8c03\u8282\u673a\u68b0\u6027\u80fd\u548c\u5f39\u6027<\/strong><\/p>\n<p><img loading=\"lazy\" decoding=\"async\" class=\"aligncenter size-full wp-image-216681\" src=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/4-12.jpg\" alt=\"\" width=\"600\" height=\"438\" srcset=\"http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/4-12.jpg 600w, http:\/\/www.cailiaoniu.com\/wp-content\/uploads\/2021\/01\/4-12-300x219.jpg 300w\" sizes=\"(max-width: 600px) 100vw, 600px\" \/><\/p>\n<p>\uff08a\uff09\u7ecf0.3M\uff0c0.5M\uff0c0.75M\u548c1M CaCl<sup>2<\/sup>\u6eb6\u6db2\u5904\u7406\u76843D\u6253\u5370\u76842.0\uff05-25\uff05CNF\u6574\u4f53\u7684\u538b\u7f29\u5e94\u529b-\u5e94\u53d8\u66f2\u7ebf\u3002<\/p>\n<p>\uff08b\uff093D\u6253\u5370\u76842.0\uff05-25\uff05CNF\u6574\u6599\u7684\u6768\u6c0f\u6a21\u91cf\u4e0e\u5bc6\u5ea6\u7684\u5173\u7cfb\u3002<\/p>\n<p>\uff08c\uff0cd\uff093D\u6253\u5370\u76842.0\uff05-25\uff05-0.5M\u6574\u6599\u7684\u5faa\u73af\u538b\u7f29\u03c3-\u03b5\u66f2\u7ebf<\/p>\n<p>\uff08e\uff09\u4e09\u4e2a3D\u6253\u5370\u7684\u6574\u6599\u57280-57.1\uff05\u7684\u538b\u7f29\u5e94\u53d8\u4e0b\u76f8\u5bf9\u7535\u963b\u53d8\u5316\u7684\u65f6\u95f4\u66f2\u7ebf\u3002<\/p>\n<p>\uff08f\uff093D\u6253\u5370\u7684\u6574\u6599\u7684\u76f8\u5bf9\u7535\u963b\u53d8\u5316\u4e0e\u538b\u529b\u7684\u5173\u7cfb\u3002<\/p>\n<p>\uff08g\uff09\u572810\u4e2a\u538b\u7f29\u5faa\u73af\u4e2d\uff0c\u57287.1\uff05\uff0c14.3\uff05\u548c50.0\uff05\u5e94\u53d8\u7684\u5faa\u73af\u538b\u7f29\u4e0b\u7684\u7535\u963b\u53d8\u5316\u3002<\/p>\n<p><strong>\u3010\u5c0f\u7ed3\u3011<\/strong><\/p>\n<p>\u603b\u4e4b\uff0c\u672c\u6587\u9075\u5faa3D\u6253\u5370\u548c\u5438\u6e7f\u76d0\u7ed3\u5408\u7684\u5408\u7406\u8bbe\u8ba1\u7b56\u7565\uff0c\u63d0\u51fa\u4e86\u4e00\u79cd\u8d85\u5f39\u6027\u548c\u79bb\u5b50\u5bfc\u7535CNF\u6574\u4f53\u6750\u6599\u3002TEMPO\u6c27\u5316\u7684CNF\u57282.0\uff05\u548c2.5\uff05\u7684\u6d53\u5ea6\u4e0b\u8868\u73b0\u51fa\u4f18\u5f02\u7684\u53ef\u6253\u5370\u6027\uff0c\u5e76\u4e14\u6253\u5370\u7684\u7ed3\u6784\u8868\u73b0\u51fa\u826f\u597d\u7684\u5f62\u72b6\u4fdd\u771f\u5ea6\u3002\u53ef\u4ee5\u901a\u8fc7CaCl<sub>2<\/sub>\u4ea4\u8054\u548c\u51b7\u51bb\u5e72\u71e5\u6765\u5de9\u56fa\u7d27\u5bc6\u81f4\u5bc6\u7684\u7ed3\u6784\uff0c\u4ece\u800c\u4f7f\u6253\u5370\u7ebf\u6761\u5206\u8fa8\u7387\u8fbe\u5230300\u03bcm\u3002\u9664\u4e86\u4ea4\u8054\u4ee5\u5916\uff0cCNF\u819c\u4e0a\u591a\u4f59\u7684CaCl<sub>2<\/sub>\u6676\u4f53\u8fd8\u53ef\u7528\u4f5c\u5438\u6e7f\u76d0\uff0c\u4ee5\u8c03\u8282\u5f39\u6027\u6027\u80fd\u548c\u79bb\u5b50\u5bfc\u7535\u6027\u80fd\u3002\u901a\u8fc7\u9010\u6e10\u589e\u52a0CaCl<sub>2<\/sub>\u542b\u91cf\uff0c\u53ef\u4ee5\u89c2\u5bdf\u52303D\u6253\u5370\u7684CNF\u6574\u4f53\u7ed3\u6784\u7684\u521a\u786c\u5230\u5f39\u6027\u7684\u8f6c\u53d8\uff0c\u5176\u6768\u6c0f\u6a21\u91cf\u9075\u5faa\u53cd\u5e38\u7684\u8d1f\u5e42\u5b9a\u5f8b\uff08\u6bd4\u4f8b\u7cfb\u6570\u4e3a-2.01\uff09\u4e0e\u5bc6\u5ea6\u589e\u52a0\u7684\u5173\u7cfb\u3002\u7531\u4e8e\u5438\u6536\u7684\u6c34\u5177\u6709\u589e\u5851\u4f5c\u7528\uff0c\u56e0\u6b643D\u6253\u5370\u7684CNF\u6574\u6599\u5177\u6709\u51fa\u8272\u7684\u9762\u5185\u548c\u9762\u5916\u5f39\u6027\uff0c\u53ef\u4ee5\u627f\u53d7\u9ad8\u8fbe100\u6b21\u7684\u5faa\u73af\u538b\u7f29\u53d8\u5f62\uff0c\u5728\u73af\u5883\u6e29\u5ea6\u548c\u76f8\u5bf9\u6e7f\u5ea6\uff08RH\uff09\u4e0b\u5e94\u53d8\u6062\u590d\u7387\u8d85\u8fc791\uff05\u3002\u968f\u7740RH\u589e\u81f365\uff05\uff0c3D\u6253\u5370\u7684CNF\u6574\u4f53\u6750\u6599\u8868\u73b0\u51fa\u751a\u81f3\u66f4\u9ad8\u7684\u5f39\u6027\uff0c\u53ef\u4ee5\u5728500\u6b21\u5faa\u73af\u538b\u7f29\u53d8\u5f62\u540e\u4fdd\u630191\uff05\u4ee5\u4e0a\u7684\u5e94\u53d8\u6062\u590d\u3002\u8fd9\u9879\u5de5\u4f5c\u63d0\u51fa\u4e86\u4e00\u79cd\u53ef\u884c\u7684\u7b56\u7565\uff0c\u53ef\u4ee5\u5c06\u5178\u578b\u7684\u521a\u6027CNF\u6574\u6599\u8f6c\u6362\u4e3a\u8d85\u5f39\u6027\u7ed3\u6784\uff0c\u4e0d\u4ec5\u53ef\u4ee5\u6269\u5c55\u5230\u5176\u4ed6\u7c7b\u578b\u7684\u6750\u6599\uff0c\u800c\u4e14\u8fd8\u4e3a3D\u6253\u5370CNF\u6574\u6599\u5728\u8f6f\u7535\u5b50\uff0c\u538b\u529b\u4f20\u611f\u5668\u548c\u8bb8\u591a\u5176\u4ed6\u9886\u57df\u4e2d\u4f7f\u7528\u63d0\u4f9b\u4e86\u673a\u4f1a\u3002<\/p>\n<p><strong>\u6587\u732e\u94fe\u63a5\uff1a<\/strong><strong>\u201c<\/strong><a href=\"http:\/\/202.114.202.219\/rwt\/ACS\/https\/PB4XE63PMFSYGLUQPJUB\/doi\/10.1021\/acsnano.0c10577\"><strong>Superelastic, Hygroscopic, and Ionic Conducting Cellulose Nanofibril Monoliths by 3D Printing<\/strong><\/a><strong>\u201d(ACS Nano, 2021,DOI:<\/strong> <strong>: 10.1021\/acsnano.0c10577)<\/strong><\/p>\n<p>\u672c\u6587\u7531\u6750\u6599\u4eba\u5fae\u89c2\u4e16\u754c\u7f16\u8bd1\u4f9b\u7a3f\uff0c\u6750\u6599\u725b\u6574\u7406\u7f16\u8f91\u3002<\/p>\n<p>\u6b22\u8fce\u5927\u5bb6\u5230\u6750\u6599\u4eba\u5ba3\u4f20\u79d1\u6280\u6210\u679c\u5e76\u5bf9\u6587\u732e\u8fdb\u884c\u6df1\u5165\u89e3\u8bfb\uff0c\u6295\u7a3f\u90ae\u7bb1tougao@cailiaoren.com\u3002<\/p>\n<p>\u6750\u6599\u4eba\u6295\u7a3f\u4ee5\u53ca\u5185\u5bb9\u5408\u4f5c\u53ef\u52a0\u7f16\u8f91\u5fae\u4fe1\uff1acailiaokefu \u3002<\/p>\n<p><strong>\u3010\u7b2c\u4e00\u4f5c\u8005\u7b80\u4ecb\u3011<\/strong><\/p>\n<p><strong>\u9648\u5a9b,<\/strong><strong>\u4e2d\u56fd\u6797\u4e1a\u79d1\u5b66\u7814\u7a76\u9662\u6728\u6750\u5de5\u4e1a\u7814\u7a76\u6240\u52a9\u7406\u7814\u7a76\u5458\uff0c\u957f\u671f\u4ece\u4e8b\u7eb3\u7c73\u7ea4\u7ef4\u7d20\u5236\u5907\u3001\u7eb3\u7c73\u7ea4\u7ef4\u7d20\u529f\u80fd\u6750\u6599\u5f00\u53d1\uff0c\u7814\u7a76\u8bba\u6587\u53d1\u8868\u5728<\/strong>ACS Nano, ACS Sustainable Chemistry &amp; Engineering\uff0cCellulose\u7b49\u671f\u520a\u3002<\/p>\n<p><strong>\u3010\u901a\u8baf\u4f5c\u8005\u7b80\u4ecb\u3011<\/strong><\/p>\n<p><strong>\u59dc\u950b\uff08Feng Jiang<\/strong><strong>\uff09,<\/strong><strong>\u52a0\u62ff\u5927\u4e0d\u5217\u98a0\u54e5\u4f26\u6bd4\u4e9a\u5927\u5b66\u52a9\u7406\u6559\u6388\uff0c\u52a0\u62ff\u5927\u751f\u7269\u8d28\u53ef\u518d\u751f\u529f\u80fd\u6750\u6599\u9996\u5e2d\u79d1\u5b66\u5bb6\uff08Tier II Canada Research Chair in Sustainable Functional Biomaterials<\/strong><strong>\uff09\u3002Carbohydrate Polymers<\/strong><strong>\u7f16\u59d4\u3002<\/strong><\/p>\n<p>\u4e3b\u8981\u7814\u7a76\u65b9\u5411\u4e3a\u5929\u7136\u9ad8\u5206\u5b50\u7eb3\u7c73\u6750\u6599\u7684\u5f00\u53d1\uff0c\u6539\u6027\u53ca\u5e94\u7528\u3002\u7814\u7a76\u9886\u57df\u6d89\u53ca\u5929\u7136\u9ad8\u5206\u5b50\u7eb3\u7c73\u6750\u6599\u7eff\u8272\u63d0\u53d6\uff0c\u6c14\u51dd\u80f6\u548c\u6c34\u51dd\u80f6\u7684\u5236\u5907\uff0c\u589e\u6750\u5236\u9020\uff0c\u4ee5\u53ca\u5728\u70ed\u7ba1\u7406\u3001\u50a8\u80fd\u3001\u73af\u5883\u4fee\u590d\u3001\u548c\u4f20\u611f\u5668\u7b49\u9886\u57df\u7684\u529f\u80fd\u6027\u5e94\u7528\u3002\u7814\u7a76\u8bba\u6587\u53d1\u8868\u5728 Nature Materials, Science Advances, Joule, Advanced Materials, Advanced Energy Materials, Advanced Functional Materials, Angewandte Chemie, ACS Nano, Energy Storage Materials, Journal of Materials Chemistry A, Chemical Engineering Journal, Nanoscale Horizons, Chemistry of Materials, ACS Applied Materials &amp; Interfaces, ACS Sustainable Chemistry &amp; Engineering, Carbohydrate Polymers \u7b49\u671f\u520a\u3002<\/p>\n<p><strong>\u56e2\u961f\u7814\u7a76\u65b9\u5411\uff1a<\/strong>\u5929\u7136\u9ad8\u5206\u5b50\u7eb3\u7c73\u6750\u6599\uff0c\u81ea\u7ec4\u88c5\uff0c\u8d85\u5f3a\u8d85\u97e7\u590d\u5408\u6750\u6599\uff0c\u6c14\u51dd\u80f6\uff0c\u6c34\u51dd\u80f6\uff0c3D \u6253\u5370\uff0c\u70ed\u7ba1\u7406\uff0c\u53ef\u7a7f\u6234\u4ea7\u54c1\uff0c\u4f20\u611f\u5668\u7b49\u3002<\/p>\n<p><strong>\u76f8\u5173\u4f18\u8d28\u8bba\u6587\u63a8\u8350\uff08\u8fd1\u4e24\u5e74\uff09\uff1a<\/strong><\/p>\n<ol>\n<li>Hengfei Qin, Yue Zhou, Qianyu Huang, Zhou Yang, Ruoyu Dong, Long Li, Jianghong Tang, Chunyong Zhang, <strong><u>Feng Jiang.<\/u><\/strong> Metal organic framework (MOF)\/wood derived multi-cylinders high-power 3D reactor. ACS Applied Materials &amp; Interfaces. <a href=\"https:\/\/doi.org\/10.1021\/acsami.0c21664\">https:\/\/doi.org\/10.1021\/acsami.0c21664<\/a><\/li>\n<\/ol>\n<p><strong>\u00a0<\/strong>Mingyao Song, Jungang Jiang, Hengfei Qin, Xueyong Ren, <strong><u>Feng Jiang.<\/u><\/strong> Flexible and super thermal-insulating cellulose nanofibrils\/emulsion composite aerogel with quasi-closed pores. <em>ACS Applied Materials &amp; Interfaces,<\/em> 2020, 12, 40, 45363-45372.<\/p>\n<ol>\n<li>Penghui Zhu, Yudi Kuang, Yuan Wei, Fang Li, Huajie Ou, <strong><u>Feng Jiang,<\/u><\/strong> Gang Chen. Electrostatic self-assembly enabled conductive TEMPO-oxidized fibers\/carbon nanotubes network for humidity sensing. <em>Chemical Engineering Journal,<\/em> 2021, 404, 127105.<\/li>\n<li>Jungang Jiang, Hale Oguzlu, <strong><u>Feng Jiang.<\/u><\/strong> 3D Printing of lightweight, super-strong yet flexible all-cellulose structure. <em>Chemical Engineering Journal,<\/em> 2021, 405, 126668.<\/li>\n<li>Yuhang Ye, Yifan Zhang, Yuan Chen, Xiaoshuai Han, <strong><u>Feng Jiang.<\/u><\/strong> Cellulose nanofibrils enhanced, strong, stretchable, freezing-tolerant ionic conductive organohydrogel for multi-functional sensors. <em>Advanced Functional Materials,<\/em> 2020, 2003430.<\/li>\n<li>Jungang Jiang, Nancy Carrillo-Enriquez, Hale Oguzlu, Xushen Han, Ran Bi, Mingyao Song, Jack Saddler, Runcang Sun, <strong><u>Feng Jiang.<\/u><\/strong> High production yield and more thermally stable lignin containing cellulose nanocrystals isolated using a ternary acidic deep eutectic solvent. <em>ACS Sustainable Chemistry &amp; Engineering,<\/em> 2020, 8, 7182\u2013719<\/li>\n<li>Hengfei Qin, Kun Fu, Ying Zhang, Yuhang Ye, Mingyao Song, Yudi Kuang, Soo-Hwan Jang, <strong><u>Feng Jiang,<\/u><\/strong> Lifeng Cui, Flexible nanocellulose enhanced Li<sup>+<\/sup> conducting membrane for solid polymer electrolyte. <em>Energy Storage Materials,<\/em> 2020, 28, 293-299.<\/li>\n<li>Huan Tao, Nathalie Lavoine, <strong><u>Feng Jiang,<\/u><\/strong> Juntao Tang, Ning Lin. Reducing End Modification on Cellulose Nanocrystals: Strategy, Characterization, Applications and Challenges. <em>Nanoscale Horizons,<\/em> 2020, 5, 607-627.<\/li>\n<li>Xiaoshuai Han, Yuhang Ye, Frank Lam, Junwen Pu, <strong><u>Feng Jiang.<\/u><\/strong> Hydrogen-bonding-induced assembly of aligned cellulose nanofibers into ultrastrong and tough bulk materials. <em>Journal of Materials Chemistry A,<\/em> 2019, 7, 27023<\/li>\n<\/ol>\n<p><strong>\u00a0<\/strong><\/p>\n<p>&nbsp;<\/p>\n","protected":false},"excerpt":{"rendered":"<p>\u3010\u5f15\u8a00\u3011 \u8fdb\u6765\uff0c\u5177\u6709\u8d85\u5f39\u6027\u548c\u538b\u7f29\u56de\u5f39\u529b\u7684\u4e09\u7ef4(3D)\u8d85\u6750\u6599\u5728\u9694\u70ed\uff0c\u538b\u529b\u4f20\u611f\u5668\u548c\u80fd\u91cf\u5b58\u50a8\u7b49\u65b9\u9762\u5c55\u73b0\u51fa\u5e7f\u9614\u7684\u5e94\u7528\u524d\u666f\u800c\u5907\u53d7\u5173\u6ce8\u3002\u76ee\u524d\u5df2\u6709\u591a\u79cd\u6280\u672f\u7528\u4e8e\u6784\u5efa\u6b64\u7c7b\u8d85\u5f39\u60273&#8230;<\/p>\n","protected":false},"author":7084,"featured_media":216682,"comment_status":"open","ping_status":"closed","sticky":false,"template":"","format":"standard","meta":{"footnotes":""},"categories":[215],"tags":[20,54],"class_list":["post-216677","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-jiedu","tag-zhineng","tag-making"],"_links":{"self":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/216677"}],"collection":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts"}],"about":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/users\/7084"}],"replies":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcomments&post=216677"}],"version-history":[{"count":2,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/216677\/revisions"}],"predecessor-version":[{"id":216973,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/posts\/216677\/revisions\/216973"}],"wp:featuredmedia":[{"embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=\/wp\/v2\/media\/216682"}],"wp:attachment":[{"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fmedia&parent=216677"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Fcategories&post=216677"},{"taxonomy":"post_tag","embeddable":true,"href":"http:\/\/www.cailiaoniu.com\/index.php?rest_route=%2Fwp%2Fv2%2Ftags&post=216677"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}